Hot press molding press and crystal glass hot press molding method

Through the hot press forming press and the crystal glass hot press forming method, the problem of low yield in glass parts processing is solved, efficient glass molding and polishing is achieved, the yield is improved and the cost is reduced.

CN118724431APending Publication Date: 2024-10-01SICHUAN XUHONG OPTOELECTRONICS TECH +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410889426.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

During the processing of glass parts, there is a problem of low yield.

Method used

Using a hot press forming press and a crystal glass hot press forming method, the glass blank is placed between the first heating structure and the second heating structure, using the effects of heat radiation, heat conduction and pressure to form, and using cooling components to quickly cool it Then flame polishing is performed on the polished components to cover surface defects such as indentations caused by the pressing process.

Benefits of technology

It effectively improves the yield of glass parts, reduces raw material consumption and costs, avoids the problem of breakage caused by contact with cutting tools, and increases the yield of glass parts by 10% to 15%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724431A_ABST
    Figure CN118724431A_ABST
Patent Text Reader

Abstract

The invention provides a hot-press forming press machine and a crystal glass hot-press forming method, and the hot-press forming press machine comprises a workbench assembly; the heating assembly comprises a first heating structure and a second heating structure, the first heating structure is connected with the workbench assembly, and the second heating structure corresponds to the first heating structure; the driving assembly is connected with the second heating structure, and the second heating structure has a pressing state close to the first heating structure and a to-be-pressed state far away from the first heating structure; the cooling assembly and the heating assembly are correspondingly arranged; and the polishing assembly comprises a flame spray gun, and the flame spray gun is connected with the workbench assembly. According to the technical scheme, the problem that in the prior art, the yield is low in the glass part machining process is effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of glass processing, and in particular to a hot pressing molding press and a crystal glass hot pressing molding method. Background Art

[0002] Crystal parts are widely used in decoration, lighting, optical instruments and other fields due to their unique gloss and texture. With the rapid development of the automobile industry, the diversity and personalized needs of vehicle accessories are increasing, and crystal parts are often used in vehicle lighting, decoration, gear levers and function buttons.

[0003] Generally, in the process of processing crystal glass parts, CNC machining of blanks is usually adopted, and a series of processing procedures such as rough carving, fine carving, and polishing are performed on the blanks.

[0004] In the prior art, glass processing methods have problems such as low efficiency, low yield and high cost, such as CN106965365A. Summary of the invention

[0005] A technical problem to be solved by the present application is that in the process of glass parts processing, there is a problem of low yield.

[0006] In order to solve the above technical problems, the present application provides a hot pressing forming press and a crystal glass hot pressing forming method.

[0007] A hot pressing forming press provided according to the present application includes: a workbench assembly; a heating assembly, the heating assembly includes a first heating structure and a second heating structure, the first heating structure is connected to the workbench assembly, and the second heating structure is arranged corresponding to the first heating structure; a driving assembly, the driving assembly is connected to the second heating structure, and the second heating structure has a pressurizing state close to the first heating structure and a pressurizing state away from the first heating structure; a cooling assembly, the cooling assembly is arranged corresponding to the heating assembly; and a polishing assembly, the polishing assembly includes a flame spray gun, and the flame spray gun is connected to the workbench assembly.

[0008] In some embodiments, the cooling assembly includes a spray gun structure, which is disposed on both sides of the heating assembly. The spray gun structure includes a nozzle, and the spray gun structure is rotatably connected to the workbench assembly, and the nozzle is disposed toward the heating assembly.

[0009] In some embodiments, the spray gun structure also includes a spray gun, a guide rail and a mounting seat, the mounting seat is rotatably connected to the workbench assembly, the guide rail is set on the mounting seat, the spray gun is movably connected to the guide rail, the nozzle is located on the spray gun, and the spray gun has a cooling state close to the heating component and a cooling state away from the heating component.

[0010] According to another aspect of the present application, a crystal glass hot pressing molding method is also provided. The crystal glass hot pressing molding method adopts the above-mentioned hot pressing molding press. The crystal glass hot pressing molding method includes the following steps: placing the raw material on the first heating structure for preheating, and the driving component drives the second heating structure to move in the direction close to the first heating structure to press and mold the raw material; using the cooling component to cool the first heating structure, the second heating structure and the molded glass piece; the driving component drives the second heating structure to move away from the first heating structure to take out the glass piece; flame polishing the glass piece; and annealing the glass piece.

