Preparation method and application of copper selenide and platinum composite material

Through the preparation of copper selenide@platinum composite materials, the photothermal properties of copper selenide and the catalytic effect of platinum are used to solve the problem of tumor hypoxia and antioxidants caused by radiotherapy, and achieve the synergistic effect of radiosensitization and photothermal therapy. Significantly improve the killing power and treatment efficiency of tumor cells.

CN118723938AActive Publication Date: 2024-10-01HENAN UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410800759.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-01
Estimated Expiration
2044-06-20

AI Technical Summary

Technical Problem

Radiotherapy (RT) easily causes damage to adjacent normal tissues when killing tumors. The hypoxic nature of the tumor microenvironment makes tumor cells resistant to radiation, and the antioxidant system in cancer cells reduces radiation efficiency.

Method used

A copper selenide@platinum composite material is prepared, using copper selenide as a photothermal material to perform photothermal treatment under near-infrared light. Platinum nanoparticles catalyze the decomposition of H2O2 in the tumor site, overcome the hypoxia problem and enhance the effect of radiotherapy.

Benefits of technology

It achieves the synergistic effect of radiosensitization of tumors and photothermal therapy, significantly improves the efficiency of radiotherapy and the killing power of tumor cells, and has good biocompatibility and circulation stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118723938A_ABST
    Figure CN118723938A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method and application of a copper selenide and platinum composite material, H2SeO3 and polyvinylpyrrolidone (PVP) are dissolved in deionized water, stirring is performed, a hydrazine hydrate solution is added, stirring reaction is performed at the room temperature, precipitates are washed and dispersed in water, and selenium nanosphere dispersion liquid is obtained; the preparation method comprises the following steps: mixing selenium nanosphere dispersion liquid with a PVP (Polyvinyl Pyrrolidone) solution, a K2PtCl4 solution and absolute ethyl alcohol, stirring and reacting at 50-70 DEG C, centrifugally washing, precipitating and dispersing in water to obtain selenium-platinum nanoparticle dispersion liquid, mixing and stirring the selenium-platinum nanoparticle dispersion liquid with the PVP solution, a copper salt solution and an ascorbic acid solution, then adding an H2O2 solution, stirring and reacting, centrifugally washing and precipitating, and drying to obtain the platinum-selenium nanoparticle composite material. The copper selenide and platinum composite material is obtained. Copper selenide serving as a photo-thermal material has good photo-thermal conversion performance, and photo-thermal therapy on tumors can be achieved; the platinum nanoparticles growing on the surface of the copper selenide-platinum composite material have a radiotherapy sensitization effect, the radiotherapy effect can be further improved, and the prepared copper selenide-platinum composite material achieves RT / PTT combined therapy on tumors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of radiotherapy sensitization and synergistic treatment of tumors by photothermal and radiotherapy, and in particular to a preparation method and application of a copper selenide@platinum composite material. Background Art

[0002] Among the main treatment strategies, radiotherapy (RT) is a powerful treatment strategy that has been used for more than a century. It exerts a non-invasive tumor-killing effect by directly damaging DNA and indirectly generating cytotoxic reactive oxygen species (ROS). As a classic tumor treatment method, RT has its unique advantages, such as being not limited by tissue depth. However, some inherent defects of RT also limit its long-term application, mainly in the following three aspects: 1) The ionizing radiation used to kill tumors may cause damage to adjacent normal tissues, thereby causing serious toxic side effects to the body. 2) The hypoxic nature within the tumor microenvironment (TME) may make tumor cells resistant to radiation, ultimately leading to failure of tumor eradication. 3) Since elevated antioxidants are a general feature of the cancer phenotype, the antioxidant system in cancer cells will prevent them from counteracting these damaging effects by quenching excess free radicals. For example, the concentration of glutathione (GSH) in cancer cells is about four times that in normal cells, which has the ability to inhibit ROS before they reach the target site and ultimately reduces the efficiency of radiation to a large extent.

[0003] In the past two decades, the rapid development of emerging advanced nanomaterials and nanobiotechnologies has provided a promising opportunity for tumor radiosensitization. Various nanomaterials have been widely studied and applied to enhance the efficacy of radiotherapy, which is attributed to their versatile physicochemical properties, such as good biocompatibility, inherent radiosensitizing activity, high loading capacity for multiple types of drugs, and enhanced tumor tissue permeability and retention (EPR) effect.

[0004] Previously, nanomaterial-mediated radiosensitization approaches have focused on enhancing intracellular radiation energy deposition through high-Z (atomic number) nanoradiosensitizers. In recent years, a large number of new nanoradiosensitizers and radiosensitization strategies have been proposed. These nanoradiosensitizers and radiosensitization strategies can not only enhance ionizing radiation energy deposition, but also have the ability to catalyze ROS production, manipulate TME (such as reducing intracellular glutathione (GSH) concentration, converting low-toxic intracellular H2O2 into highly active HO·, and improving intratumoral oxygen levels) or regulate cell cycle / signaling pathways to make cancer cells more sensitive to radiation, thereby significantly enhancing the therapeutic effect of RT and reducing its side effects at the same time. For example, photocatalytic semiconductor nanoparticles can be activated by X-rays to promote ROS production, thereby enhancing the radiation effect. Some nanomaterials have the ability to deplete glutathione (GSH) in tumors, thereby preventing the clearance of radiation-induced ROS from glutathione (GSH), ultimately improving treatment outcomes. Some iron (Fe) / copper (Cu)-based nanomaterials can convert intracellular H2O2 into highly active HO·, thereby damaging cancer cells and enhancing the RT treatment effect. Nanomaterials with the ability to improve oxygen levels can effectively overcome tumor hypoxia, reduce radioresistance, and ultimately improve radiation efficiency.

