High-refraction high-dispersion optical glass

By optimizing the combination of SiO2, B2O3, La2O3, Y2O3, Gd2O3 and other ingredients, controlling the (SiO2+B2O3)/Y2O3 ratio, and adding other oxides, the thermal expansion and bubble problems of high refractive and high dispersion optical glass under temperature changes are solved. It achieves the effects of high refractive index, low thermal expansion coefficient and excellent bubble degree.

CN118724459AInactive Publication Date: 2024-10-01CDGM OPTICAL GLASS
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411138664.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-08-26
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing high-refractive and high-dispersion optical glass has a large thermal expansion coefficient in an environment with large temperature changes, causing changes in the imaging properties of optical elements. Unreasonable component design can easily cause bubbles in the glass, leading to scrapping of the glass.

Method used

Using a combination of SiO2+B2O3: 5~30%, La2O3+Y2O3+Gd2O3: 45~75%, ZrO2: 2~15%, Nb2O5: 1~15%, TiO2: 5~20%, control (SiO2 +B2O3)/Y2O3 is 0.2~3.5, add Ta2O5, RO, Rn2O, WO3, ZnO, Al2O3, Yb2O3, GeO2 and other ingredients to optimize the refractive index, Abbe number and thermal expansion coefficient, and improve the bubble degree.

Benefits of technology

It achieves optical glass with excellent bubble degree and low thermal expansion coefficient while maintaining high refractive index and Abbe number, improving the stability and internal quality of optical glass.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_10
    Figure SMS_10
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention provides high-refraction and high-dispersion optical glass, which comprises the following components in percentage by weight: 8-30% of SiO2 + B2O3; 45 to 75 percent of La2O3, Y2O3 and Gd2O3; zrO2: 2%-15%; 1 to 15% of Nb2O5; and 6 to 20% of TiO2, wherein the ratio of (SiO2 + B2O3) / Y2O3 is 0.2 to 3.5. Through reasonable component design, the optical glass obtained by the invention has an expected refractive index and Abbe number, and also has excellent bubble degree and lower thermal expansion coefficient.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application for the invention patent application with application number 202211031626.X, application date August 26, 2022, and name “High refractive and high dispersion optical glass”. Technical Field

[0002] The invention relates to optical glass, in particular to high-refractive and high-dispersion optical glass. Background Art

[0003] In recent years, with the popularity of digital cameras, surveillance security, and vehicle-mounted imaging, the demand for optical components mounted on these devices has continued to increase. High-refractive and high-dispersion optical glass is an optical material that can be widely used in these instruments. Optical components installed in vehicle-mounted optical instruments, as well as optical components installed in heat-generating optical instruments such as projectors, copiers, and laser printers, are used in environments with large temperature changes. If the thermal expansion coefficient of the optical glass is too large, the thermal expansion of the optical components will occur due to changes in ambient temperature. Because the expansion coefficient is different from that of the optical component fixing fixture, stress is generated in the optical component, which in turn generates birefringence, causing changes in imaging characteristics. Therefore, it is expected that optical glass has a lower thermal expansion coefficient. On the other hand, in addition to the desired optical properties, optical glass must also have excellent internal quality (streaks, bubbles, inclusions, etc.). If the component design of the optical glass is unreasonable, it is easy to cause a large number of bubbles in the glass, resulting in the scrapping of the glass. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a high-refractive and high-dispersion optical glass with excellent bubble degree and low thermal expansion coefficient.

[0005] The technical solution adopted by the present invention to solve the technical problem is:

[0006] (1) High-refractive and high-dispersion optical glass, whose components, expressed in weight percentage, contain: SiO2+B2O3: 5-30%; La2O3+Y2O3+Gd2O3: 45-75%; ZrO2: 2-15%; Nb2O5: 1-15%; TiO2: 5-20%, of which (SiO2+B2O3) / Y2O3 is 0.2-3.5.