[0011] In some embodiments, the method satisfies the following conditions:

[0012] When x1>1mm, P≥15Mpa;

[0013] When 0mm<x1≤1mm, 5Mpa<P≤15Mpa;

[0014] When x1 = 0 mm, P = 5 MPa;

[0015] Wherein, x1 is the distance between the position of the first heating structure during the mold closing process and its position during the pressing state;

[0016] P is the pressure of the drive assembly.

[0017] In some embodiments, the method satisfies the following conditions: a release agent is sprayed on the surfaces of the first heating structure and the second heating structure; and the cooling component performs a swinging motion during the process of cooling the first heating structure, the second heating structure and the glass piece by the cooling component.

[0018] In some embodiments, the method satisfies the following conditions: when T1≤400° C., the driving component drives the second heating structure to move upward;

[0019] Wherein, T1 is the temperature of the glass element.

[0020] In some embodiments, the method satisfies the following conditions: preheating the glass piece using a flame spray gun, T2 = 700 ± 10°C;

[0021] Where T2 is the temperature of the flame spray gun.

[0022] In some embodiments, the method satisfies the following conditions: after preheating, the surface of the glass piece is polished using a flame spray gun; during the polishing process, 1mm≤d≤5mm, 1500℃≤T2≤2000℃, 2mm / s≤v≤3mm / s;

[0023] Where, d is the polishing flame diameter;

[0024] v is the moving speed of the polishing flame.

[0025] In some embodiments, the method satisfies the following condition: after polishing is completed, the flame spray gun is cooled down in steps and the glass piece is kept warm.

[0026] Through the above technical scheme, the hot pressing molding press provided by the present application places the glass blank between the first heating structure and the second heating structure, and the vertical driving component drives the second heating structure to press the blank downward. The blank is deformed under the action of thermal radiation, heat conduction and pressure, and is formed according to the outer shapes of the first heating structure and the second heating structure. The cooling component quickly cools the formed glass to facilitate the removal of the glass from between the first heating structure and the second heating structure. The removed glass is placed in the polishing component for flame polishing to slightly melt the glass surface and cover the surface defects such as indentations produced during the pressing process. The technical scheme of the present application effectively solves the problem of low yield in the glass parts processing process in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 A schematic diagram of the front view of the hot pressing press disclosed in an embodiment of the present application is shown;

[0029] Figure 2 A schematic flow chart of the crystal glass hot pressing forming method disclosed in the embodiment of the present application is shown.

[0030] Description of reference numerals:

[0031] 10. Workbench assembly; 20. Heating assembly; 21. First heating structure; 211. First mold; 212. First heating unit; 22. Second heating structure; 221. Second mold; 222. Second heating unit; 30. Driving assembly; 40. Cooling assembly. DETAILED DESCRIPTION

[0032] The following is a further detailed description of the implementation methods of the present application in conjunction with the accompanying drawings and examples. The detailed descriptions and drawings of the following examples are used to exemplarily illustrate the principles of the present application, but cannot be used to limit the scope of the present application. The present application can be implemented in many different forms and is not limited to the specific embodiments of the present application, but includes all technical solutions that fall within the scope of the claims.

[0033] The present application provides these embodiments to make the present application thorough and complete, and to fully express the scope of the present application to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of the materials, the numerical expressions and the numerical values ​​set forth in these embodiments should be interpreted as being merely exemplary, and not as limiting.

[0034] It should be noted that, in the description of this application, unless otherwise specified, the meaning of "multiple" is greater than or equal to two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on this application. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.

[0035] In addition, the words "first", "second" and similar words used in this application do not indicate any order, quantity or importance, but are only used to distinguish different parts. "Vertical" does not mean vertical in the strict sense, but is within the tolerance range. "Parallel" does not mean parallel in the strict sense, but is within the tolerance range. "Include" or "comprising" and similar words mean that the elements before the word include the elements listed after the word, and do not exclude the possibility of including other elements.

