Surface modified hard carbon as well as preparation method and application thereof
By evenly but not completely coating the surface of the hard carbon material with the piezoelectric material, a hard carbon material rich in closed pore structure is formed, which solves the shortcomings of the hard carbon anode material in fast charging performance and achieves high-capacity and high-efficiency sodium Ion embedding improves battery safety and lifespan.
Patent Information
- Application Number
- CN202410903460.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-01
AI Technical Summary
Existing hard carbon anode materials have problems such as high cost, low capacity, low first storage efficiency and poor fast charging performance in terms of fast charging performance, which affects the safety and life of the battery.
Using surface-modified hard carbon materials, piezoelectric materials (such as NaNbO3, NaTaO3, LiNbO3, LiTaO3, KNbO3) are uniformly but not completely coated on the hard carbon surface, and its piezoelectric effect is used to promote the rapid embedding of sodium ions to form a rich Hard carbon material with closed cell structure.
It achieves high capacity, high first-time storage efficiency and excellent fast charging performance, reduces production costs, and improves battery safety and life.
Smart Images

Figure CN118724062A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of novel energy storage batteries, and in particular to a surface-modified hard carbon material and a preparation method and application thereof. Background Art
[0002] Clean energy has the defects of intermittency and instability, which inevitably affect the stability and reliability of the power grid. To address this problem, photovoltaic or wind power must be equipped with low-cost, sustainable, long-life, and highly safe energy storage batteries. Although lithium-ion batteries are the mainstream of energy storage batteries at present, they are limited by lithium resources and have potential safety hazards. In contrast, sodium-ion batteries have the advantages of abundant resources, low cost, and good safety. They are suitable for large-scale energy storage and improve the reliability of new power. However, sodium ions cannot use graphite negative electrodes due to their large radius and incompatibility with carbon layers. Therefore, practical sodium-ion batteries generally use amorphous hard carbon as the negative electrode. At present, hard carbon negative electrodes face the disadvantages of high cost, low capacity, low initial storage efficiency, and poor fast charging performance, especially fast charging performance, which is related to the safety and life of the battery. The fast charging performance of hard carbon is closely related to its pore structure and surface structure. To improve the fast charging ability of the material, its pore structure and surface structure need to be regulated. Therefore, those skilled in the art provide a surface-modified hard carbon material and its preparation method and application to solve the problems raised in the above background technology. Summary of the invention
[0003] The object of the present invention is to provide a surface-modified hard carbon material and a preparation method and application thereof, so as to solve the problems raised in the above background technology.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] A surface-modified hard carbon material, the surface-modified hard carbon material is composed of hard carbon and a piezoelectric material on the surface, the weight ratio of the piezoelectric material to the hard carbon is 0.5 to 5:100; the hard carbon material is rich in closed-pore structure, the average diameter of the closed pores is greater than 5.0 nm, and the interlayer spacing of the carbon layer is greater than 0.40 nm. The piezoelectric material is selected from at least one of NaNbO3, NaTaO3, LiNbO3, LiTaO3, and KNbO3. The piezoelectric material is uniformly but not completely coated on the surface of the hard carbon. The surface-modified hard carbon material has high capacity, high first storage efficiency and excellent fast charging performance.
[0006] The present invention also discloses a method for preparing the surface-modified hard carbon, the steps of which are as follows:
[0007] 1) pre-burning the biochar in an oxidizing atmosphere;
[0008] 2) placing the pre-burned biomass charcoal in a protective reaction chamber and carbonizing it at high temperature under an inert atmosphere to obtain hard carbon;
[0009] 3) The piezoelectric material is uniformly coated on the surface of the hard carbon to obtain surface-modified hard carbon.
[0010] As a further embodiment of the present invention:
[0011] In step 1), the biochar is selected from coconut shell charcoal, bamboo charcoal, fruit core charcoal, charcoal, starch charcoal, and straw charcoal. Biochar is low-cost and renewable, rich in natural pore structure, and is conducive to obtaining high capacity. The biochar is placed in front of the reaction chamber for crushing and pickling. The crushing method is selected from ball milling, mechanical milling, and air flow milling. Preferably, the crushing is also required to be screened. After crushing and screening, the particle size of the biochar is 3 to 10 μm; the pickling solution contains hydrofluoric acid. After pickling, the concentration of silicon is reduced to below 100 ppm and the ash content is reduced to below 0.3%. Crushing and pickling are conducive to improving specific capacity and first coulomb efficiency. The oxidizing atmosphere is selected from air and oxygen, the pre-burning temperature is 400 to 600 ° C, and the pre-burning time is 1 to 3 hours. Through pre-burning, the carbon layer is easy to form a cross-linked structure, which is conducive to promoting the formation of closed pores during high-temperature carbonization. The oxygen-containing functional groups formed by pre-oxidation are also conducive to the uniform but not complete coating of subsequent piezoelectric materials.