[0007] (2) The high-refractive and high-dispersion optical glass according to (1), wherein the components, expressed in weight percentage, further contain: Ta2O5: 0-5%; and / or RO: 0-10%; and / or Rn2O: 0-8%; and / or WO3: 0-5%; and / or ZnO: 0-10%; and / or Al2O3: 0-8%; and / or Yb2O3: 0-10%; and / or GeO2: 0-5%; and / or a clarifier: 0-2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

[0008] (3) High-refractive and high-dispersion optical glass, containing ZrO2, Nb2O5, and TiO2, wherein the composition, expressed in weight percentage, contains 5-30% SiO2+B2O3 and 45-75% La2O3+Y2O3+Gd2O3, wherein (SiO2+B2O3) / Y2O3 is 0.2-3.5, and the refractive index of the high-refractive and high-dispersion optical glass is greater than 1.97, the Abbe number is 25-34, and the thermal expansion coefficient α -30 / 70℃ 85×10 -7 / K or less, and the bubble degree is above grade A.

[0009] (4) The high-refractive and high-dispersion optical glass according to (3), wherein the components, expressed in weight percentage, contain: ZrO2: 2-15%; and / or Nb2O5: 1-15%; and / or TiO2: 5-20%; and / or Ta2O5: 0-5%; and / or RO: 0-10%; and / or Rn2O: 0-8%; and / or WO3: 0-5%; and / or ZnO: 0-10%; and / or Al2O3: 0-8%; and / or Yb2O3: 0-10%; and / or GeO2: 0-5%; and / or a clarifier: 0-2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

[0010] (5) The high-refractive and high-dispersion optical glass according to any one of (1) to (4), wherein the components thereof, expressed in weight percentage, satisfy one or more of the following eight conditions:

[0011] 1) (La2O3+TiO2) / Nb2O5 is 3.0 to 30.0, preferably (La2O3+TiO2) / Nb2O5 is 4.0 to 25.0, more preferably (La2O3+TiO2) / Nb2O5 is 5.0 to 20.0, and further preferably (La2O3+TiO2) / Nb2O5 is 5.5 to 15.0;

[0012] 2) Nb2O5 / Y2O3 is 0.1 to 2.0, preferably Nb2O5 / Y2O3 is 0.2 to 1.5, more preferably Nb2O5 / Y2O3 is 0.3 to 1.3, and further preferably Nb2O5 / Y2O3 is 0.3 to 1.0;

[0013] 3) Y2O3 / TiO2 is 0.3 to 3.0, preferably Y2O3 / TiO2 is 0.4 to 2.0, more preferably Y2O3 / TiO2 is 0.5 to 1.5, and further preferably Y2O3 / TiO2 is 0.7 to 1.3;

[0014] 4) (SiO2+B2O3) / Y2O3 is 0.4 to 3.0, preferably (SiO2+B2O3) / Y2O3 is 0.5 to 2.5, and more preferably (SiO2+B2O3) / Y2O3 is 0.7 to 1.8;

[0015] 5) (Nb2O5+WO3+Gd2O3) / TiO2 is 0.1 to 3.0, preferably (Nb2O5+WO3+Gd2O3) / TiO2 is 0.2 to 2.5, more preferably (Nb2O5+WO3+Gd2O3) / TiO2 is 0.3 to 2.0, and further preferably (Nb2O5+WO3+Gd2O3) / TiO2 is 0.4 to 1.5;

[0016] 6) (RO + ZnO) / Y2O3 is 1.0 or less, preferably (RO + ZnO) / Y2O3 is 0.8 or less, more preferably (RO + ZnO) / Y2O3 is 0.5 or less, and further preferably (RO + ZnO) / Y2O3 is 0.2 or less;

[0017] 7) (RO + Gd2O3) / Y2O3 is less than 1.0, preferably (RO + Gd2O3) / Y2O3 is less than 0.8, more preferably (RO + Gd2O3) / Y2O3 is less than 0.6, and further preferably (RO + Gd2O3) / Y2O3 is less than 0.3;

[0018] 8) (WO3+TiO2) / Y2O3 is 0.3 to 3.0, preferably (WO3+TiO2) / Y2O3 is 0.4 to 2.5, more preferably (WO3+TiO2) / Y2O3 is 0.5 to 2.0, and further preferably (WO3+TiO2) / Y2O3 is 0.7 to 1.5,

[0019] The RO is one or more of MgO, CaO, SrO and BaO.

