Sulfur autotrophic filler and preparation method thereof

By using porous diatomaceous earth and reinforced diatomaceous earth as carriers in sulfur autotrophic fillers, combining trace elements and activated carbon, the problems of slow adhesion and long periods of traditional sulfur autotrophic denitrification fillers are solved, and efficient nitrates are achieved Nitrogen removal and low cost production.

CN118724272BActive Publication Date: 2024-11-19HOHAI UNIV +2

Patent Information

Application Number
CN202411215030.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-19
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

During the use of traditional sulfur autotrophic denitrification fillers, there are problems such as lower effluent pH, slow microorganism adhesion, and long cycles, and require a large amount of organic matter as carbon source and electron donor, resulting in poor heterotrophic denitrification effect.

Method used

Sulfur autotrophic filler consisting of 60~85% sulfur, 1~20% limestone, 1~10% iron tailings, 1~5% diatomaceous earth, 1~5% activated carbon and 1~5% trace elements, and is passed through carbonic acid Treatment and calcination form porous diatomaceous earth, increasing the colonization site of bacteria, and increasing porosity through alkali treatment and hydrochloric acid reaction, forming strengthened diatomaceous earth to improve the mechanical properties and denitrification efficiency of the filler.

Benefits of technology

The sulfur autotrophic filler with rapid in-use, high strength, high purification efficiency and little microbial loss is achieved, which improves the deep denitrification effect of nitrate nitrogen in wastewater, reduces the risk of effluent biological pollution, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724272B_ABST
    Figure CN118724272B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of sewage treatment, and specifically relates to a sulfur autotrophic filler and a preparation method thereof. Take diatomite and limestone, place them in a carbonic acid solution and mix them thoroughly, so that the carbonic acid penetrates deeply into the diatomite and then calcines to obtain porous diatomite; react the porous diatomite with sodium hydroxide to ionize part of the silicon in the diatomite to obtain alkali-treated diatomite; acidify the alkali-treated diatomite with hydrochloric acid to obtain reinforced diatomite; mix the reinforced diatomite with bacterial cells, so that the bacterial cells are colonized on the reinforced diatomite to obtain bacteria-containing diatomite; mix the bacteria-containing diatomite with other components to prepare a sulfur autotrophic filler. The sulfur autotrophic filler of the present invention has high sewage denitrification efficiency, is not easy to lose bacterial cells, and has good mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of sewage treatment, and in particular relates to a sulfur autotrophic filler and a preparation method thereof. Background Art

[0002] Generally, there are few bioavailable carbon sources in the secondary effluent of sewage treatment plants, and the C / N ratio is low. The denitrification effect of direct heterotrophic denitrification is extremely poor. Traditional heterotrophic denitrification technology requires the addition of a large amount of organic matter such as methanol, acetic acid and sodium acetate as energy and carbon sources due to the lack of electron donors during the treatment process. Autotrophic denitrification refers to the process in which autotrophic denitrifying bacteria (certain chemoautotrophic microorganisms) use inorganic carbon (CO2, HCO3 - 、CO3 2- ) as carbon sources, mainly inorganic substances (S, S2 - 、H2、S2O3 2- ,Fe,Fe 2+ NH4 + etc.) as electron donors for nitrate nitrogen reduction to complete microbial metabolism, converting NO3 - -N is reduced to N2. Research on autotrophic denitrification in the past 20 years at home and abroad has shown that autotrophic denitrifying bacteria have broad application prospects in treating nitrate nitrogen pollution in groundwater and surface water and deep denitrification of domestic sewage.

[0003] Some chemotrophic and phototrophic sulfur-oxidizing bacteria can utilize reduced sulfur (S 2- , S 0 , SO3 2- , S4O6 2- , S2O3 2- The denitrification capacity of different sulfides from strong to weak are S2O3 2- >FeS>FeS2>S) as electron donors, obtain energy through reduced sulfur, and use nitrate as electron acceptor to reduce it to nitrogen gas, completing the process of autotrophic denitrification. Sulfur autotrophic denitrification fillers are almost all granular or block solids, among which elemental sulfur and sulfide fillers have the advantages of low price, easy transportation, simple operation, etc., but there are still many problems in the process of use, such as the decrease of effluent pH with the progress of the reaction, slow microbial attachment, and long cycle. Summary of the invention

[0004] The present invention mainly provides a sulfur autotrophic filler which can be put into use quickly, has high strength, high purification efficiency and low microbial loss, and a preparation method thereof. The technical scheme is as follows:

[0005] A sulfur autotrophic filler and a preparation method thereof, comprising the following components by mass percentage: 60-85% sulfur, 1-20% limestone, 1-10% iron tailings, 1-5% diatomaceous earth, 1-5% activated carbon and 1-5% trace elements; the diatomaceous earth is bacteria-containing diatomaceous earth containing sulfur autotrophic denitrifying bacteria.

[0006] Furthermore, the sulfur autotrophic denitrifying bacteria include one or more of denitrifying Thiobacillus, denitrifying Thiospirillum, and denitrifying Thiomonas; and the trace elements include manganese, zinc, copper, cobalt, molybdenum, and nickel.