[0012] As a further embodiment of the present invention:
[0013] In step 2), the carbonization temperature is 1200-1400°C, the inert gas is selected from nitrogen, argon, and helium, and the flow rate of the inert gas is 50-200 cm 3 / min, the heating rate is 1-5℃ / min, and the carbonization time is 2-4 hours. Under these conditions, the pre-oxidized biochar is effectively carbonized to form hard carbon, and obtains a closed-cell structure and a large pore size.
[0014] As a further embodiment of the present invention:
[0015] In step 3), the piezoelectric material is selected from at least one of NaNbO3, NaTaO3, LiNbO3, LiTaO3, and KNbO3, and the weight ratio of the piezoelectric material to the hard carbon is 0.5 to 5:100. Under this condition, the piezoelectric material can be uniformly but incompletely coated on the hard carbon. During the embedding process of the sodium ions into the hard carbon, stress will be generated, which will induce the piezoelectric effect and promote the rapid embedding of the sodium ions. The piezoelectric material is a commercial material. Preferably, the piezoelectric material is crushed before coating, and the crushing method is selected from ball milling, sand milling, and air flow milling. Preferably, the particle size after crushing is 10 to 100 nm.
[0016] The coating method is selected from high-speed mixing coating, ball milling coating or mechanical fusion coating. Mechanical fusion coating is used, which is conducive to achieving close combination of hard carbon material and piezoelectric material, forming piezoelectric effect, and achieving uniform and incomplete coating. The uniform and incomplete coating means that the piezoelectric material particles are evenly distributed on the surface of the hard carbon particles; the coating area accounts for 30% to 60% of the hard carbon surface area.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. The present invention uses low-cost, resource-sustainable biomass charcoal as a precursor, first pre-oxidizes it in an oxygen atmosphere, then obtains hard carbon with a rich pore structure through high-temperature carbonization in an inert atmosphere, and finally coats it with a piezoelectric material to obtain a hard carbon material with a surface modified with a piezoelectric material.
[0019] 2. The present invention adopts cheap and sustainable biomass carbon raw materials and a simple method to prepare hard carbon materials, which has low energy consumption, low cost, short cycle, and is conducive to large-scale production.
[0020] 3. The hard carbon prepared by the present invention forms abundant large-diameter closed pores through pre-oxidation of biomass carbon. The piezoelectric effect of the piezoelectric material can promote the diffusion of sodium ions in the carbon layer, which is conducive to achieving high specific capacity, high first coulomb efficiency, and excellent fast charging performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 X-ray diffraction pattern (XRD) of hard carbon prepared in Example 1 of the present invention;
[0022] Figure 2 This is a transmission electron microscope (TEM) photograph of the hard carbon prepared in Example 1 of the present invention;
[0023] Figure 3 This is a scanning electron microscope photo (SEM) of the surface modified hard carbon prepared in Preparation Example 1 of the present invention;
[0024] Figure 4 Ta element energy spectrum scanning (EDX) of the surface modified hard carbon prepared in Preparation Example 1 of the present invention;
[0025] Figure 5 This is the first charge and discharge curve of the surface modified hard carbon prepared in Preparation Example 1 of the present invention;
[0026] Figure 6 This is a cycle life diagram of the surface modified hard carbon prepared in Preparation Example 1 of the present invention;
[0027] Figure 7 This is a rate performance diagram of the surface modified hard carbon prepared in Preparation Example 1 of the present invention;
[0028] Figure 8 This is a SEM photo of the hard carbon prepared in Comparative Example 1;
[0029] Fig. 9 The charge and discharge curve of the hard carbon prepared in Comparative Example 1;
[0030] Fig.10 This is a rate performance diagram of the hard carbon prepared in Comparative Example 1;
[0031] Fig.11 This is the TEM photo of the hard carbon prepared in Comparative Example 4. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] See also Figures 1 to 11 In an embodiment of the present invention, a surface-modified hard carbon material and a preparation method and application thereof are provided, wherein the surface-modified hard carbon material is composed of hard carbon and a piezoelectric material on the surface, and the weight ratio of the piezoelectric material to the hard carbon is 0.5 to 5:100; the hard carbon material is rich in closed-pore structure, the average diameter of the closed pores is greater than 5.0 nm, and the interlayer spacing of the carbon layer is greater than 0.40 nm. The piezoelectric material is selected from at least one of NaNbO3, NaTaO3, LiNbO3, LiTaO3, and KNbO3. The piezoelectric material is uniformly but not completely coated on the surface of the hard carbon. The surface-modified hard carbon material has high capacity, high first storage efficiency, and excellent fast charging performance.