[0020] (6) The high-refractive and high-dispersion optical glass according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: SiO2+B2O3: 8-25%, preferably SiO2+B2O3: 10-20%; and / or La2O3+Y2O3+Gd2O3: 50-75%, more preferably La2O3+Y2O3+Gd2O3: 55-70%; and / or ZrO2: 3-12%, preferably ZrO2: 4-10%; and / or Nb2O5: 3-12%, preferably Nb2O5: 5-10%; and / or Ta2O5: 0-3%, preferably Ta2O5: 0-1%; and / or TiO2: 6-18%, preferably TiO2: 8-15; and / or RO: 0-5%, preferably RO: 0-2% ; and / or Rn2O: 0-3%, preferably Rn2O: 0-2%; and / or WO3: 0-3%, preferably WO3: 0-2%; and / or ZnO: 0-5%, preferably ZnO: 0-2%; and / or Al2O3: 0-4%, preferably Al2O3: 0-2%; and / or Yb2O3: 0-5%, preferably Yb2O3: 0-2%; and / or GeO2: 0-3%, preferably GeO2: 0-1%; and / or clarifier: 0-1%, preferably clarifier: 0-0.5%, wherein RO is one or more of MgO, CaO, SrO, and BaO, Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

[0021] (7) The high-refractive and high-dispersion optical glass according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: SiO2: 1-15%, preferably SiO2: 2-10%, more preferably SiO2: 4-9%; and / or B2O3: 2-18%, preferably B2O3: 4-12%, more preferably B2O3: 5-10%; and / or La2O3: 35-65%, preferably La2O3: 40-60%, more preferably La2O3: 42-55%; and / or Y2O3: 5-25%, preferably Y2O3: 6-20%, more preferably Y2O3: 8-18%, further preferably Y2O3: 8-15%; and / or Gd2O3: 0-10%, preferably Gd2O3: 0-6%, more preferably Gd2O3: 0-4%.

[0022] (8) The high-refractive and high-dispersion optical glass according to any one of (1) to (4), wherein its components do not contain Ta2O5; and / or do not contain WO3; and / or do not contain Yb2O3; and / or do not contain RO; and / or do not contain Rn2O; and / or do not contain ZnO; and / or do not contain Al2O3; and / or do not contain GeO2, wherein RO is one or more of MgO, CaO, SrO, and BaO, and Rn2O is one or more of Li2O, Na2O, and K2O.

[0023] (9) The high-refractive and high-dispersion optical glass according to any one of (1) to (4), wherein the refractive index n of the high-refractive and high-dispersion optical glass is d is 1.97 or more, preferably 1.98 or more, more preferably 1.99 or more; the Abbe number v d It is 25-34, preferably 26-33, more preferably 27-32, further preferably 28-31.

[0024] (10) The high-refractive and high-dispersion optical glass according to any one of (1) to (4), wherein the density ρ of the high-refractive and high-dispersion optical glass is 5.20 g / cm 3 Below, preferably 5.10 g / cm 3 Below, more preferably 5.00 g / cm 3 Below; and / or thermal expansion coefficient α -30 / 70℃ 85×10 -7 / K or less, preferably 80×10 -7 / K or less, more preferably 75×10 -7 / K or less; and / or water resistance stability D W 2 or more, preferably 1; and / or acid resistance stability D A 2 or more, preferably 1; and / or weather resistance CR is 2 or more, preferably 1; and / or Knoop hardness H K 670×10 7 Pa or more, preferably 680×10 7 Pa or more, more preferably 690×10 7 Pa or more; and / or Young's modulus E is 11500×10 7 Pa~15500×10 7 Pa, preferably 12000×10 7 Pa~15000×10 7 Pa, more preferably 12500×10 7 Pa~14500×10 7 Pa, more preferably 13000×10 7 Pa~14000×10 7Pa; and / or the bubble degree is A grade or above, preferably A0 grade or above, more preferably A 00 Grade; and / or wear degree F A It is 80-125, preferably 85-115, and more preferably 90-105.

[0025] (11) A glass preform made of the high-refractive and high-dispersion optical glass described in any one of (1) to (10).

[0026] (12) An optical element made of the high-refractive and high-dispersion optical glass described in any one of (1) to (10), or made of the glass preform described in (11).

[0027] (13) An optical instrument comprising the high-refractive and high-dispersion optical glass described in any one of (1) to (10), and / or the optical element described in (12).