[0005] Another basic therapeutic strategy to improve the efficacy of RT is to combine useful therapies with RT to produce a synergistic effect. Photothermal therapy (PTT) is reported to be one of the most effective candidates for RT combined therapy. By using photothermal agents that absorb in the near-infrared (NIR) range, PTT can convert NIR light energy into thermal energy for tumor ablation. On the one hand, the hyperthermia induced during PTT can improve radiosensitivity by increasing intratumoral blood flow, thereby enhancing oxygenation status and reversing hypoxia-induced radioresistance. Hyperthermia causes double-stranded DNA breaks, preventing DNA repair after RT. In addition, hyperthermia can kill S-phase cancer cells that are insensitive to radiation to improve the efficiency of radiotherapy. On the other hand, due to its higher penetration ability, RT can compensate for the incomplete ablation of deep tumors by NIR. Therefore, nanomaterials with photothermal ablation and radiosensitization properties are promising to improve treatment outcomes. Inspired by this, the present invention prepares a nanoparticle for combined RT / PTT treatment of cancer, and can improve hypoxia at the tumor site. Summary of the invention

[0006] To solve the above problems, the present invention provides a preparation method and application of a copper selenide@platinum composite material, using copper selenide as a photothermal material. Under the irradiation of near-infrared light, copper selenide nanospheres have good photothermal conversion performance and can achieve photothermal treatment of tumors. The high-Z (atomic number) platinum nanoparticles grown on their surface have the effect of radiosensitization, and platinum can catalyze the decomposition of H2O2 in the tumor site, overcome the problem of tumor hypoxia, and further enhance the effect of radiotherapy.

[0007] The present invention is specifically implemented by the following technical scheme. According to a method for preparing a copper selenide@platinum composite material proposed in the present invention, it comprises the following steps:

[0008] (1) H2SeO3 and polyvinyl pyrrolidone are dissolved in deionized water, and the mixture is stirred continuously for 10 to 30 minutes. A certain amount of hydrazine hydrate solution is then added thereto, and the mixture is reacted at room temperature for 3 to 6 hours under stirring conditions. The reaction product is centrifuged, and the precipitate obtained by centrifugation is washed with deionized water and then dispersed in deionized water to obtain a 0.1 to 10 mg / mL selenium nanosphere dispersion;

[0009] (2) taking the selenium nanosphere dispersion prepared in step (1), mixing it with a polyvinyl pyrrolidone aqueous solution, a K2PtCl4 aqueous solution and anhydrous ethanol in a volume ratio of 6:2-6:0.01-0.1:0-50, stirring and reacting at 50-70° C. for 5-12 hours, after the stirring is completed, centrifuging the obtained product, collecting the precipitate obtained by centrifugation and washing it with deionized water, and then dispersing it in deionized water to obtain a 0.1-10 mg / mL selenium@platinum nanoparticle dispersion;

[0010] (3) The selenium@platinum nanoparticle dispersion prepared in step (2), the polyvinyl pyrrolidone aqueous solution, the copper salt aqueous solution, and the ascorbic acid aqueous solution are sequentially added into the same container and stirred for 3 to 10 minutes, and then the hydrogen peroxide aqueous solution is added thereto and stirred for 3 to 10 minutes. After stopping the stirring, the obtained product is centrifuged and the precipitate obtained by centrifugation is washed with deionized water to obtain a copper selenide@platinum composite material.

[0011] Preferably, in step (1), the mass ratio of H2SeO3 to polyvinyl pyrrolidone is 0.774:0.2-1.2, the ratio of the mass of H2SeO3 to the volume of hydrazine hydrate solution is 0.774 g:1.5-3 mL, and the volume ratio of the deionized water used to dissolve H2SeO3 and polyvinyl pyrrolidone to the volume of the hydrazine hydrate solution is 100-200:1.5-3.

[0012] Preferably, the mass fraction of the hydrazine hydrate solution is 80%.

[0013] Preferably, in step (2), the concentration of the polyvinyl pyrrolidone aqueous solution is 0.01-0.1 g / mL, the concentration of the K2PtCl4 aqueous solution is 500 mmol / L; the centrifuge speed is 12000 rpm / min, and the centrifugation time is 10 min.

[0014] Preferably, in step (3), the volume ratio of the selenium@platinum nanoparticle dispersion, the polyvinyl pyrrolidone aqueous solution, the copper salt aqueous solution, and the ascorbic acid aqueous solution is 1:1:0.5 to 0.7:2.

[0015] Preferably, in step (3), the concentration of the polyvinyl pyrrolidone aqueous solution is 5-15 mg / mL, the concentration of the copper salt aqueous solution is 0.05-0.15 mmol / L, the concentration of the ascorbic acid aqueous solution is 0.01-5 mol / L, and the copper salt is at least one of copper chloride, copper nitrate and copper sulfate.

[0016] Preferably, the mass fraction of the aqueous hydrogen peroxide solution in step (3) is 30%, and the volume ratio of the aqueous hydrogen peroxide solution to the selenium@platinum nanoparticle dispersion is 40-80 μL:1 mL.

[0017] The present invention also provides a copper selenide@platinum composite material obtained according to the preparation method. The copper selenide@platinum composite material is a core-shell structure, wherein the copper selenide nanospheres are cores and the platinum nanoparticles are shells grown on the surfaces of the copper selenide nanospheres.

[0018] The copper selenide@platinum composite material obtained according to the above preparation method can be used as a radiotherapy sensitizer and photothermal material for tumor treatment, wherein the copper selenide nanospheres act as photothermal materials, and the platinum nanoparticles on their surface act as radiotherapy sensitizers, and the synergistic effect of the two realizes the RT / PTT combined treatment of tumors.