[0034] The present invention also discloses a method for preparing the surface-modified hard carbon, the steps of which are as follows:
[0035] 1) pre-burning the biochar in an oxidizing atmosphere;
[0036] 2) placing the pre-burned biomass charcoal in a protective reaction chamber and carbonizing it at high temperature under an inert atmosphere to obtain hard carbon;
[0037] 3) The piezoelectric material is uniformly coated on the surface of the hard carbon to obtain surface-modified hard carbon.
[0038] As a further embodiment of the present invention:
[0039] In step 1), the biochar is selected from coconut shell charcoal, bamboo charcoal, fruit core charcoal, charcoal, starch charcoal, and straw charcoal. Biochar is low-cost and renewable, rich in natural pore structure, and is conducive to obtaining high capacity. The biochar is placed in front of the reaction chamber for crushing and pickling. The crushing method is selected from ball milling, mechanical milling, and air flow milling. Preferably, the crushing is also required to be screened. After crushing and screening, the particle size of the biochar is 3 to 10 μm; the pickling solution contains hydrofluoric acid. After pickling, the concentration of silicon is reduced to below 100 ppm and the ash content is reduced to below 0.3%. Crushing and pickling are conducive to improving specific capacity and first coulomb efficiency. The oxidizing atmosphere is selected from air and oxygen, the pre-burning temperature is 400 to 600 ° C, and the pre-burning time is 1 to 3 hours. Through pre-burning, the carbon layer is easy to form a cross-linked structure, which is conducive to promoting the formation of closed pores during high-temperature carbonization. The oxygen-containing functional groups formed by pre-oxidation are also conducive to the uniform but not complete coating of subsequent piezoelectric materials.
[0040] As a further embodiment of the present invention:
[0041] In step 2), the carbonization temperature is 1200-1400°C, the inert gas is selected from nitrogen, argon, and helium, and the flow rate of the inert gas is 50-200 cm 3 / min, the heating rate is 1-5℃ / min, and the carbonization time is 2-4 hours. Under these conditions, the pre-oxidized biochar is effectively carbonized to form hard carbon, and obtains a closed-cell structure and a large pore size.
[0042] As a further embodiment of the present invention:
[0043] In step 3), the piezoelectric material is selected from at least one of NaNbO3, NaTaO3, LiNbO3, LiTaO3, and KNbO3, and the weight ratio of the piezoelectric material to the hard carbon is 0.5 to 5:100. Under this condition, the piezoelectric material can be uniformly but incompletely coated on the hard carbon. During the embedding process of the sodium ions into the hard carbon, stress will be generated, which will induce the piezoelectric effect and promote the rapid embedding of the sodium ions. The piezoelectric material is a commercial material. Preferably, the piezoelectric material is crushed before coating, and the crushing method is selected from ball milling, sand milling, and air flow milling. Preferably, the particle size after crushing is 10 to 100 nm.
[0044] The coating method is selected from high-speed mixing coating, ball milling coating or mechanical fusion coating. Mechanical fusion coating is used, which is conducive to achieving close combination of hard carbon material and piezoelectric material, forming piezoelectric effect, and achieving uniform and incomplete coating. The uniform and incomplete coating means that the piezoelectric material particles are evenly distributed on the surface of the hard carbon particles; the coating area accounts for 30% to 60% of the hard carbon surface area.