[0036] It should also be noted that in the description of this application, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device.

[0037] All terms used in this application have the same meaning as those understood by those of ordinary skill in the art to which this application belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, such as general dictionaries, should be interpreted as having a meaning consistent with their meaning in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined herein.

[0038] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered part of the specification.

[0039] like Figure 1 As shown, the hot pressing forming press disclosed in the embodiment of the present application includes: a workbench assembly 10, a heating assembly 20, a driving assembly 30, a cooling assembly 40 and a polishing assembly, the heating assembly 20 includes a first heating structure 21 and a second heating structure 22, the first heating structure 21 is connected to the workbench assembly 10, the second heating structure 22 is arranged corresponding to the first heating structure 21, the driving assembly 30 is connected to the second heating structure 22, the second heating structure 22 has a pressurizing state close to the first heating structure 21 and a pressurizing state away from the first heating structure 21, the cooling assembly is arranged corresponding to the heating assembly 20, and the polishing assembly includes a flame spray gun, which is connected to the workbench assembly 10.

[0040] By applying the technical solution of the embodiment of the present application, a glass blank is placed between the first heating structure 21 and the second heating structure 22, and the driving component 30 drives the second heating structure 22 to press the blank downward. The blank is deformed under the action of heat radiation, heat conduction and pressure, and is formed according to the outer shapes of the first heating structure 21 and the second heating structure 22. The cooling component 40 quickly cools the formed glass to facilitate the removal of the glass from between the first heating structure 21 and the second heating structure 22. The removed glass is placed in the polishing component for flame polishing, so that the surface of the glass is slightly melted to cover the surface defects such as the indentation produced during the pressing process. The technical solution of this embodiment effectively solves the problem of low yield in the glass parts processing process in the prior art.

[0041] like Figure 1 As shown, in the technical solution of this embodiment, the cooling assembly 40 includes a spray gun structure, which is arranged on both sides of the heating assembly 20. The spray gun structure includes a nozzle, and the spray gun structure is rotatably connected to the workbench assembly 10, and the nozzle is arranged toward the heating assembly 20. The rotation of the spray gun structure drives the nozzle to swing, and the nozzle sprays cooling gas to cool the heating assembly 20, so as to take out the formed glass piece. The spray gun structure includes multiple spray gun structures, and the multiple spray gun structures are evenly arranged on both sides of the heating assembly 20 to cool evenly over time. The spray gun structure is penetrated on the workbench assembly 10, and the spray gun structure is connected to the driven gear, and the driven gear is located on the side of the workbench assembly 10 away from the nozzle. The driving gear is connected to the output shaft of the motor, and the driving gear is meshed with multiple driven gears, and at the same time drives the multiple driven gears to rotate, and the multiple nozzles swing synchronously, and the cooling is more uniform.

[0042] like Figure 1As shown, in the technical solution of this embodiment, the spray gun structure also includes a spray gun, a guide rail and a mounting seat, the mounting seat is rotatably connected to the workbench assembly 10, the guide rail is arranged on the mounting seat, the spray gun is movably connected to the guide rail, the nozzle is located on the spray gun, and the spray gun has a cooling state close to the heating assembly 20 and a state to be cooled away from the heating assembly 20. The distance between the spray gun and the heating assembly 20 can be changed, thereby changing the distance between the nozzle and the heating assembly 20, so that the structure can be applied to the cooling of glass pieces of different sizes, and has stronger versatility. The bottom of the spray gun has a groove consistent with the shape of the guide rail, the guide rail is partially arranged in the groove, and the spray gun moves along the extension direction of the guide rail.

[0043] like Figure 1 As shown, in the technical solution of this embodiment, the first heating structure 21 includes a first mold 211 and a first heating part 212, and the first mold 211 is connected to the first heating part 212; the second heating structure includes a second mold 221 and a second heating part 222, and the second mold 221 is connected to the second heating part 222. The shapes of the first mold 211 and the second mold 221 are designed according to the shape of the glass product. The first heating part 212 is connected to the workbench assembly 10, and the second heating part 222 is connected to the driving assembly 30. The driving assembly 30 uses a hydraulic press. The driving assembly 30 drives the second heating part 222 to move in the vertical direction. The second heating part 222 and the first heating part 212 are close to each other so that the first mold 211 and the second mold 221 press the glass set therebetween into a desired shape.