[0007] A method for preparing the above-mentioned sulfur autotrophic filler, the preparation steps of the sulfur autotrophic filler include: taking diatomaceous earth and limestone, placing them in a carbonic acid solution and mixing them thoroughly, allowing the carbonic acid to penetrate into the diatomaceous earth and then calcining to obtain porous diatomaceous earth; reacting the porous diatomaceous earth with sodium hydroxide to ionize part of the silicon in the diatomaceous earth, and obtaining alkali-treated diatomaceous earth; acidifying the alkali-treated diatomaceous earth with hydrochloric acid to obtain reinforced diatomaceous earth; mixing the reinforced diatomaceous earth with bacterial cells, allowing the bacterial cells to colonize on the reinforced diatomaceous earth, and obtaining bacteria-containing diatomaceous earth; mixing the bacteria-containing diatomaceous earth with other components to prepare the sulfur autotrophic filler.

[0008] Further, the following steps are included:

[0009] a. Prepare a saturated solution of carbonic acid at 3-8°C, place diatomaceous earth and limestone in the carbonic acid solution, and mix thoroughly until the precipitate no longer decreases; then heat to 70-90°C, stir and react until the precipitate no longer forms, separate and collect the precipitate, dry the precipitate thoroughly, and heat to 700-800°C at a rate of 3-8°C and calcine for 2-3 hours to obtain porous diatomaceous earth;

[0010] b. Mix the porous diatomaceous earth with sodium hydroxide, and stir the mixture at 70-80°C for 1-2 hours to ionize part of the silicon in the diatomaceous earth, thereby obtaining a reaction solution containing alkali-treated diatomaceous earth;

[0011] c. Add hydrochloric acid to the reaction solution while stirring until the pH value no longer changes; stop stirring and let stand for 3-5 hours, collect the precipitate, and obtain the reinforced diatomaceous earth;

[0012] d. Fully mix the fortified diatomaceous earth with trace elements and sulfur, add water to disperse, inoculate the activated bacteria, ferment at 200-220 rpm for 48-72 hours, collect the precipitate, and obtain the bacteria-containing diatomaceous earth;

[0013] e. Mix the bacteria-containing diatomaceous earth with other components and granulate them to obtain sulfur autotrophic filler.

[0014] Furthermore, the mass ratio of limestone to diatomaceous earth in step a is 1:3-5.

[0015] Furthermore, the mass ratio of sodium hydroxide to porous diatomaceous earth in step b is 1:8-12.

[0016] Furthermore, the mass ratio of sulfur to reinforced diatomaceous earth in step d is 1:2.5-3; and the inoculation amount of the bacterial cell planting in step d is 5-10%.

[0017] Furthermore, the preparation steps of the sulfur autotrophic filler include: dissolving sodium alginate in hot water, adding sodium polyacrylate, and mixing thoroughly to obtain a viscous liquid; adding bacteria-containing diatomaceous earth and other components to the viscous liquid, mixing evenly to obtain a paste, and then dripping the paste dropwise into a saturated boric acid solution, standing at 0-5°C for 6-12h, filtering and washing thoroughly, and drying below 35°C to obtain the filler.

[0018] Furthermore, the mass ratio of the sodium alginate to the polyacrylic acid is 1:3-8; the mass ratio of the sodium alginate to the bacteria-containing diatomaceous earth is 1:3-5.

[0019] Furthermore, the paste is poured into a mesh partition with a pore size of 3 to 20 mm, and dripped into a saturated boric acid solution drop by drop through the mesh of the partition to form spherical particles with a diameter of 3 to 20 mm.

[0020] By adopting the above scheme, the method of the present invention has the following advantages:

[0021] The sulfur autotrophic denitrifying bacteria of the sulfur autotrophic filler of the present invention are colonized on diatomaceous earth, and the filler contains bacterial bodies, which increases the concentration of microorganisms and reduces the bacterial colonization time in sewage. The bacteria grow quickly, the sewage denitrification efficiency is high, the bacterial bodies are not easily lost, and the risk of effluent biological pollution is reduced.

[0022] The present invention treats diatomite and limestone in carbonic acid to make calcium carbonate form soluble calcium bicarbonate, which penetrates into the pores inside the diatomite. The pores are enlarged by calcination to increase the surface area while making the added calcium element remain in the pores and not easy to escape, which is beneficial to the colonization of bacteria in the later stage.

[0023] The present invention ionizes part of silicon through alkali treatment, increases pores and generates sodium silicate, providing a basis for the subsequent formation of calcium silicate.

[0024] The bacterial cells of the present invention are deeply implanted in the macropores inside the diatomaceous earth, thereby improving the mechanical properties of the filler and the tolerance of microorganisms.

[0025] The sodium silicate of the present invention generates calcium silicate in the presence of hydrochloric acid and calcium ions, and the calcium silicate is evenly distributed in the pores after calcination and alkali treatment, and is fully combined with the diatomite matrix skeleton, thereby improving the compressive strength and impact resistance of the filler.