[0019] Compared with the prior art, the present invention has obvious advantages and beneficial effects. By means of the above technical solution, the present invention can achieve considerable technical progress and practicality, and has a wide range of utilization value, and has at least the following advantages:

[0020] (1) The present invention unifies radiotherapy sensitization and photothermal therapy on a copper selenide @ platinum composite material. The composite material has a distinct core-shell structure, with copper selenide nanospheres as the core and Pt nanoparticles as the shell grown on the surface of the copper selenide nanospheres. The copper selenide @ platinum composite nanomaterial can produce a strong plasma resonance effect. Copper selenide, as a photothermal material, has good photothermal conversion performance, can efficiently absorb near-infrared light and convert light energy into thermal energy, thereby achieving photothermal therapy for tumors. The high-Z (atomic number) platinum nanoparticles grown on its surface have the effect of radiotherapy sensitization, acting as a radiotherapy sensitizer, and platinum can catalyze the decomposition of H2O2 in the tumor site to produce highly active substances, overcome the problem of tumor hypoxia, and further enhance the effect of radiotherapy.

[0021] (2) The copper selenide@platinum composite material (CS@Pt) prepared by the present invention has excellent photothermal performance. -2 Under 980nm near-infrared laser irradiation, 100μg mL -1The temperature of the CS@Pt dispersion can be raised to 69°C within 8 minutes. After five heating-cooling cycles, CS@Pt still has efficient light absorption and photothermal conversion properties, so CS@Pt has good cyclic stability. Experiments have shown that CS@Pt also has good biocompatibility and significant radiosensitization effects, which can enhance the damage of X-rays to tumor cell DNA and inhibit tumor cell proliferation. At a radiation dose of 6Gy, CS@Pt achieved 98% inhibition of tumor cell proliferation, while the control group without CS@Pt only inhibited 62% year-on-year. CS@Pt combined with radiotherapy and photothermal therapy can effectively inhibit tumor cell cloning and significantly increase the tumor cell mortality rate. Therefore, the CS@Pt composite material prepared by the present invention has excellent photothermal properties, biocompatibility and radiosensitization effects, enhances the lethality of radiotherapy to tumors, and realizes RT / PTT combined treatment of tumors.

[0022] (3) The preparation method provided by the present invention is simple and convenient, the reaction process is easy to control, the yield is high, and it is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the preparation process of the copper selenide@platinum composite material (CS@Pt) of the present invention and tumor treatment.

[0024] Figure 2 1 and 2 are transmission electron micrographs of CS@Pt prepared in Example 1 and Example 2, wherein (a) corresponds to Example 1 and (b) corresponds to Example 2.

[0025] Figure 3 This is the XRD pattern of CS@Pt prepared in Example 2.

[0026] Figure 4 The dispersions of CS@Pt with different concentrations prepared in Example 2 were heated to 1 W cm -2 Temperature rise curve within 8 minutes of near-infrared laser irradiation.

[0027] Figure 5 The dispersion of CS@Pt prepared in Example 2 was -2 Graph of five heating-cooling cycles under near-infrared laser irradiation.

[0028] Figure 6 This is a biocompatibility test diagram of CS@Pt prepared in Example 2 with esophageal squamous cell carcinoma cells (KYSE30) and human intravenous endothelial cells (HUVEC).

[0029] Figure 7 These are pictures of KYSE30 cell clone formation in the CS@Pt group and the Control group under different radiation doses.

[0030] Figure 8 It is the DNA damage detection diagram of KYSE30 cells in CS@Pt group and Control group under 4Gy radiation dose.

[0031] Fig. 9 It is the fluorescence graph of reactive oxygen species level in KYSE30 cells under different treatment conditions.

[0032] Fig.10 These are pictures of KYSE30 cell clone formation under different treatment conditions.

[0033] Fig.11 These are pictures of live-dead staining of KYSE30 cells under different treatment conditions.

[0034] Fig.12 This is a schematic diagram of the operation flow of the in vivo experiment in mice.

[0035] Fig.13 These are optical photographs of tumors in mice in six experimental groups that underwent different treatments.

[0036] Fig.14 This is a comparison of the average tumor mass in mice from six experimental groups that underwent different treatments. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] The present invention is described in detail with specific examples below. If no specific conditions are specified in the following examples, they are all carried out according to conventional conditions or conditions recommended by the manufacturer. The raw materials and reagents used without specifying the manufacturer are all conventional products that can be purchased from the market.

[0039] Embodiment 1:

[0040] (1) Preparation of Se nanosphere dispersion: 774 mg H2SeO3 and 1.2 g polyvinylpyrrolidone (PVP) were dissolved in 100 mL deionized water in turn, and 2.2 mL of 80% N2H4·H2O solution was added dropwise thereto after continuous stirring for 10 min. The mixture was reacted at room temperature for 3 h under stirring. The reaction system turned red and was centrifuged at 10,000 r / min for 10 min. The precipitate was collected and washed three times with deionized water. The precipitate after washing was selenium nanospheres. The selenium nanospheres were dispersed in deionized water to prepare a selenium nanosphere dispersion with a concentration of 4 mg / mL.