[0028] The beneficial effects of the present invention are as follows: through reasonable component design, the optical glass obtained by the present invention has a desired refractive index and Abbe number, and has excellent bubble degree and low thermal expansion coefficient. DETAILED DESCRIPTION

[0029] The following is a detailed description of the embodiments of the high-refractive and high-dispersion optical glass of the present invention, but the present invention is not limited to the following embodiments, and can be implemented by appropriate changes within the scope of the purpose of the present invention. In addition, although there are cases where the repeated description is appropriately omitted, the main purpose of the invention is not limited thereto. In the following content, the high-refractive and high-dispersion optical glass of the present invention is sometimes referred to as optical glass or glass.

[0030] [High refractive and high dispersion optical glass]

[0031] The following is an explanation of the range of each component (ingredient) of the high refractive and high dispersion optical glass of the present invention. In the present invention, unless otherwise specified, the content and total content of each component are all expressed in weight percentage (wt%), that is, the content and total content of each component are expressed in weight percentage relative to the total amount of glass material converted into oxide composition. Here, the "composition converted into oxide" means that when the oxides, complex salts and hydroxides used as raw materials for the optical glass components of the present invention decompose and transform into oxides during melting, the total amount of the oxide material is taken as 100%.

[0032] Unless otherwise specified in specific circumstances, the numerical ranges listed in the present invention include upper and lower limits, "above" and "below" include endpoint values, and all integers and fractions included in the range, without being limited to the specific values ​​listed when the range is defined. "And / or" referred to herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.

[0033] <Essential Components and Optional Components>

[0034] B2O3 is a glass network forming component, which has the effect of improving the glass solubility and resistance to devitrification, and reducing the glass transition temperature and density. The present invention obtains the above effects by containing more than 2% B2O3, preferably more than 4% B2O3, and more preferably more than 5% B2O3; but if its content exceeds 18%, the stability of the glass decreases, and the refractive index decreases, and it is difficult to achieve the high refractive index of the present invention. Therefore, the upper limit of the content of B2O3 in the present invention is 18%, preferably 12%, and more preferably 10%.

[0035] SiO2 is also a network-forming component, which can adjust the thermal expansion coefficient of glass, improve the resistance to devitrification and chemical stability of glass, and also improve the thermal stability and high-temperature viscosity of glass; if its content exceeds 15%, the melting performance of glass tends to deteriorate and the transition temperature increases. Therefore, the content of SiO2 in the present invention is 1 to 15%, preferably 2 to 10%, and more preferably 4 to 9%.

[0036] In some embodiments, by controlling the total content of SiO2 and B2O3 (SiO2+B2O3) within the range of 5 to 30%, the glass abrasion resistance and weather resistance can be optimized while maintaining the glass forming stability, and the glass devitrification resistance can be prevented from decreasing. Therefore, SiO2+B2O3 is preferably 5 to 30%, more preferably 8 to 25%, and further preferably 10 to 20%.

[0037] La2O3 is an effective component for improving the refractive index of glass, and has a significant effect on improving the chemical stability and resistance to devitrification of glass. If its content is less than 35%, it is difficult to achieve the required optical constants; if the content is higher than 65%, the devitrification tendency of the glass increases and the thermal stability deteriorates. Therefore, the content of La2O3 is limited to 35-65%, preferably 40-60%, and more preferably 42-55%.

[0038] Y2O3 can improve the refractive index and devitrification resistance of glass and adjust the Young's modulus of glass. The present invention achieves the above effects by containing more than 5% Y2O3; if its content exceeds 25%, the chemical stability and weather resistance of glass deteriorate. Therefore, the content of Y2O3 in the present invention is 5-25%, preferably 6-20%, more preferably 8-18%, and further preferably 8-15%.

[0039] In some embodiments, the ratio (SiO2+B2O3) / Y2O3 between the total content of SiO2 and B2O3 SiO2+B2O3 and the content of Y2O3 is controlled within the range of 0.2 to 3.5, which is beneficial to improving the bubble degree of the glass and preventing the increase of the thermal expansion coefficient of the glass. Therefore, it is preferred that (SiO2+B2O3) / Y2O3 is 0.2 to 3.5, and it is more preferred that (SiO2+B2O3) / Y2O3 is 0.4 to 3.0. Furthermore, controlling (SiO2+B2O3) / Y2O3 within the range of 0.5 to 2.5 can further improve the hardness and weather resistance of the glass. Therefore, it is further preferred that (SiO2+B2O3) / Y2O3 is 0.5 to 2.5, and it is further preferred that (SiO2+B2O3) / Y2O3 is 0.7 to 1.8.