[0026] The calcium chloride obtained by reacting the residual calcium chloride in the reinforced diatomite with hydrochloric acid acts on the sodium alginate during the filler granulation process to cross-link the sodium alginate, thus saving the cost of adding additional calcium chloride and preventing other impurities from being introduced into the raw materials.

[0027] The composite filler of the present invention promotes the formation of a multiphase denitrification and dephosphorization reaction hot zone, accelerates the reaction speed, and the filler has a large specific surface area and good internal air permeability and mass transfer conditions, which can enable the microorganisms to fully contact the sulfur source in the filler, provide more binding sites, thereby improving the denitrification efficiency and providing a good environment for microbial growth.

[0028] The preparation method of the invention is simple, the raw materials are easily available and the product is single, the preparation cost is low, the products can be fully utilized, the waste generated is small, the processing difficulty is low, and it is environmentally friendly and safe. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Schematic diagram of pilot experiments of Examples 1 to 3;

[0030] Figure 2 is a graph showing changes in nitrate nitrogen concentrations in the inlet and outlet water of the pilot test in Example 1;

[0031] Figure 3 is a graph showing changes in total nitrogen concentrations in the inlet and outlet water of the pilot test in Example 1;

[0032] Figure 4 is a graph showing changes in nitrate nitrogen concentrations in the inlet and outlet water of the pilot test in Example 2;

[0033] Figure 5 is a graph showing changes in total nitrogen concentrations in the inlet and outlet water of the pilot test in Example 2;

[0034] Figure 6 is a graph showing changes in nitrate nitrogen concentrations in the inlet and outlet water of the pilot test in Example 3;

[0035] Figure 7 is a graph showing changes in total nitrogen concentrations in the inlet and outlet water of the pilot test in Example 3;

[0036] Figure 8 is a graph showing changes in total phosphorus concentrations in the influent and effluent of the pilot test in Example 1;

[0037] Fig. 9 is a graph showing the turbidity changes of the influent and effluent of the pilot test in Example 1;

[0038] Fig.10 is a graph showing changes in sulfate ion concentrations of influent and effluent in the pilot test of Example 1;

[0039] Fig.11is a graph showing changes in chloride ion concentrations of the influent and effluent of the pilot test in Example 1;

[0040] Figure 1 Middle: 1-autotrophic denitrification filter; 2-clean water tank; 3-blower; 4-backwash pump. DETAILED DESCRIPTION

[0041] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Example 1: (1) A saturated carbonic acid solution is prepared at 3°C, diatomaceous earth and limestone are placed in a carbonic acid solution at a mass ratio of 3:1, and the mixture is fully mixed until the precipitate no longer decreases; the temperature is then raised to 80°C, and the mixture is stirred to react until the precipitate no longer generates, the precipitate is separated and collected, and after the precipitate is fully dried, the temperature is raised to 750°C at a rate of 5°C and calcined for 2 hours to obtain porous diatomaceous earth;

[0043] (2) mixing porous diatomaceous earth and sodium hydroxide in a mass ratio of 8:1, stirring and reacting at 70-80°C for 1.5 hours to ionize part of the silicon in the diatomaceous earth, and obtaining a reaction solution containing alkali-treated diatomaceous earth;

[0044] (3) Adding hydrochloric acid to the reaction solution while stirring until the pH value no longer changes; stopping stirring and leaving the solution to stand for 3 hours, collecting the precipitate, and obtaining reinforced diatomaceous earth;

[0045] (4) Take fortified diatomaceous earth and sulfur in a mass ratio of 1:2.5, add trace elements and mix thoroughly, disperse with water, inoculate activated denitrifying Thiobacillus bacteria at an inoculum rate of 6%, ferment at a speed of 200-220 rpm for 60 h, collect the precipitate, and obtain bacterial diatomaceous earth;

[0046] (5) Take 1 part of sodium alginate and dissolve it in hot water, add 5 parts of sodium polyacrylate, and mix thoroughly to obtain a viscous liquid; add 3 parts of bacterial diatomaceous earth, 70 parts of industrial sulfur, 10 parts of limestone, 5 parts of iron tailings, 3 parts of trace elements and 2 parts of activated carbon to the viscous liquid, mix well to obtain a paste, and then pour the paste into a mesh partition with a pore size of 5 mm, drip into a saturated boric acid solution drop by drop through the mesh of the partition to form spherical particles with a diameter of 5 mm, let it stand at 0-5°C for 10 h, filter and wash thoroughly, and dry below 35°C to obtain a spherical sulfur autotrophic filler.