[0041] (2) 3 mL of the selenium nanosphere dispersion prepared in step (1) was taken and mixed with 3 mL of PVP aqueous solution (concentration of 0.1 g / mL) and 0.05 mL of K2PtCl4 aqueous solution (concentration of 500 mmol / L). The mixed solution was stirred at 50° C. for 5 h. After the stirring, the obtained product was centrifuged at a speed of 10000 r / min for 10 min. The precipitate obtained by centrifugation was collected and washed with deionized water. The washed precipitate was dispersed in deionized water to prepare a selenium@platinum nanoparticle dispersion with a concentration of 1 mg / mL, which was recorded as Se@Pt dispersion;

[0042] (3) Preparation of copper selenide@platinum composite material dispersion: 1 mL of the Se@Pt dispersion prepared in step (2) was taken, and 1 mL of a 10 mg / mL PVP aqueous solution, 0.5 mL of a 0.1 mmol / L CuCl2 aqueous solution, and 2 mL of a 0.1 mol / L ascorbic acid (AA) aqueous solution were added into a beaker in sequence and stirred for 5 min. After stirring, a brown solution A was obtained. 60 μL of a 30% H2O2 aqueous solution was added to the solution A and stirred for 3 min. The solution was then centrifuged at 10,000 r / min for 10 min. The precipitate obtained by centrifugation was collected and washed twice with deionized water. The precipitate after washing was the copper selenide@platinum composite material, which was a nanoparticle, denoted as CS@Pt.

[0043] Embodiment 2:

[0044] (1) This step is the same as step (1) of Example 1;

[0045] (2) 3 mL of the selenium nanosphere dispersion prepared in step (1) was taken and mixed with 3 mL of PVP aqueous solution (concentration of 0.1 g / mL), 0.05 mL of K2PtCl4 aqueous solution (concentration of 500 mmol / L), and 6 mL of anhydrous ethanol. The mixed solution was stirred at 70° C. for 5 h. After the stirring, the obtained product was centrifuged at a speed of 10000 r / min for 10 min. The precipitate obtained by centrifugation was collected and washed with deionized water. The washed precipitate was dispersed in deionized water to prepare a selenium@platinum nanoparticle dispersion with a concentration of 1 mg / mL, which was recorded as Se@Pt dispersion;

[0046] (3) This step is the same as step (3) of Example 1.

[0047] Embodiment 3:

[0048] (1) This step is the same as step (1) of Example 1;

[0049] (2) 3 mL of the selenium nanosphere dispersion prepared in step (1) was taken and mixed with 3 mL of PVP aqueous solution (concentration of 0.1 g / mL), 0.05 mL of K2PtCl4 aqueous solution (concentration of 500 mmol / L), and 25 mL of anhydrous ethanol. The mixed solution was stirred at 60° C. for 5 h. After the stirring, the obtained product was centrifuged at a speed of 10,000 r / min for 10 min. The precipitate obtained by centrifugation was collected and washed with deionized water. The washed precipitate was dispersed in deionized water to prepare a selenium@platinum nanoparticle dispersion with a concentration of 1 mg / mL, which was recorded as Se@Pt dispersion;

[0050] (3) This step is the same as step (3) of Example 1.

[0051] Embodiment 4:

[0052] (1) This step is the same as step (1) of Example 1;

[0053] (2) This step is the same as step (2) of Example 1;

[0054] (3) Preparation of copper selenide@platinum composite material dispersion: 1 mL of the Se@Pt dispersion prepared in step (2) was taken, and 1 mL of a 15 mg / mL PVP aqueous solution, 0.7 mL of a 0.15 mmol / L copper nitrate aqueous solution, and 2 mL of a 0.5 mol / L ascorbic acid (AA) aqueous solution were added into a beaker in sequence and stirred for 8 min. After stirring, a brown solution A was obtained. 80 μL of a 30% H2O2 aqueous solution was added to the solution A and stirred for 5 min. The solution was then centrifuged at 10,000 r / min for 10 min. The precipitate obtained by centrifugation was collected and washed twice with deionized water. The precipitate after washing was the copper selenide@platinum composite material, which was a nanoparticle, denoted as CS@Pt.

[0055] Figure 1 is a schematic diagram of the preparation process of the copper selenide @ platinum composite material (CS@Pt) of the present invention and tumor treatment (taking copper salt as copper chloride as an example), CS@Pt is the abbreviation of copper selenide @ platinum nanocomposite material, such as Figure 1 As shown in the figure, N2H4·H2O was used as a reducing agent to prepare Se nanospheres, and then K2PtCl4 was added to control the temperature to regulate the growth of Pt nanoparticles on the surface of Se nanospheres. Then, a copper source was introduced, and under the action of hydrogen peroxide, Se nanospheres were converted into Cu 2-x Se nanospheres (where x = 0 to 1). Cu 2-x Se@Pt is composed of Pt nanoparticles and Cu 2-x Se (x = 0 ~ 1) nanospheres. Copper selenide nanospheres have good photothermal conversion performance and can achieve photothermal treatment of tumors, and the high-Z platinum nanoparticles grown on their surface have the effect of radiosensitization, and platinum can catalyze the decomposition of H2O2 in the tumor site, overcome the problem of tumor hypoxia, and further improve the effect of radiotherapy. Therefore, the copper selenide @ platinum composite material prepared by the present invention has excellent photothermal performance and radiosensitization effect, and can increase the intracellular oxygen content (as is known to all, there is a large amount of H2O2 inside tumor cells, and Pt can catalyze the decomposition of H2O2 to produce oxygen), and realize RT / PTT combined treatment of tumors.

[0056] Figure 2 is the transmission electron microscopy image of CS@Pt prepared in Example 1 and Example 2, Figure 2 (a) corresponds to Example 1. It can be clearly seen that CS@Pt has an obvious core-shell structure, with the copper selenide nanospheres as the core and Pt densely coated on the surface of the copper selenide to form a shell layer. Figure 2 (b) corresponds to Example 2. The light-colored spheres in the figure are copper selenide nanospheres, and the dark-colored particles are Pt nanoparticles, indicating that adding anhydrous ethanol in step (2) is beneficial to the formation of Pt nanoparticles.