[0040] Gd2O3 can improve the refractive index and chemical stability of glass, but if its content is higher than 10%, the devitrification resistance and abrasion resistance of glass will deteriorate. Therefore, the content of Gd2O3 is 0-10%, preferably 0-6%, and more preferably 0-4%.

[0041] In some embodiments, by controlling the total content of La2O3, Y2O3 and Gd2O3 La2O3+Y2O3+Gd2O3 within the range of 45-75%, the glass is more likely to obtain a desired refractive index and Abbe number, and optimize the devitrification resistance and weather resistance of the glass. Therefore, preferably La2O3+Y2O3+Gd2O3 is 45-75%, more preferably La2O3+Y2O3+Gd2O3 is 50-75%, and further preferably La2O3+Y2O3+Gd2O3 is 55-70%.

[0042] Yb2O3 is also a component that gives glass high refractive and low dispersion properties. If its content exceeds 8%, the anti-crystallization performance of the glass decreases. Therefore, the content of Yb2O3 is 0-10%, preferably 0-5%, more preferably 0-2%, and more preferably no Yb2O3 is contained.

[0043] ZrO2 can improve the viscosity, hardness, refractive index and chemical stability of optical glass, and can also reduce the thermal expansion coefficient of glass; when the content of ZrO2 is too high, the resistance to devitrification of glass decreases, the difficulty of melting increases, the melting temperature rises, and inclusions appear inside the glass and the light transmittance decreases. Therefore, the content of ZrO2 in the present invention is 2-15%, preferably 3-12%, and more preferably 4-10%.

[0044] TiO2 is a high-refractive and high-dispersion component, which can significantly improve the refractive index and dispersion of glass. The inventors have found that a proper amount of TiO2 can increase the stability of glass; but if too much TiO2 is contained, the transmittance of the glass will be significantly reduced, and the chemical stability of the glass will also tend to deteriorate. Therefore, the content of TiO2 in the present invention is 5-20%, preferably 6-18%, and more preferably 8-15%.

[0045] In some embodiments, by controlling the ratio of the content of Y2O3 to the content of TiO2, Y2O3 / TiO2, within the range of 0.3 to 3.0, the weather resistance of the glass can be improved and the abrasion resistance can be optimized. Therefore, it is preferred that Y2O3 / TiO2 is 0.3 to 3.0, and more preferably Y2O3 / TiO2 is 0.4 to 2.0. Furthermore, controlling Y2O3 / TiO2 within the range of 0.5 to 1.5 can further improve the chemical stability and bubble degree of the glass. Therefore, it is further preferred that Y2O3 / TiO2 is 0.5 to 1.5, and it is further preferred that Y2O3 / TiO2 is 0.7 to 1.3.

[0046] Nb2O5 is a high-refractive and high-dispersion component that can improve the refractive index and devitrification resistance of glass and reduce the thermal expansion coefficient of glass. In the present invention, the above effect is obtained by containing more than 1% Nb2O5. Preferably, the lower limit of the content of Nb2O5 is 3%, and the lower limit is more preferably 5%. If the content of Nb2O5 exceeds 15%, the thermal stability and weather resistance of the glass will decrease, and the light transmittance will decrease. Therefore, in the present invention, the upper limit of the content of Nb2O5 is 15%, preferably 12%, and more preferably 10%.

[0047] In some embodiments, by controlling the ratio of the total content of La2O3 and TiO2 La2O3+TiO2 to the content of Nb2O5 (La2O3+TiO2) / Nb2O5) within the range of 3.0 to 30.0, the chemical stability of the glass can be improved and the abrasiveness of the glass can be optimized. Therefore, it is preferred that (La2O3+TiO2) / Nb2O5 is 3.0 to 30.0, and it is more preferred that (La2O3+TiO2) / Nb2O5 is 4.0 to 25.0. Furthermore, by controlling (La2O3+TiO2) / Nb2O5 within the range of 5.0 to 20.0, the thermal expansion coefficient of the glass can be further reduced and the hardness of the glass can be improved. Therefore, it is further preferred that (La2O3+TiO2) / Nb2O5 is 5.0 to 20.0, and it is further preferred that (La2O3+TiO2) / Nb2O5 is 5.5 to 15.0.