[0047] Example 2: (1) A saturated carbonic acid solution is prepared at 8°C, diatomaceous earth and limestone are placed in a carbonic acid solution at a mass ratio of 5:1, and the mixture is thoroughly mixed until the precipitate no longer decreases; the temperature is then raised to 80°C, and the mixture is stirred to react until the precipitate no longer forms, the precipitate is separated and collected, and after the precipitate is fully dried, the temperature is raised to 750°C at a rate of 5°C and calcined for 2 hours to obtain porous diatomaceous earth;

[0048] (2) mixing porous diatomaceous earth and sodium hydroxide in a mass ratio of 8:1, stirring and reacting at 70-80°C for 1.5 hours to ionize part of the silicon in the diatomaceous earth, and obtaining a reaction solution containing alkali-treated diatomaceous earth;

[0049] (3) Adding hydrochloric acid to the reaction solution while stirring until the pH value no longer changes; stopping stirring and leaving the solution to stand for 3 hours, collecting the precipitate, and obtaining reinforced diatomaceous earth;

[0050] (4) Take fortified diatomaceous earth and sulfur in a mass ratio of 1:2.5, add trace elements and mix thoroughly, disperse with water, inoculate activated denitrifying Thiobacillus bacteria at an inoculum rate of 6%, ferment at a speed of 200-220 rpm for 60 h, collect the precipitate, and obtain bacterial diatomaceous earth;

[0051] (5) Take 1 part of sodium alginate and dissolve it in hot water, add 5 parts of sodium polyacrylate, and mix thoroughly to obtain a viscous liquid; add 3 parts of bacterial diatomaceous earth, 70 parts of industrial sulfur, 10 parts of limestone, 5 parts of iron tailings, 3 parts of trace elements and 2 parts of activated carbon to the viscous liquid, mix well to obtain a paste, and then pour the paste into a mesh partition with a pore size of 5 mm, drip into a saturated boric acid solution drop by drop through the mesh of the partition to form spherical particles with a diameter of 5 mm, let it stand at 0-5°C for 10 h, filter and wash thoroughly, and dry below 35°C to obtain a sulfur autotrophic filler.

[0052] Example 3: (1) A saturated carbonic acid solution is prepared at 3°C, diatomaceous earth and limestone are placed in a carbonic acid solution at a mass ratio of 3:1, and the mixture is thoroughly mixed until the precipitate no longer decreases; the temperature is then raised to 80°C, and the mixture is stirred to react until the precipitate no longer forms, the precipitate is separated and collected, and after the precipitate is fully dried, the temperature is raised to 750°C at a rate of 5°C and calcined for 2 hours to obtain porous diatomaceous earth;

[0053] (2) mixing porous diatomaceous earth and sodium hydroxide in a mass ratio of 12:1, stirring and reacting at 70-80°C for 1.5 hours to ionize part of the silicon in the diatomaceous earth, and obtaining a reaction solution containing alkali-treated diatomaceous earth;

[0054] (3) Adding hydrochloric acid to the reaction solution while stirring until the pH value no longer changes; stopping stirring and leaving the solution to stand for 3 hours, collecting the precipitate, and obtaining reinforced diatomaceous earth;

[0055] (4) Take fortified diatomaceous earth and sulfur in a mass ratio of 1:2.5, add trace elements and mix thoroughly, disperse with water, inoculate activated denitrifying Thiobacillus bacteria at an inoculum rate of 6%, ferment at a speed of 200-220 rpm for 60 h, collect the precipitate, and obtain bacterial diatomaceous earth;

[0056] (5) Take 1 part of sodium alginate and dissolve it in hot water, add 5 parts of sodium polyacrylate, and mix thoroughly to obtain a viscous liquid; add 3 parts of bacterial diatomaceous earth, 70 parts of industrial sulfur, 10 parts of limestone, 5 parts of iron tailings, 3 parts of trace elements and 2 parts of activated carbon to the viscous liquid, mix well to obtain a paste, and then pour the paste into a mesh partition with a pore size of 5 mm, drip into a saturated boric acid solution drop by drop through the mesh of the partition to form spherical particles with a diameter of 5 mm, let it stand at 0-5°C for 10 h, filter and wash thoroughly, and dry below 35°C to obtain a sulfur autotrophic filler.

[0057] Example 4: (1) A saturated carbonic acid solution was prepared at 3°C, diatomaceous earth and limestone were placed in a carbonic acid solution at a mass ratio of 3:1, and the mixture was thoroughly mixed until the precipitate no longer decreased; the temperature was then raised to 80°C, and the mixture was stirred to react until the precipitate no longer generated, the precipitate was separated and collected, and after the precipitate was fully dried, the temperature was raised to 750°C at a rate of 5°C and calcined for 2 h to obtain porous diatomaceous earth;

[0058] (2) mixing porous diatomaceous earth and sodium hydroxide in a mass ratio of 10:1, stirring and reacting at 70-80°C for 1.5 hours to ionize part of the silicon in the diatomaceous earth, and obtaining a reaction solution containing alkali-treated diatomaceous earth;

[0059] (3) Adding hydrochloric acid to the reaction solution while stirring until the pH value no longer changes; stopping stirring and leaving the solution to stand for 3 hours, collecting the precipitate, and obtaining reinforced diatomaceous earth;

[0060] (4) Take fortified diatomaceous earth and sulfur in a mass ratio of 1:2.5, add trace elements and mix thoroughly, disperse with water, inoculate activated denitrifying Thiobacillus bacteria at an inoculum rate of 6%, ferment at a speed of 200-220 rpm for 60 h, collect the precipitate, and obtain bacterial diatomaceous earth;