[0057] Figure 3 is the XRD pattern of CS@Pt prepared in Example 2. Figure 3 It can be determined that the prepared composite material is composed of Cu 2-x It is composed of Se (wherein x=0 to 1) and Pt.

[0058] The following experiments verify the efficacy of the copper selenide@platinum composite material (CS@Pt) prepared by the present invention in tumor treatment applications. The CS@Pt used in the following experiments is the copper selenide@platinum composite material (CS@Pt) prepared in Example 2.

[0059] Experiment 1

[0060] The copper selenide@platinum composite material prepared in Example 2 was prepared into a concentration of 0 μg mL -1 , 50 μg mL -1 , 100 μg mL -1 The power density of the solution was 1.0 W cm -2 The 980nm near-infrared laser was used for irradiation, and the temperature was recorded every 30s using an infrared thermal imager for a total of 8 minutes. The temperature rise curves of CS@Pt dispersions of different concentrations were plotted using the origin drawing software, with time as the horizontal axis and the temperature recorded at the corresponding time as the vertical axis, as shown in the figure. Figure 4 As shown, at a power density of 1.0 W cm -2 Within 8 minutes of 980nm near-infrared laser irradiation, the heating effect of CS@Pt dispersions with different concentrations showed concentration dependence. The higher the concentration of CS@Pt dispersion, the more obvious its heating effect was within the same time. -2 Under 980nm near-infrared laser irradiation, 100μg mL -1 The temperature of the CS@Pt dispersion can rise to 69 °C within 8 min.

[0061] Experiment 2

[0062] The CS@Pt prepared in Example 2 was prepared into 100 μg mL -1 The dispersion was used with a power density of 1.0 W cm -2The dispersion was irradiated with a 980nm near-infrared laser, and the temperature was recorded every 30 seconds using an infrared thermal imager. The laser was turned off after recording for 2.5 minutes. The dispersion was cooled for 2 minutes before the laser was turned on again. The temperature was recorded every 30 seconds during the cooling process. This operation was repeated five times. During the 2nd to 5th laser irradiation, the temperature was recorded every 30 seconds using an infrared thermal imager. The laser was turned off after recording for 2 minutes. The temperature was recorded for 3 minutes during the last cooling process. The origin drawing software was used to draw a graph of the five heating-cooling cycles of the CS@Pt dispersion, with time as the horizontal axis and the temperature recorded at the corresponding time as the vertical axis, as shown in the figure below. Figure 5 As shown, it can be clearly seen that after five heating-cooling cycles, CS@Pt still has efficient light absorption and photothermal conversion characteristics, and the maximum temperatures that can be reached after five heating-cooling cycles are not much different, reflecting that the prepared CS@Pt has good stability.

[0063] Experiment 3

[0064] Esophageal squamous cell carcinoma cell (KYSE30) is a cell line derived from human esophageal squamous cell carcinoma, and human umbilical vein endothelial cell (HUVEC) is a cell line derived from human umbilical vein endothelial cell. Both KYSE30 and HUVEC were provided by the Key Laboratory of Tumor Epigenetics of Henan Province, New District Hospital, the First Affiliated Hospital of Henan University of Science and Technology, and were purchased from the Cell Bank of the Chinese Academy of Sciences (ATCC). KYSE30 and HUVEC were cultured in 1640 medium containing 10% fetal bovine serum (FBS) and DMEM medium containing 10% FBS, respectively.

[0065] KYSE30 and HUVEC were inoculated in 96-well plates (5000 cells per well). The culture medium of KYSE30 was 1640 medium containing 10% FBS, and the culture medium of HUVEC was DMEM medium containing 10% FBS. After culturing for 24 h, the culture medium of KYSE30 was replaced with 1640 medium containing different concentrations of CS@Pt (the concentrations of CS@Pt were 0 μg mL -1 , 20 μg mL -1 , 40 μg mL -1 , 60 μg mL -1 , 80 μg mL -1 ), the HUVEC culture medium was replaced with DMEM medium containing different concentrations of CS@Pt (the concentrations of CS@Pt were 0 μg mL -1 , 20 μg mL -1 , 40 μg mL -1 , 60 μg mL -1 , 80 μg mL -1), and then cultured for another 24 h, the culture medium of KYSE30 and HUVEC was replaced with fresh 1640 culture medium and DMEM culture medium, and then 10 μL of CCK8 reagent was added to each of them and incubated for 2 h. Then, the cell activity was detected by a microplate reader, and the origin software was used to plot the CS@Pt concentration as the horizontal axis and the KYSE30 cell activity and HUVEC cell activity as the vertical axis, as shown in the figure. Figure 6 As shown, the CS@Pt used in this experiment is the CS@Pt prepared in Example 2. Figure 6 It is shown that the CS@Pt prepared in Example 2 has good biocompatibility with esophageal squamous cell carcinoma cells (KYSE30) and human intravenous endothelial cells (HUVEC).

[0066] Experiment 4

[0067] This experiment was divided into CS@Pt group and Control group. KYSE30 cells were seeded in 6-well plates in each group (2000 cells per well). The initial culture medium of both CS@Pt group and Control group was 1640 medium containing 10% FBS. After 24 h of culture, the culture medium of CS@Pt group was replaced with 60 μg mL -1 The 1640 medium containing CS@Pt, the medium of the Control group was replaced with an equal amount of 1640 medium without CS@Pt; after 6 hours of culture, the KYSE30 cells of the CS@Pt group and the Control group were irradiated with different doses of X-rays. Then the medium of both groups was replaced with fresh 1640 medium, and the KYSE30 cells were cultured for another week. After one week, the KYSE30 cells were fixed with 4% paraformaldehyde and stained with crystal violet reagent, and then photographed with an exposure machine to obtain the clone formation pictures of KYSE30 cells under different radiation doses, as shown in the figure. Figure 7 As shown. Figure 7 It can be seen that with the increase of radiation dose, the proliferation of KYSE30 cells was significantly inhibited. Under the same radiation dose, the CS@Pt group had a more obvious inhibitory effect on the proliferation of KYSE30 cells than the Control group, indicating that the CS@Pt prepared by the present invention can significantly enhance the inhibitory effect on the proliferation of KYSE30 cells.