[0044] like Figure 1 and Figure 2 As shown, in the technical solution of this embodiment, the hot pressing molding method of crystal glass adopts the above-mentioned hot pressing molding press, and the hot pressing molding method of crystal glass includes the following steps: placing the raw material on the first heating structure 21 for preheating, and the driving component 30 drives the second heating structure 22 to move in the direction close to the first heating structure 21 to press and mold the raw material; using the cooling component 40 to cool the first heating structure 21, the second heating structure 22 and the formed glass piece; the driving component 30 drives the second heating structure 22 to move away from the first heating structure 21 to take out the glass piece; flame polishing the glass piece; annealing the glass piece. The composition of the glass in this application is:

[0045] SiO2=69.13% B2O3=10.75% BaO=3.07% Na2O=10.40% K2O=6.29% As2O3=0.36% Firstly, the first mold 211 and the second mold 221 are designed according to the appearance of the glass piece, the first mold 211 is fixed on the first heating part 212, the second mold 221 is fixed on the second heating part 222, the glass is placed on the first mold 211, the first heating part 212 and the second heating part 222 preheat the glass, when the glass temperature is 600~700℃, the driving component 30 drives the second mold 221 to press down, and the glass is hot-pressed. Table 1 shows the molding effect of the glass under different preheating temperature conditions.

[0046] Table 1

[0047]

[0048] During the hot pressing process, the mold temperature is 550℃~600℃. When the temperature is lower than 550℃, the temperature difference with the raw material is too high, and the product is prone to cracks. When the temperature is higher than 600℃, the product is prone to stick to the mold. Table 2 shows the molding effect of glass under different mold temperature conditions.

[0049] Table 2

[0050]

[0051] like Figure 2 As shown, in the technical solution of this embodiment, the method meets the following conditions:

[0052] When x1>1mm, P≥15Mpa;

[0053] When 0mm<x1≤1mm, 5Mpa<P≤15Mpa;

[0054] When x1 = 0 mm, P = 5 MPa;

[0055] Wherein, x1 is the distance between the position of the first heating structure 21 during the mold closing process and its position during the pressing state;

[0056] P is the pressure of the driving assembly 30 .

[0057] During the molding process, the thermal expansion and contraction rates of different locations on the glass surface are different. If the pressure is small, it is easy to form concave and convex points on the glass surface. Therefore, when x1>1mm, P≥15Mpa. When 0mm<x1≤1mm, P≤15Mpa, to avoid the second mold 221 impacting the glass surface and causing the glass surface to break; 5Mpa<P, to avoid the problem of incomplete mold closing due to insufficient pressure. When x1=0mm, P=5Mpa, and keep it for more than 10 seconds to ensure that the glass is not prone to rebound after the mold is opened.

[0058] like Figure 2 As shown, in the technical solution of the embodiment of the present application, the method meets the following conditions: the first heating structure 21 and the second heating structure 22 are sprayed with a release agent; during the cooling process of the cooling component 40 cooling the first heating structure 21, the second heating structure 22 and the glass piece, the cooling component 40 performs a swinging motion. Before hot pressing, the molding surfaces of the first mold 211 and the second mold 221 are first sprayed with a release agent to reduce the occurrence of mold sticking. After the hot pressing molding is completed, the cooling component is started to cool the first mold 211, the second mold 221 and the glass piece. The spray gun sprays cooling gas to reduce the temperature of the glass piece to below 400°C, and the driving component 30 drives the second mold 221 away from the first mold 211 to open the mold. During the cooling process, the positions of the multiple spray guns are first adjusted so that the distance between the nozzle and the first mold 211 and the second mold 221 is 10cm to 15cm. When the distance is less than 10cm, the conical gas sprayed by the spray gun has a small coverage range and a poor cooling effect; when the distance is greater than 15cm, the entire device occupies a large space. During the cooling process, start the motor and control the spray gun to swing to avoid the problem of the glass part having a local temperature that is too low and a large temperature difference across the glass part, which may cause the product to break.