[0045] Preparation Case 1
[0046] 2 g D 50 Bamboo charcoal of about 6 μm was placed in a tube furnace and heated at 400°C for 2 hours in an air atmosphere. Then, Ar gas was introduced and the temperature was raised to 1200°C. The temperature was kept at this temperature for 4 hours to obtain a hard carbon material. The obtained material was an amorphous hard carbon material as shown in XRD analysis. Figure 1 TEM analysis shows that the hard carbon is rich in closed-pore structure, the pore size is greater than 5nm, and the interlayer spacing of the carbon layer is greater than 0.4nm. Figure 2 The NaTaO3 with a particle size of 10-100 nm and hard carbon were mixed evenly at a weight ratio of 1:100, and then fused and coated using a fusion coating machine. SEM and Ta element EDS surface scanning analysis showed that NaTaO3 coated the hard carbon evenly and incompletely, as shown in Figure 2. Figure 3 and Figure 4 .
[0047] The hard carbon-based material prepared in this preparation case is used as the working electrode, sodium metal is used as the counter electrode, glass fiber membrane is used as the diaphragm, 1 mol / L NaPF6 diethylene glycol dimethyl ether solution is used as the electrolyte, and a button cell is assembled to perform constant current charge and discharge tests with a voltage range of 0.01 to 2 V. At 0.1C (30 mA / g), the charge and discharge curve is as follows Figure 5 As shown in the figure, the first charge capacity can reach 338.2mAh / g, and the first storage efficiency can reach 88.6%. After 100 cycles at 1C, the capacity retention rate is 96.8%, which is Figure 6 The discharge capacity at 5C current is 88.2% of that at 0.1C current. Figure 7 After battery disassembly and testing, no sodium precipitation was found at 5C current.
[0048] Preparation Case 2
[0049] 2 g D 50 The fruit core carbon of about 5μm was placed in a tubular furnace and heated at 600℃ for 1 hour in an air atmosphere. Then, Ar gas was passed through and the temperature was raised to 1300℃. The material was kept at this temperature for 3 hours to obtain a hard carbon negative electrode material. The obtained material was analyzed as an amorphous hard carbon material by XRD. According to TEM analysis, the hard carbon is rich in closed-pore structure, the pore size is greater than 5nm, and the interlayer spacing of the carbon layer is greater than 0.4nm. LiTaO3 with a particle size of 10 to 100nm was mixed evenly with hard carbon in a weight ratio of 2:100, and a fusion coating machine was used for fusion coating. According to SEM and Ta element EDS surface scanning analysis, LiTaO3 uniformly and incompletely coated the hard carbon.
[0050] Using the same test method as preparation case 1, the first charge capacity at 0.1C was 341.4 mAh / g, the first storage efficiency was 88.9%, after 100 cycles at 1C, the capacity retention rate was 95.9%, and the discharge capacity at 5C current was 87.6% relative to the 0.1C current capacity retention rate. After battery disassembly and inspection, no sodium precipitation was found at 5C current.
[0051] Preparation Case 3
[0052] 2 grams of straw charcoal were placed in a tubular furnace, heated at 500°C in an air atmosphere for 1.5 hours, then changed to Ar gas, and the temperature was raised to 1400°C, kept at this temperature for 2 hours to obtain a hard carbon negative electrode. The obtained material was analyzed by XRD to be a low-crystalline hard carbon material. KNbO3 with a particle size of 10 to 100 nm was mixed evenly with hard carbon in a weight ratio of 2:100, and a fusion coating machine was used for fusion coating. According to SEM and Nb element EDS surface scanning analysis, KNbO3 uniformly and incompletely coated the hard carbon. According to the same test method as Example 1, the first charge capacity at 0.1C was 337.2mAh / g, the first storage efficiency was 89.5%, and the capacity retention rate was 96.1% after 100 cycles at 1C. The discharge capacity at 5C current was 86.6% relative to the 0.1C current capacity retention rate. After battery disassembly and detection, there was no sodium precipitation at 5C current.
[0053] Comparative Example 1
[0054] The preparation of hard carbon is the same as in Example 1, except that it is not coated with NaTaO3. Figure 8 The surface is relatively smooth. The electrochemical test conditions are the same as in Example 1. The test results show that the 0.1C first charge capacity is 297.6 mAh / g and the first storage efficiency is 82.7%. Fig. 9 The discharge capacity retention rate at 5C current is 77.3% relative to that at 0.1C current. Fig.10 After battery disassembly and testing, sodium precipitation occurred under 5C current.