[0068] Experiment 5

[0069] This experiment was divided into CS@Pt group and Control group. KYSE30 cells were seeded in confocal dishes in each group (2000 cells per well). The initial culture medium of both CS@Pt group and Control group was 1640 medium containing 10% FBS. After 48 h of culture, the culture medium of CS@Pt group was replaced with 60 μg mL -1The culture medium of the control group was replaced with an equal amount of 1640 culture medium without CS@Pt. After culturing for 6 h, the KYSE30 cells of the CS@Pt group and the control group were irradiated with X-rays at a radiation dose of 4 Gy. Then, the culture medium of the two groups was replaced with fresh 1640 culture medium. The cells were stained with DNA damage detection reagent and photographed using a confocal microscope. Figure 8 The DNA damage of KYSE30 cells in the CS@Pt group and the Control group when the radiation dose was 4 Gy. The results show that radiotherapy inhibits tumor proliferation by killing DNA, and the CS@Pt prepared in Example 2 can enhance the damage of X-rays to cell DNA.

[0070] Experiment 6

[0071] This experiment was divided into six experimental groups, namely, Control group, CS@Pt group, RT group, CS@Pt+L group, CS@Pt+RT group, and CS@Pt+RT+L group. KYSE30 cells were seeded in 12-well plates in each group (100,000 cells per well). The initial culture medium of each group was 1640 culture medium containing 10% FBS. After culturing for 24 h, the culture medium of the CS@Pt group, CS@Pt+L group, CS@Pt+RT group, and CS@Pt+RT+L group was replaced with 60 μg mL -1 The culture medium of the control group and the RT group was replaced with an equal amount of 1640 culture medium without CS@Pt. After culturing for 6 h, the KYSE30 cells in the RT group, the CS@Pt+RT group, and the CS@Pt+RT+L group were irradiated with 4 Gy of X-rays for radiotherapy. Then, the cells in the CS@Pt+RT+L group were irradiated with a 980 nm near-infrared laser for 5 min for photothermal therapy (laser power was 1 W / cm 2 ); After 6 h of culture, the KYSE30 cells in the CS@Pt+L group were directly irradiated with a 980 nm near-infrared laser for 5 min for photothermal treatment (laser power was 1 W / cm 2 , without X-ray irradiation). The control group and the CS@Pt group were not irradiated with X-rays or near-infrared lasers. After the six experimental groups completed the above experimental steps, the reactive oxygen species expression level of each group was detected using an reactive oxygen species fluorescent probe, and photographed using a confocal microscope. Fig. 9 The fluorescence images of the reactive oxygen species expression levels of KYSE30 cells in different groups and under different treatment conditions obtained according to the above experimental steps are shown in Figure 1. Fig. 9It can be seen that the CS@Pt+RT group showed the most significant expression level of reactive oxygen species, indicating that Pt can catalyze the decomposition of hydrogen peroxide into water and oxygen, both of which are reactants of reactive oxygen species. 2+ It can react with GSH, reduce the intracellular GSH content, and prevent ROS from being removed by GSH, which further increases the ROS content. However, since photothermal therapy is performed after radiotherapy, the cell morphology is completely lost after photothermal therapy. In the subsequent staining, washing the cells may cause some ROS to disappear. Therefore, the ROS fluorescence signal of the CS@Pt+RT+L treatment combination will become weaker.

[0072] Experiment 7

[0073] This experiment was divided into six experimental groups, namely, Control group, CS@Pt group, RT group, CS@Pt+L group, CS@Pt+RT group, and CS@Pt+RT+L group. KYSE30 cells were seeded in 6-well plates in each group (2000 cells per well). The initial culture medium of each group was 1640 medium containing 10% FBS. After culturing for 24 h, the culture medium of CS@Pt group, CS@Pt+L group, CS@Pt+RT group, and CS@Pt+RT+L group was replaced with 60 μg mL -1 The culture medium of the control group and the RT group was replaced with an equal amount of 1640 culture medium without CS@Pt. After culturing for 6 h, the KYSE30 cells in the RT group, the CS@Pt+RT group, and the CS@Pt+RT+L group were irradiated with 6 Gy of X-rays for radiotherapy. Then, the cells in the CS@Pt+RT+L group were irradiated with a 980 nm near-infrared laser for 5 min for photothermal therapy (laser power was 1 W / cm 2 ); After 6 h of culture, the KYSE30 cells in the CS@Pt+L group were directly irradiated with a 980 nm near-infrared laser for 5 min for photothermal treatment (laser power was 1 W / cm 2 , no X-ray irradiation). The control group and the CS@Pt group were not irradiated with X-rays or near-infrared lasers. After the six experimental groups completed the above experimental steps, the culture medium of the six experimental groups was replaced with fresh 1640 culture medium, and the cells were cultured for one week. After one week, the KYSE30 cells were fixed with 4% paraformaldehyde and stained with crystal violet reagent, and then photographed with an exposure machine to obtain the clone formation pictures of KYSE30 cells in different groups and under different treatment conditions, as shown in Figure 2. Fig.10As shown, compared with the Control group, CS@Pt group, and RT group, the CS@Pt+L group, CS@Pt+RT group, and CS@Pt+RT+L group all effectively inhibited the clone formation of KYSE30 cells, indicating that both radiotherapy and photothermal therapy can effectively inhibit the clone formation of KYSE30 cells, and the CS@Pt+RT+L group had the best therapeutic effect.