[0061] (5) Take 1 part of sodium alginate and dissolve it in hot water, add 5 parts of sodium polyacrylate, and mix thoroughly to obtain a viscous liquid; add 3 parts of bacterial diatomaceous earth, 70 parts of industrial sulfur, 10 parts of limestone, 5 parts of iron tailings, 3 parts of trace elements and 2 parts of activated carbon to the viscous liquid, mix well to obtain a paste, and then pour the paste into a mesh partition with a pore size of 5 mm, drip into a saturated boric acid solution drop by drop through the mesh of the partition to form spherical particles with a diameter of 5 mm, let it stand at 0-5°C for 10 h, filter and wash thoroughly, and dry below 35°C to obtain a sulfur autotrophic filler.

[0062] Example 5: (1) A saturated carbonic acid solution is prepared at 3°C, diatomaceous earth and limestone are placed in a carbonic acid solution at a mass ratio of 3:1, and the mixture is thoroughly mixed until the precipitate no longer decreases; the temperature is then raised to 80°C, and the mixture is stirred to react until the precipitate no longer forms, the precipitate is separated and collected, and after the precipitate is fully dried, the temperature is raised to 750°C at a rate of 5°C and calcined for 2 hours to obtain porous diatomaceous earth;

[0063] (2) mixing porous diatomaceous earth and sodium hydroxide in a mass ratio of 8:1, stirring and reacting at 70-80°C for 1.5 hours to ionize part of the silicon in the diatomaceous earth, and obtaining a reaction solution containing alkali-treated diatomaceous earth;

[0064] (3) Adding hydrochloric acid to the reaction solution while stirring until the pH value no longer changes; stopping stirring and leaving the solution to stand for 5 hours, collecting the precipitate, and obtaining reinforced diatomaceous earth;

[0065] (4) Take fortified diatomaceous earth and sulfur in a mass ratio of 1:2.5, add trace elements and mix thoroughly, disperse with water, inoculate activated denitrifying Thiobacillus bacteria at an inoculum rate of 6%, ferment at a speed of 200-220 rpm for 60 h, collect the precipitate, and obtain bacterial diatomaceous earth;

[0066] (5) Take 1 part of sodium alginate and dissolve it in hot water, add 5 parts of sodium polyacrylate, and mix thoroughly to obtain a viscous liquid; add 3 parts of bacterial diatomaceous earth, 70 parts of industrial sulfur, 10 parts of limestone, 5 parts of iron tailings, 3 parts of trace elements and 2 parts of activated carbon to the viscous liquid, mix well to obtain a paste, and then pour the paste into a mesh partition with a pore size of 5 mm, drip into a saturated boric acid solution drop by drop through the mesh of the partition to form spherical particles with a diameter of 5 mm, let it stand at 0-5°C for 10 h, filter and wash thoroughly, and dry below 35°C to obtain a sulfur autotrophic filler.

[0067] Example 6: (1) A saturated carbonic acid solution was prepared at 3°C, diatomaceous earth and limestone were placed in a carbonic acid solution at a mass ratio of 3:1, and the mixture was thoroughly mixed until the precipitate no longer decreased; the temperature was then raised to 80°C, and the mixture was stirred to react until the precipitate no longer generated, the precipitate was separated and collected, and after the precipitate was fully dried, the temperature was raised to 750°C at a rate of 5°C and calcined for 2 h to obtain porous diatomaceous earth;

[0068] (2) mixing porous diatomaceous earth and sodium hydroxide in a mass ratio of 8:1, stirring and reacting at 70-80°C for 1.5 hours to ionize part of the silicon in the diatomaceous earth, and obtaining a reaction solution containing alkali-treated diatomaceous earth;

[0069] (3) Adding hydrochloric acid to the reaction solution while stirring until the pH value no longer changes; stopping stirring and leaving the solution to stand for 3 hours, collecting the precipitate, and obtaining reinforced diatomaceous earth;

[0070] (4) Take fortified diatomaceous earth and sulfur in a mass ratio of 1:2.5, add trace elements and mix thoroughly, disperse with water, inoculate activated denitrifying Thiobacillus bacteria at an inoculum rate of 6%, ferment at a speed of 200-220 rpm for 60 h, collect the precipitate, and obtain bacterial diatomaceous earth;

[0071] (5) Dissolve 1 part of sodium alginate in hot water, add 5 parts of sodium polyacrylate, and mix thoroughly to obtain a viscous liquid; add 5 parts of bacterial diatomaceous earth, 70 parts of industrial sulfur, 10 parts of limestone, 5 parts of iron tailings, 5 parts of trace elements and 2 parts of activated carbon to the viscous liquid, mix well to obtain a paste, and then pour the paste into a mesh partition with a pore size of 5 mm, drip into a saturated boric acid solution drop by drop through the mesh of the partition to form spherical particles with a diameter of 5 mm, let stand at 0-5°C for 10 h, filter and wash thoroughly, and dry below 35°C to obtain a sulfur autotrophic filler.