[0055] Comparative Example 2
[0056] The preparation of hard carbon is the same as in Example 1, except that the weight ratio of NaTaO3 to hard carbon is 0.2: 100. The electrochemical test conditions are the same as in Example 1, and the test results show that the 0.1C first charge capacity is 302.8mAh / g, the first storage efficiency is 84.2%, and the discharge capacity at 5C current is 80.4% relative to the 0.1C current capacity retention rate. After battery disassembly and detection, sodium precipitation occurs at 5C current.
[0057] Comparative Example 3
[0058] The preparation of hard carbon is the same as in Example 1, except that the weight ratio of NaTaO3 to hard carbon is 8:100, and NaTaO3 completely covers the hard carbon. The electrochemical test conditions are the same as in Example 1, and the test results show that the first charge capacity at 0.1C is 301.1mAh / g, the first storage efficiency is 83.7%, and the discharge capacity at 5C current is 78.8% relative to the 0.2C current capacity retention rate. After battery disassembly and detection, sodium precipitation occurs at 5C discharge current.
[0059] Comparative Example 4
[0060] The preparation of hard carbon is the same as that of Example 1, except that the hard carbon is not pre-burned. After testing, there is no obvious closed-cell structure. Fig.11 The electrochemical test conditions were the same as those in Example 1. The test results showed that the first charge capacity at 0.1C was 291.5 mAh / g, the first storage efficiency was 85.1%, and the discharge capacity at 5C current was 82.7% relative to the 0.1C current capacity retention rate. After battery disassembly and testing, sodium precipitation occurred at 5C current.
[0061] Comparative Example 5
[0062] The preparation of hard carbon is the same as that of Example 1, except that the hard carbon is not pre-burned and is not coated with NaTaO3. The electrochemical test conditions are the same as those of Example 1. The test results show that the first charge capacity at 0.1C is 291.7mAh / g, the first storage efficiency is 80.5%, and the discharge capacity at 5C current is 73.5% relative to the 0.1C current capacity retention rate. After battery disassembly and testing, sodium precipitation occurs at 5C current.
[0063] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A surface-modified hard carbon material, characterized in that: The surface modified hard carbon material consists of hard carbon and piezoelectric material on the surface, and the weight ratio of the piezoelectric material to the hard carbon is 0.5-5:
100.
2. A surface-modified hard carbon material according to claim 1, characterized in that: The hard carbon material is rich in closed-pore structure, the average diameter of the closed pores is greater than 5.0 nm, and the interlayer spacing of the carbon layers is greater than 0.40 nm.
3. The surface-modified hard carbon material according to claim 1, characterized in that: The piezoelectric material is selected from at least one of NaNbO3, NaTaO3, LiNbO3, LiTaO3, and KNbO3.
4. The method for preparing a surface-modified hard carbon material according to claim 1, characterized in that: The preparation steps are as follows: 1) pre-burning the biochar in an oxidizing atmosphere; 2) placing the pre-burned biomass charcoal in a protective reaction chamber and carbonizing it at high temperature under an inert gas to obtain hard carbon; 3) The piezoelectric material is uniformly coated on the surface of the hard carbon to obtain surface-modified hard carbon.
5. The method for preparing a surface-modified hard carbon material according to claim 4, characterized in that: In step 1), the biomass charcoal is selected from at least one of wood charcoal, coconut shell charcoal, bamboo charcoal, fruit core charcoal, starch charcoal, and straw charcoal; The oxidizing atmosphere is selected from air and oxygen; The pre-firing temperature is 400-600° C., and the pre-firing time is 1-3 hours.
6. The method for preparing a surface-modified hard carbon material according to claim 1, characterized in that: In step 2), the carbonization temperature is 1200-1400° C. and the carbonization time is 2-4 hours; The inert gas is selected from nitrogen, argon and helium.
7. The method for preparing a surface-modified hard carbon material according to claim 1, characterized in that: In step 1), in the surface-modified hard carbon material, the piezoelectric material uniformly but not completely covers the hard carbon.
8. Use of the surface-modified hard carbon material according to any one of claims 1 to 7 in sodium ion batteries.