[0059] like Figure 2 As shown, in the technical solution of the embodiment of the present application, the method satisfies the following conditions: when T1≤400°C, the driving component 30 drives the second heating structure 22 to move upward;

[0060] Wherein, T1 is the temperature of the glass element.

[0061] When the temperature of the glass part is lower than 400℃, the glass part is basically shaped, and no micro-deformation will occur during the mold opening process, resulting in changes in the product shape.

[0062] like Figure 2 As shown, in the technical solution of the embodiment of the present application, the method meets the following conditions:

[0063] Use a flame spray gun to preheat the glass parts, T2 = 700 ± 10 ° C;

[0064] Where T2 is the temperature of the flame spray gun.

[0065] Preheat the glass to avoid the problem of glass pieces being partially heated during polishing and causing them to break. If the preheating temperature is too high, the glass will melt.

[0066] like Figure 2 As shown, in the technical solution of the embodiment of the present application, the method meets the following conditions:

[0067] After preheating, the surface of the glass piece is polished using a flame spray gun;

[0068] During polishing, 1mm≤d≤5mm, 1500℃≤T2≤2000℃, 2mm / s≤v≤3mm / s;

[0069] Where, d is the polishing flame diameter;

[0070] v is the moving speed of the polishing flame.

[0071] By using flames to melt defective areas of the glass locally, the liquid glass can achieve a self-leveling effect, and has a good polishing effect on areas with bumps and pits. The polishing flame diameter is selected according to the shape of the glass surface. Table 3 shows the effect of the polishing flame temperature and speed on the polishing effect.

[0072] Table 3

[0073]

[0074]

[0075] like Figure 2 As shown, in the technical solution of the embodiment of the present application, the method meets the following conditions:

[0076] After polishing, the flame spray gun is cooled down in steps and the glass is kept warm. The temperature of the polished glass is high. Direct cooling will cause the internal stress of the glass to increase sharply, resulting in glass cracking. Therefore, the glass needs to be cooled down in steps. First, the temperature of the spray gun is controlled at 700℃, the heat preservation time is 5 minutes, and then the temperature is uniformly reduced to 400℃, and the heat preservation time is five minutes.

[0077] Put the glass in an insulated box for annealing to further eliminate the residual stress inside the glass and improve product performance. The temperature of the insulated box is 200℃ and the annealing time is 2 hours.

[0078] Compared with traditional CNC processing, the crystal glass hot pressing molding method in this application will prevent the glass from contacting with the cutting tool or breaking due to collision during the processing. The yield rate can be increased by 10% to 15%, greatly reducing the consumption of raw materials and saving costs.

[0079] In summary, a hot pressing molding process for vehicle-mounted crystal decorative parts (crystal glass hot pressing molding method) includes raw material preparation, mold design, hot pressing molding, cooling demolding and post-processing steps. The hot pressing molding press for crystal parts (hot pressing molding press) includes a hydraulic system (drive component 30), a heating device (a first heating part 212 and a second heating part 222), a temperature control system and a cooling system. (Cooling component 40) The hydraulic system pressure is adjustable (0~25MPa), and the heating plate temperature range is from room temperature to 800℃; the pressure of the press is adjustable in stages, the temperature of the heating system is adjustable, and the temperature control system is precise; the molding mold (the first mold 211 and the second mold 221), the mold material needs to be selected from mold steel stainless steel with high corrosion resistance and high mechanical properties. This application uses a martensitic stainless steel with high hardness and high corrosion resistance; the mold size and contour shape need to reserve tolerances and margins based on the product size and the expansion coefficient of the raw material; processing technology; raw material preparation, according to the product size, select glass raw materials of suitable shape, and cut, polish, etc. to process the raw materials into suitable shapes; raw material preheating, heat the raw materials evenly to 600~700℃, and select the optimal temperature according to the product shape; when the temperature is lower than 600℃, the raw material is not fully softened.

[0080] Raw material selection: crystal glass:

[0081] SiO2=69.13% B2O3=10.75% BaO=3.07% Na2O=10.40% K2O=6.29% As2O3=0.36%.