[0072] Comparative Example 1: (1) A saturated carbonic acid solution was prepared at 3°C, diatomaceous earth and limestone were placed in a carbonic acid solution at a mass ratio of 3:1, and the mixture was thoroughly mixed until the precipitate no longer decreased; the temperature was then raised to 80°C, and the mixture was stirred to react until the precipitate no longer generated, the precipitate was separated and collected, and after the precipitate was fully dried, the temperature was raised to 750°C at a rate of 5°C and calcined for 2 h to obtain porous diatomaceous earth;

[0073] (2) Mixing porous diatomaceous earth and sodium hydroxide in a mass ratio of 8:1, stirring and reacting at 70-80°C for 1.5 hours to ionize part of the silicon in the diatomaceous earth, and obtaining a reaction solution containing alkali-treated diatomaceous earth; collecting and washing the precipitate to obtain alkali-treated diatomaceous earth;

[0074] (3) Take alkali-treated diatomaceous earth and sulfur in a mass ratio of 1:2.5, add trace elements and mix thoroughly, disperse with water, inoculate activated denitrifying Thiobacillus bacteria at an inoculum rate of 6%, ferment at a speed of 200-220 rpm for 60 h, collect the precipitate, and obtain bacterial diatomaceous earth;

[0075] (4) Take 1 part of sodium alginate and dissolve it in hot water, add 5 parts of sodium polyacrylate, and mix thoroughly to obtain a viscous liquid; add 3 parts of bacterial diatomaceous earth, 70 parts of industrial sulfur, 10 parts of limestone, 5 parts of iron tailings, 3 parts of trace elements and 2 parts of activated carbon to the viscous liquid, mix well to obtain a paste, and then pour the paste into a mesh partition with a pore size of 5 mm, drip into a saturated boric acid solution drop by drop through the mesh of the partition to form spherical particles with a diameter of 5 mm, let it stand at 0-5°C for 10 hours, filter and wash thoroughly, and dry below 35°C to obtain a sulfur autotrophic filler.

[0076] Comparative Example 2: (1) A saturated carbonic acid solution was prepared at 3°C, diatomaceous earth and limestone were placed in a carbonic acid solution at a mass ratio of 3:1, and the mixture was thoroughly mixed until the precipitate no longer decreased; the temperature was then raised to 80°C, and the mixture was stirred to react until the precipitate no longer generated, the precipitate was separated and collected, and after the precipitate was fully dried, the temperature was raised to 750°C at a rate of 5°C and calcined for 2 h to obtain porous diatomaceous earth;

[0077] (2) mixing porous diatomaceous earth and sodium hydroxide in a mass ratio of 8:1, stirring and reacting at 70-80°C for 1.5 hours to ionize part of the silicon in the diatomaceous earth, and obtaining a reaction solution containing alkali-treated diatomaceous earth;

[0078] (3) Adding hydrochloric acid to the reaction solution while stirring until the pH value no longer changes; stopping stirring and leaving the solution to stand for 3 hours, collecting the precipitate, and obtaining reinforced diatomaceous earth;

[0079] (4) Dissolve 1 part of sodium alginate in hot water, add 5 parts of sodium polyacrylate, and mix thoroughly to obtain a viscous liquid; add 3 parts of reinforced diatomaceous earth, 75 parts of industrial sulfur, 10 parts of limestone, 5 parts of iron tailings, 3 parts of trace elements and 2 parts of activated carbon to the viscous liquid, mix well to obtain a paste, and then pour the paste into a mesh partition with a pore size of 5 mm, drip into a saturated boric acid solution drop by drop through the mesh of the partition to form spherical particles with a diameter of 5 mm, let stand at 0-5°C for 10 h, filter and wash thoroughly, and dry below 35°C to obtain a sulfur autotrophic filler.

[0080] Example sample test:

[0081] according to Figure 1 The process is as follows, the sulfur autotrophic fillers of Examples 1 to 3 are respectively used in the autotrophic denitrification filter 1, and the pilot test is carried out under the action of the blower 3 and the backwash pump 4, and the water after entering the clear water tank 2. The inlet water and backwash water are the effluent from the secondary sedimentation tank of the sewage treatment plant, wherein the filler filling height is 1.15m; denitrification amount: ≥7mg / L; air washing intensity: 45-60m³ / (m²·h); water washing intensity: 15-20m³ / (m²·h); denitrification load: ≥0.45 kgNOX-N / m³d; backwashing sequence: air washing (3-5min)-steam-water combination (5-10min)-water washing (5-10min); device operation: 24h continuous operation; nitrogen drive frequency: 2 times / day; backwashing frequency: 1 time / 3 days.

[0082] The nitrate nitrogen and total nitrogen in the influent were measured, and the nitrate nitrogen and total nitrogen in the effluent were measured after the sewage treatment plant stayed for 20 minutes to evaluate the nitrogen removal effect. Figures 2~11 shown.