[0048] In some embodiments, the ratio of Nb2O5 to Y2O3, Nb2O5 / Y2O3, is controlled within the range of 0.1 to 2.0, which can increase the Young's modulus of the glass while preventing the hardness of the glass from decreasing. Therefore, Nb2O5 / Y2O3 is preferably 0.1 to 2.0, and more preferably Nb2O5 / Y2O3 is 0.2 to 1.5. Furthermore, controlling Nb2O5 / Y2O3 within the range of 0.3 to 1.3 can further optimize the bubble degree and abrasion degree of the glass. Therefore, it is further preferred that Nb2O5 / Y2O3 is 0.3 to 1.3, and it is further preferred that Nb2O5 / Y2O3 is 0.3 to 1.0.

[0049] Alkaline earth metal oxide RO (RO is one or more of MgO, CaO, SrO, BaO) can adjust the optical constants of glass and optimize the chemical stability of glass, but when its content is high, the devitrification resistance of glass decreases. Therefore, the RO content is limited to 0-10%, preferably 0-5%, and more preferably 0-2%. In some embodiments, it is further preferred that RO is not contained.

[0050] In some embodiments, the ratio (RO+Gd2O3) / Y2O3 between the total content of RO and Gd2O3 RO+Gd2O3 and the content of Y2O3 is controlled to be below 1.0, which is beneficial to reducing the density of the glass, improving the chemical stability of the glass, and optimizing the Young's modulus and bubble degree of the glass. Therefore, it is preferred that (RO+Gd2O3) / Y2O3 is below 1.0, more preferably (RO+Gd2O3) / Y2O3 is below 0.8, further preferably (RO+Gd2O3) / Y2O3 is below 0.6, and further preferably (RO+Gd2O3) / Y2O3 is below 0.3.

[0051] Alkali metal oxide Rn2O (Rn2O is one or more of Li2O, Na2O, and K2O) can reduce the transition temperature of glass, adjust the optical constants and high-temperature viscosity of glass, and improve the melting property of glass. However, when its content is high, the devitrification resistance and chemical stability of glass are reduced. Therefore, the content of Rn2O in the present invention is 0 to 8%, preferably 0 to 3%, and more preferably 0 to 2%. In some embodiments, it is further preferred that Rn2O is not contained.

[0052] WO3 can improve the refractive index and mechanical strength of glass. If the content of WO3 exceeds 5%, the thermal stability of glass decreases and the resistance to devitrification decreases. Therefore, the upper limit of the content of WO3 is 5%, preferably 3%, and more preferably 2%. In some embodiments, it is further preferred not to contain WO3.

[0053] In some embodiments, the ratio of the total content of Nb2O5, WO3, and Gd2O3, Nb2O5+WO3+Gd2O3, to the content of TiO2 (Nb2O5+WO3+Gd2O3) / TiO2 is controlled within the range of 0.1 to 3.0, which can improve the light transmittance of the glass while preventing the density from increasing. Therefore, it is preferred that (Nb2O5+WO3+Gd2O3) / TiO2 is 0.1 to 3.0, and it is more preferred that (Nb2O5+WO3+Gd2O3) / TiO2 is 0.2 to 2.5. Furthermore, by controlling (Nb2O5+WO3+Gd2O3) / TiO2 within the range of 0.3 to 2.0, the thermal expansion coefficient of the glass can be further reduced and the Young's modulus can be increased. Therefore, it is further preferred that (Nb2O5+WO3+Gd2O3) / TiO2 is 0.3 to 2.0, and it is further preferred that (Nb2O5+WO3+Gd2O3) / TiO2 is 0.4 to 1.5.

[0054] In some embodiments, the ratio of the total content of WO3 and TiO2, WO3+TiO2, to the content of Y2O3, (WO3+TiO2) / Y2O3, is controlled within the range of 0.3 to 3.0, which is beneficial to improving the chemical stability of the glass and optimizing the abrasion resistance and Young's modulus. Therefore, (WO3+TiO2) / Y2O3 is preferably 0.3 to 3.0, more preferably (WO3+TiO2) / Y2O3 is 0.4 to 2.5, further preferably (WO3+TiO2) / Y2O3 is 0.5 to 2.0, and further preferably (WO3+TiO2) / Y2O3 is 0.7 to 1.5.