[0082] After pressing, the raw material is prone to incomplete forming and breakage. When the temperature is higher than 700℃, the raw material is too soft and difficult to operate, and it is easy to deform when unloading. Preheating can be done by spray gun heating to evenly heat the raw material to the required temperature; for pressing, put the preheated raw material into the mold and turn on the hydraulic pressure; the mold temperature is 550℃~600℃. When the temperature is lower than 550℃, the temperature difference with the raw material is too high, and the product is prone to cracks. When the temperature is higher than 600℃, the product is easy to stick to the mold; the hydraulic pressure is divided into three stages. The first stage is high-pressure mold closing, and the pressure is ≥15Mpa. After contacting with the mold during pressing, the difference in thermal expansion and contraction rates at different positions on the glass surface will form a concave and convex surface. When the pressure is lower than 15MPa, the surface plane is not properly processed and it is easy to form concave and convex points; the second stage is controlled to a low pressure of 5~15MPa 1mm before the complete mold closing to prevent the impact force from causing the crystal The parts are broken; at this time, the smooth surface has been formed, the glass temperature has gradually decreased, and the texture has become hard. Continuing high pressure will easily crush and fracture it. If the pressure is lower than 5MPa, the mold cannot be closed due to insufficient pressure; the third stage, after closing the mold, use 5MPa to maintain pressure for 10 seconds; open the mold, open the mold after maintaining pressure; the mold opening is divided into two stages, the first stage is 1mm / s slow mold opening, after the mold is opened to the distance of 1mm between the upper mold and the upper surface of the glass, the second stage is mold separation, and the second stage is ≥50mm / s fast mold opening, there is no special restriction on the speed, and it is appropriately selected according to the equipment capacity and production efficiency; unloading, because the pressing mold and the glass body are still in a high temperature state, it needs to be cooled to separate the product from the mold safely to ensure that the product does not stick to the mold and does not deform. After unloading, it is transferred to the flame polishing preheating process. The cooling air gun (cooling component 40) is used for cooling, and the cooling air gun swings left and right to prevent the crystal parts from breaking due to excessive temperature difference; the product temperature is reduced to below 400°C, and the material is unloaded after full solidification to avoid micro deformation; the mold needs to be sprayed with a specific amount of release agent, combined with temperature control to prevent the crystal parts from sticking to the mold; after hot pressing and unloading, the product is transferred to the flame polishing preheating process, which requires a flame spray gun to evenly heat and keep warm, the flame temperature is 700±10°C, and the insulation time is 3min; when the insulation flame temperature is 700°C, the product is actually measured at about 600~700°C, too low preheating effect is poor, too high is easy to melt and deform; flame polishing is mainly aimed at surface point or pit defects after pressing; the diameter of the flame polishing spray gun head is 1mm~5mm, according to Selection of crystal part shape; The flame temperature of the flame spray gun reaches 1500℃~2000℃; The moving speed of the flame spray gun is 2mm / s~3mm / s; During flame polishing, the temperature and speed are controlled together to make the polished surface of the product melt slightly, covering the concave and convex points, ripples and other defects caused by the drop molding to achieve the polishing effect; Continue to heat and keep warm after flame polishing, the first stage of insulation, the flame temperature is 700±10℃, and the insulation time is 5min; the second stage of insulation flame temperature is 400±10℃, and the insulation time is 5min, and the temperature is slowly reduced in steps to prevent the product from generating stress due to rapid cooling, which leads to cracking; Put it into the insulation box for annealing for 5h, the temperature of the insulation box is 200℃, and the internal residual stress is completely removed to improve the product performance; The finished product is high-precision hot-pressed crystal parts.

[0083] So far, the embodiments of the present application have been described in detail. In order to avoid obscuring the concept of the present application, some details known in the art are not described. Based on the above description, those skilled in the art can fully understand how to implement the technical solution of the present application.

[0084] Although some specific embodiments of the present application have been described in detail by way of examples, it should be understood by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present application. It should be understood by those skilled in the art that the above embodiments may be modified or some technical features may be replaced by equivalents without departing from the scope and spirit of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there is no structural conflict.