[0083] Depend on Figure 2 and Figure 3It can be seen that the average influent nitrate nitrogen of the filler of Example 1 is 19.95 mg / L, the average effluent nitrate nitrogen is 5.59 mg / L, and the average nitrate nitrogen load is 1.22 kgN / m 3 ·d. The average influent total nitrogen was 22.32 mg / L, the average effluent total nitrogen was 10.94 mg / L, and the average total nitrogen load was 0.96 kgN / m 3 ·d. Example 2 has less limestone involved in the reaction and a lower carbonic acid concentration. Figure 4 and Figure 5 It can be seen that the average influent nitrate nitrogen of the filler of Example 2 is 19.53 mg / L, the average effluent nitrate nitrogen is 8.3 mg / L, and the average nitrate nitrogen load is 0.71 kgN / m 3 ·d; the average influent total nitrogen was 20.1 mg / L, the average effluent total nitrogen was 10.83 mg / L, and the average total nitrogen load was 0.59 kgN / m 3 ·d. The average nitrate nitrogen load and total nitrogen nitrogen load of Example 2 are significantly lower than those of Example 1, indicating that the denitrification capacity of the sulfur autotrophic filler in Example 1 is stronger than that in Example 2. It may be that the pores that are conducive to bacterial colonization produced during the diatomaceous earth and limestone treatment process in Example 2 are less than those in Example 1. The calcium ions penetrate deeply into the diatomaceous earth during the carbonation treatment, as well as the greater amount of calcium carbonate, are conducive to improving the denitrification capacity of the sulfur autotrophic filler. The amount of sodium hydroxide added in Example 3 during the alkali treatment process is less than that in Example 1. Figure 6 and Figure 7 The average influent nitrate nitrogen content was 9.30 mg / L, the average effluent nitrate nitrogen content was 2.67 mg / L, and the average nitrate nitrogen load was 0.48 kgN / m 3 ·d; the average influent total nitrogen was 11.83 mg / L, the average effluent total nitrogen was 5.72 mg / L, and the average total nitrogen load was 0.45 kgN / m 3 ·d. The average nitrate nitrogen load and total nitrogen load of Example 3 are significantly lower than those of Example 1, indicating that the alkali treatment step can improve the total nitrogen removal effect of the sulfur autotrophic filler of the present invention.

[0084] The changes in total phosphorus, turbidity, sulfate and chloride ion concentrations of the influent and effluent treated with the filler of Example 1 were respectively Figures 8 to 11 As shown by Figure 8 It can be seen that the average influent total phosphorus of Example 1 is 0.4 mg / L, and the average effluent total phosphorus is 0.17 mg / L. The sulfur autotrophic filler of the present invention also has an obvious removal effect on phosphorus. Fig. 9 It can be seen that the sulfur autotrophic filler of the present invention can reduce the turbidity of sewage and promote sewage clarification. Fig.10 and Fig.11It can be seen from the changes in the concentrations of phosphate ions and chloride ions that the use of the sulfur autotrophic filler of the present invention for sewage treatment will not increase the concentrations of phosphate ions and chloride ions and will not introduce new pollutants.

[0085] The compressive strength test of each embodiment and comparative example was carried out using a servo multifunctional high and low temperature control testing machine. Three groups of each embodiment or comparative example were tested and the average value was taken. The results are as follows:

[0086]

[0087] As can be seen from the above table, compared with Example 1, less limestone is involved in the reaction, and the compressive strength of Example 2, which has a smaller carbonic acid concentration, has decreased. It may be that less calcium ions are introduced, and the calcium ions entering the diatomite are relatively reduced, so that less calcium silicate is produced, which affects the strength of the filler. During the alkali treatment process, the amount of sodium hydroxide added in Example 3 is the least, and Example 4 is between Example 3 and Example 1, and the compressive strength of Example 4 is the highest, indicating that the silicate ions produced by the alkali treatment are conducive to the formation of calcium silicate in the later stage, but the alkali treatment that may be too deep may affect the integrity of the diatomite skeleton, but affect its mechanical strength. The modification of the compressive strength on the basis of ensuring the integrity of the skeleton can produce a significant improvement in the compressive strength of Example 4. Example 5 was left to stand for more time than the example during the acid treatment process, and its compressive strength increased significantly, indicating that the operation of standing is conducive to the generation of calcium silicate and the stable combination with the diatomite skeleton in the internal pores of the diatomite. Comparative Example 1 was not acid-treated, that is, there was no additional step of producing calcium silicate, and the compressive strength decreased significantly.

[0088] In Example 6, more bacteria-containing diatomite was added during the granulation process than in Example 1, and its compressive strength was significantly increased, indicating that the bacteria-containing diatomite in the sulfur autotrophic filler of the present invention can improve the mechanical properties of the filler. In Comparative Example 2, the sulfur autotrophic filler was not colonized with bacteria, and its compressive strength was also significantly reduced, indicating that the colonization of bacteria inside the diatomite is also conducive to the improvement of the mechanical properties of the filler.