[0074] Experiment 8

[0075] This experiment was divided into six experimental groups, namely, Control group, CS@Pt group, RT group, CS@Pt+L group, CS@Pt+RT group, and CS@Pt+RT+L group. KYSE30 cells were seeded in 12-well plates in each group (100,000 cells per well). The initial culture medium of each group was 1640 culture medium containing 10% FBS. After culturing for 24 h, the culture medium of the CS@Pt group, CS@Pt+L group, CS@Pt+RT group, and CS@Pt+RT+L group was replaced with 60 μg mL -1 The culture medium of the control group and the RT group was replaced with an equal amount of 1640 culture medium without CS@Pt. After culturing for 6 h, the KYSE30 cells in the RT group, the CS@Pt+RT group, and the CS@Pt+RT+L group were irradiated with 6 Gy of X-rays for radiotherapy. Then, the cells in the CS@Pt+RT+L group were irradiated with a 980 nm near-infrared laser for 5 min for photothermal therapy (laser power was 1 W / cm 2 ); After 6 h of culture, the KYSE30 cells in the CS@Pt+L group were directly irradiated with a 980 nm near-infrared laser for 5 min for photothermal treatment (laser power was 1 W / cm 2 , without X-ray irradiation). The control group and CS@Pt group were not irradiated with X-rays or near-infrared lasers. After the six experimental groups completed the above experimental steps, cells were stained with live-dead staining reagents and photographed with a confocal microscope. Fig.11 The live-dead staining of KYSE30 cells in different groups and under different treatment conditions obtained according to the above experimental steps. Fig.11 It showed that the tumor cell mortality rate in the CS@Pt+RT+L group (radiotherapy followed by photothermal therapy) increased significantly.

[0076] In vivo experiments in mice:

[0077] The AKR tumor (mouse esophageal tumor) model was established using male C57BL / 6 mice weighing approximately 16-18 g and 6-8 weeks old. All animal experiments were performed in accordance with the Laboratory Animal Guidelines of the First Affiliated Hospital of Henan University of Science and Technology and approved by the Animal Experiment Ethics Committee. AKR tumor cells were provided by the Henan Provincial Tumor Epigenetics Key Laboratory, New District Hospital, First Affiliated Hospital of Henan University of Science and Technology, and purchased from the Chinese Academy of Sciences Cell Bank (ATCC). AKR cell culture conditions were consistent with HUVEC cell culture conditions, and both were cultured in DMEM medium containing 10% FBS.

[0078] The experiment was divided into 6 experimental groups, each with 6 mice, and the 6 experimental groups were Control group, CS@Pt group, RT group, CS@Pt+RT group, CS@Pt+L group, and CS@Pt+RT+L group. Fig.12 As shown, the mice were fed with normal feed from day 0 to day 4, and 100 μL of AKR tumor cell suspension was injected into the body (right back) of each mouse on day 5. The AKR tumor cell suspension was obtained by adding AKR tumor cells into PBS buffer, and its cell concentration was 1×10 7 / mL. From the 6th to the 13th day, the mice were fed with normal feed. On the 14th day, the mice in the CS@Pt group, CS@Pt+RT group, CS@Pt+L group, and CS@Pt+RT+L group were injected with CS@Pt material at a dose of 15 mg / kg. The CS@Pt material was injected through the tail vein in the form of a dispersion. The CS@Pt dispersion was a certain amount of CS@Pt dispersed in PBS buffer with a concentration of 5 mg / mL. The Control group and the RT group were injected with the same volume of normal saline without CS@Pt. 12 hours after the injection, the RT group, CS@Pt+RT group, and CS@Pt+RT+L group were irradiated with X-rays at a radiation dose of 6Gy to the tumor site (the back of the mouse, as shown in the figure). Fig.12 The CS@Pt+RT+L group was then irradiated with a 980nm near-infrared laser for 5 minutes for photothermal therapy (laser power was 1W / cm 2 ); 12 h after the injection of CS@Pt dispersion, the mice in the CS@Pt+L group were directly irradiated with a 980nm near-infrared laser for 5 min for photothermal therapy (laser power was 1 W / cm 2, no X-ray irradiation). The mice in the Control group and the CS@Pt group were not irradiated with X-rays or near-infrared lasers. Next, the above operation was repeated once on the 16th, 18th, 20th, 22nd, and 24th days. Each time, the mice in the CS@Pt group, CS@Pt+RT group, CS@Pt+L group, and CS@Pt+RT+L group were injected with PBS buffer (concentration of 5 mg / mL) containing CS@Pt according to the above operation and conditions, and the mice in the Control group and the RT group were injected with an equal amount of saline without CS@Pt. After 12 hours, the mice in the RT group, the CS@Pt+RT group, and the CS@Pt+RT+L group were irradiated with X-rays according to the above operation. The mice in the CS@Pt+RT+L group were irradiated with near-infrared lasers after X-ray irradiation. The mice in the CS@Pt+L group were directly irradiated with near-infrared lasers 12 hours after the injection of CS@Pt. The mice in the Control group and the CS@Pt group were not irradiated with X-rays or near-infrared lasers. On the 25th day, all mice were dissected, and the tumors in the mice were removed and marked, and then photographed and weighed.