Claims

1. A hot pressing press, It is characterized in that include: Workbench assembly (10); A heating assembly (20), the heating assembly (20) comprising a first heating structure (21) and a second heating structure (22), the first heating structure (21) being connected to the workbench assembly (10), and the second heating structure (22) being arranged corresponding to the first heating structure (21); a driving assembly (30), the driving assembly (30) being connected to the second heating structure (22), the second heating structure (22) having a pressure-applying state close to the first heating structure (21) and a pressure-ready state far from the first heating structure (21); A cooling component (40), the cooling component being arranged corresponding to the heating component (20); A polishing assembly, comprising a flame spray gun, wherein the flame spray gun is connected to the workbench assembly (10).

2. The hot press molding press according to claim 1, It is characterized in that The cooling assembly (40) comprises a spray gun structure, which is arranged on both sides of the heating assembly (20), and the spray gun structure comprises a nozzle, and the spray gun structure is rotatably connected to the workbench assembly (10), and the nozzle is arranged toward the heating assembly (20).

3. The hot press molding press according to claim 2, It is characterized in that The spray gun structure also includes a spray gun, a guide rail and a mounting seat, wherein the mounting seat is rotatably connected to the workbench assembly (10), the guide rail is arranged on the mounting seat, the spray gun is movably connected to the guide rail, the nozzle is located on the spray gun, and the spray gun has a cooling state close to the heating assembly (20) and a cooling state away from the heating assembly (20).

4. A crystal glass hot pressing molding method, It is characterized in that The hot pressing molding method for crystal glass adopts the hot pressing molding press machine described in any one of claims 1 to 3, and the hot pressing molding method for crystal glass comprises the following steps: The raw material is placed on the first heating structure (21) for preheating, and the driving component (30) drives the second heating structure (22) to move in a direction close to the first heating structure (21) to press and shape the raw material; Using the cooling component (40) to cool the first heating structure (21), the second heating structure (22) and the formed glass piece; The driving component (30) drives the second heating structure (22) to move away from the first heating structure (21) to take out the glass piece; flame polishing the glass piece; The glass piece is subjected to an annealing treatment.

5. The crystal glass hot pressing forming method according to claim 4, It is characterized in that The method meets the following conditions: When x 1 >1mm, P≥15Mpa; When 0mm<x 1 When ≤1mm, 5Mpa<P≤15Mpa; When x 1 =0mm, P=5Mpa; Among them, x 1 is the distance between the position of the first heating structure (21) during the mold closing process and its position during the pressing state; P is the pressure of the driving component (30).

6. The crystal glass hot pressing forming method according to claim 4, It is characterized in that The method meets the following conditions: A release agent is sprayed on the surfaces of the first heating structure (21) and the second heating structure (22); During the process in which the cooling component (40) cools the first heating structure (21), the second heating structure (22) and the glass piece, the cooling component (40) performs a swinging motion.

7. The crystal glass hot pressing forming method according to claim 4, It is characterized in that The method meets the following conditions: When T 1 ≤400° C., the driving component (30) drives the second heating structure (22) to move upward; Among them, T 1 is the temperature of the glass.

8. The crystal glass hot pressing forming method according to claim 4, It is characterized in that The method meets the following conditions: The glass piece is preheated by the flame spray gun, T 2 =700±10℃; Where T 2 is the temperature of the flame spray gun.

9. The crystal glass hot pressing forming method according to claim 8, It is characterized in that The method meets the following conditions: After preheating is completed, the surface of the glass piece is polished using the flame spray gun; During polishing, 1mm≤d≤5mm, 1500℃≤T 2 ≤2000℃, 2mm / s≤v≤3mm / s; Where, d is the polishing flame diameter; v is the moving speed of the polishing flame.

10. The crystal glass hot pressing forming method according to claim 9, It is characterized in that The method meets the following conditions: After polishing is completed, the flame spray gun is stepped down to keep the glass piece warm.

Citation Information

Patent Citations

  • Glass profiling device and glass profiling method

    CN107739145A

  • Electromagnetic assistance precision hot press forming method for small-bore optical glass element

    CN109678323A

  • Quartz glass rod flame polishing and annealing device and method thereof

    CN111825321A

  • Glass element forming equipment

    JP2005035833A

  • Press molding method for an optical element and apparatus therefor

    US5188650A