[0089] For those skilled in the art, various other corresponding changes and deformations can be made according to the technical solutions and concepts described above, and all of these changes and deformations should fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a sulfur autotrophic filler, characterized in that: In terms of mass percentage, it includes the following components: 60-85% sulfur, 1-20% limestone, 1-10% iron tailings, 1-5% diatomaceous earth, 1-5% activated carbon and 1-5% trace elements; The diatomaceous earth is a bacterial diatomaceous earth containing sulfur-containing autotrophic denitrifying bacteria; The preparation steps of the sulfur autotrophic filler include: taking diatomite and limestone, placing them in a carbonic acid solution and mixing them thoroughly, allowing the carbonic acid to penetrate into the diatomite, and then calcining to obtain porous diatomite; reacting the porous diatomite with sodium hydroxide to ionize part of the silicon in the diatomite, and obtaining alkali-treated diatomite; acidifying the alkali-treated diatomite with hydrochloric acid to obtain reinforced diatomite; mixing the reinforced diatomite with bacterial cells, allowing the bacterial cells to colonize on the reinforced diatomite, and obtaining bacteria-containing diatomite; mixing the bacteria-containing diatomite with other components to prepare the sulfur autotrophic filler.

2. The method for preparing the sulfur autotrophic filler according to claim 1, characterized in that: The sulfur autotrophic denitrifying bacteria include one or more of denitrifying Thiobacillus, denitrifying Thiospirillum, and denitrifying Thiomonas; and the trace elements include manganese, zinc, copper, cobalt, molybdenum, and nickel.

3. The method for preparing the sulfur autotrophic filler according to claim 1, characterized in that: The following steps are involved: a. Prepare a saturated solution of carbonic acid at 3-8°C, place diatomaceous earth and limestone in the carbonic acid solution, and mix thoroughly until the precipitate no longer decreases; then heat to 70-90°C, stir and react until the precipitate no longer forms, separate and collect the precipitate, dry the precipitate thoroughly, and heat to 700-800°C at a rate of 3-8°C and calcine for 2-3 hours to obtain porous diatomaceous earth; b. Mix the porous diatomaceous earth with sodium hydroxide, and stir the mixture at 70-80°C for 1-2 hours to ionize part of the silicon in the diatomaceous earth, thereby obtaining a reaction solution containing alkali-treated diatomaceous earth; c. Add hydrochloric acid to the reaction solution while stirring until the pH value no longer changes; stop stirring and let stand for 3-5 hours, collect the precipitate, and obtain the reinforced diatomaceous earth; d. Fully mix the fortified diatomaceous earth with trace elements and sulfur, add water to disperse, inoculate the activated bacteria, ferment at 200-220 rpm for 48-72 hours, collect the precipitate, and obtain the bacteria-containing diatomaceous earth; e. Mix the bacteria-containing diatomaceous earth with other components and granulate them to obtain sulfur autotrophic filler.

4. The method for preparing the sulfur autotrophic filler according to claim 3, characterized in that: The mass ratio of limestone to diatomaceous earth in step a is 1:3-5.

5. The method for preparing the sulfur autotrophic filler according to claim 3, characterized in that: The mass ratio of sodium hydroxide to porous diatomaceous earth in step b is 1:8-12.

6. The method for preparing the sulfur autotrophic filler according to claim 3, characterized in that: The mass ratio of sulfur to reinforced diatomaceous earth in step d is 1:2.5-3; the inoculation amount of the bacterial cell planting in step d is 5-10%.

7. The method for preparing the sulfur autotrophic filler according to claim 1, characterized in that: The preparation steps of the sulfur autotrophic filler include: dissolving sodium alginate in hot water, adding sodium polyacrylate, and mixing thoroughly to obtain a viscous liquid; adding bacteria-containing diatomaceous earth and other components into the viscous liquid, mixing evenly to obtain a paste, and then dripping the paste into a saturated boric acid solution drop by drop, standing at 0-5°C for 6-12 hours, filtering and washing thoroughly, and drying below 35°C to obtain the filler.

8. The method for preparing the sulfur autotrophic filler according to claim 7, characterized in that: The mass ratio of the sodium alginate to polyacrylic acid is 1:3-8; the mass ratio of the sodium alginate to bacteria-containing diatomaceous earth is 1:3-5.

9. The method for preparing the sulfur autotrophic filler according to claim 7, characterized in that: The paste is poured into a mesh partition with a pore size of 3 to 20 mm, and dripped dropwise into a saturated boric acid solution through the mesh of the partition to form spherical particles with a diameter of 3 to 20 mm.

Citation Information

Patent Citations

  • Mud based dechlorinating agent and its preparing method

    CN101584963A

  • Compound bacterium agent / immobilized cell microorganism method for treating polyester wastewater

    CN102583781A

  • Boric acid modified active carbon and preparation method thereof

    CN103551115A

  • Desulfurizer containing diatomite and preparation method thereof

    CN103736452A

  • Diatomite ceramic biological membrane filtering core for sewage treatment, and preparation method thereof

    CN110697908A

Cited By

  • High-porosity anti-mineralization sulfur autotrophic denitrification filter material capable of slowly releasing trace elements and preparation method of high-porosity anti-mineralization sulfur autotrophic denitrification filter material

    CN121361892A