[0079] Fig.13 These are optical photographs of tumors in mice in the six experimental groups after the above-mentioned different treatments. Each experimental group had six tumors (only three tumors were obtained in the CS@Pt+RT+L group). Fig.14 This is a comparison chart of the average tumor mass (unit: g) of mice in the six experimental groups after the above different treatments. Fig.13 and Fig.14 It can be seen that: compared with the control group (Control group), the CS@Pt group did not show an inhibitory effect on the tumor. The RT group showed a certain inhibitory effect on the tumor, and the tumor mass was reduced by 48.1% compared with the control group (Control group). Both the CS@Pt+RT and CS@Pt+L groups showed relatively excellent anti-tumor effects, with tumor masses being 20.7% and 29.6% of the control group, respectively. The CS@Pt+RT+L group showed the best anti-tumor effect, with some tumors completely ablated, and the mass of unablated tumors was only 1.13% of the control group.

[0080] The above experiments show that the copper selenide@platinum composite material (CS@Pt) prepared by the present invention has excellent photothermal performance and radiotherapy sensitization effect, can enhance the lethality of radiotherapy for tumors, and can realize RT / PTT combined treatment of tumors.

[0081] The above is only an embodiment of the present invention, and does not limit the present invention in any form. The present invention can also have other forms of embodiments according to the above structures and functions, which are not listed one by one. Therefore, any simple modification, equivalent change and modification made by any technician familiar with the profession to the above embodiment according to the technical essence of the present invention without departing from the scope of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a copper selenide@platinum composite material, characterized in that The following steps are involved: (1) H2SeO3 and polyvinyl pyrrolidone are dissolved in deionized water, and the mixture is stirred continuously for 10 to 30 minutes. A certain amount of hydrazine hydrate solution is then added thereto, and the mixture is reacted at room temperature for 3 to 6 hours under stirring conditions. The reaction product is centrifuged, and the precipitate obtained by centrifugation is washed with deionized water and then dispersed in deionized water to obtain a 0.1 to 10 mg / mL selenium nanosphere dispersion; (2) taking the selenium nanosphere dispersion prepared in step (1), mixing it with a polyvinyl pyrrolidone aqueous solution, a K2PtCl4 aqueous solution and anhydrous ethanol in a volume ratio of 6:2-6:0.01-0.1:0-50, stirring and reacting at 50-70° C. for 5-12 hours, after the stirring is completed, centrifuging the obtained product, collecting the precipitate obtained by centrifugation and washing it with deionized water, and then dispersing it in deionized water to obtain a 0.1-10 mg / mL selenium@platinum nanoparticle dispersion; (3) The selenium@platinum nanoparticle dispersion prepared in step (2), the polyvinyl pyrrolidone aqueous solution, the copper salt aqueous solution, and the ascorbic acid aqueous solution are sequentially added into the same container and stirred for 3 to 10 minutes, and then the hydrogen peroxide aqueous solution is added thereto and stirred for 3 to 10 minutes. After stopping the stirring, the obtained product is centrifuged and the precipitate obtained by centrifugation is washed with deionized water to obtain a copper selenide@platinum composite material.

2. The method for preparing the copper selenide@platinum composite material according to claim 1, characterized in that In step (1), the mass ratio of H2SeO3 to polyvinyl pyrrolidone is 0.774:0.2-1.2, the mass ratio of H2SeO3 to the volume of hydrazine hydrate solution is 0.774 g:1.5-3 mL, and the volume ratio of deionized water used to dissolve H2SeO3 and polyvinyl pyrrolidone to the volume of hydrazine hydrate solution is 100-200:1.5-3.

3. The method for preparing the copper selenide@platinum composite material according to claim 1 or 2, characterized in that The mass fraction of the hydrazine hydrate solution is 80%.

4. The method for preparing the copper selenide@platinum composite material according to claim 1, characterized in that In step (2), the concentration of the polyvinyl pyrrolidone aqueous solution is 0.01-0.1 g / mL, and the concentration of the K2PtCl4 aqueous solution is 500 mmol / L; the centrifuge speed is 12000 rpm / min, and the centrifugation time is 10 min.

5. The method for preparing the copper selenide@platinum composite material according to claim 1, characterized in that In step (3), the volume ratio of the selenium@platinum nanoparticle dispersion, the polyvinyl pyrrolidone aqueous solution, the copper salt aqueous solution, and the ascorbic acid aqueous solution is 1:1:0.5 to 0.7:

2.

6. The method for preparing the copper selenide@platinum composite material according to claim 1 or 5, characterized in that In step (3), the concentration of the polyvinyl pyrrolidone aqueous solution is 5-15 mg / mL, the concentration of the copper salt aqueous solution is 0.05-0.15 mmol / L, the concentration of the ascorbic acid aqueous solution is 0.01-5 mol / L, and the copper salt is at least one of copper chloride, copper nitrate and copper sulfate.

7. The method for preparing the copper selenide@platinum composite material according to claim 1 or 5, characterized in that The mass fraction of the aqueous hydrogen peroxide solution in step (3) is 30%, and the volume ratio of the aqueous hydrogen peroxide solution to the selenium@platinum nanoparticle dispersion is 40-80 μL:1 mL.

8. The copper selenide@platinum composite material obtained by the preparation method as claimed in claim 1 has a core-shell structure, wherein the copper selenide nanospheres are cores and the platinum nanoparticles are shells grown on the surface of the copper selenide nanospheres.

9. Use of the copper selenide@platinum composite material obtained by the preparation method as claimed in claim 1 as a radiotherapy sensitizer and photothermal material in tumor treatment.

Citation Information

Patent Citations

  • Copper-based nano photo-thermal material, preparation method thereof and application of copper-based nano photo-thermal material in cancer treatment

    CN113633770A

  • Copolymer-associated nanomaterial

    US20110037029A1