[0055] ZnO can adjust the refractive index and dispersion of glass, and reduce the high temperature viscosity and transition temperature of glass. If the content of ZnO is too high, the difficulty of glass molding increases and the anti-crystallization performance deteriorates. Therefore, the content of ZnO is 0 to 10%, preferably 0 to 5%, and more preferably 0 to 2%. In some embodiments, it is further preferred that ZnO is not contained.

[0056] In some embodiments, the ratio (RO+ZnO) / Y2O3 between the total content of RO and ZnO RO+ZnO and the content of Y2O3 is controlled to be less than 1.0, which can improve the weather resistance of the glass, optimize the abrasion resistance, and prevent the bubble degree and thermal expansion coefficient of the glass from deteriorating. Therefore, it is preferred that (RO+ZnO) / Y2O3 is less than 1.0, more preferably (RO+ZnO) / Y2O3 is less than 0.8, further preferably (RO+ZnO) / Y2O3 is less than 0.5, and further preferably (RO+ZnO) / Y2O3 is less than 0.2.

[0057] Ta2O5 has the effect of increasing the refractive index and improving the devitrification resistance of glass, but if its content is too high, the thermal stability of the glass will decrease and the density will increase; on the other hand, compared with other components, Ta2O5 is very expensive. From the perspective of practicality and cost, its usage should be minimized. Therefore, the content of Ta2O5 in the present invention is limited to 0-5%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that Ta2O5 is not contained.

[0058] Al2O3 can improve the chemical stability of glass, but when its content exceeds 8%, the meltability and light transmittance of glass deteriorate. Therefore, the content of Al2O3 in the present invention is 0 to 8%, preferably 0 to 4%, and more preferably 0 to 2%. In some embodiments, it is further preferred that Al2O3 is not contained.

[0059] GeO2 has the effect of increasing the refractive index and resistance to devitrification, but if its content is too high, the chemical stability of the glass will decrease; on the other hand, compared with other components, GeO2 is very expensive, and its usage should be minimized from the perspective of practicality and cost. Therefore, the content of GeO2 in the present invention is limited to 0-5%, preferably 0-3%, more preferably 0-1%, and it is further preferred that GeO2 is not contained.

[0060] In the present invention, by containing 0-2% of one or more components of Sb2O3, SnO, SnO2, and CeO2 as a clarifier, the clarification effect of the glass can be improved, and the bubble degree of the glass can be improved. The content of the clarifier is preferably 0-1%, and the content of the clarifier is more preferably 0-0.5%. Since the component types and contents of the optical glass of the present invention are reasonably designed and its bubble degree is excellent, it is further preferred that no clarifier is contained in some embodiments. When the content of Sb2O3 exceeds 2%, the glass tends to have reduced clarification performance. At the same time, due to its strong oxidizing effect, the corrosion of the platinum or platinum alloy vessel for melting glass and the deterioration of the forming mold are promoted. Therefore, the present invention preferably contains 0-2% of Sb2O3, more preferably 0-1%, further preferably 0-0.5%, and further preferably does not contain Sb2O3. SnO and SnO2 can also be used as clarifiers, but when their content exceeds 2%, the glass tends to increase in coloring, or when the glass is heated, softened, and molded again, Sn will become the starting point for nucleation, resulting in a tendency to devitrification. Therefore, the content of SnO2 in the present invention is preferably 0-2%, more preferably 0-1%, further preferably 0-0.5%, and further preferably does not contain SnO2; the content of SnO is preferably 0-2%, more preferably 0-1%, further preferably 0-0.5%, and further preferably does not contain SnO. The role and content ratio of CeO2 are consistent with those of SnO2, and its content is preferably 0-2%, more preferably 0-1%, further preferably 0-0.5%, and further preferably does not contain CeO2.

[0061] <Components that should not be contained>

[0062] In the glass of the present invention, even if oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo are contained alone or in combination in small amounts, the glass will be colored and absorption will occur at specific wavelengths in the visible light region, thereby weakening the property of the present invention of improving the visible light transmittance. Therefore, it is preferably substantially free of oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo, especially for optical glasses that require transmittance at wavelengths in the visible light region.

[0063] The oxides of Th, Cd, Tl, Os, Be and Se have a tendency to be controlled in recent years as harmful chemical substances, and environmental protection measures are necessary not only in the manufacturing process of glass, but also in the processing process and the disposal after productization. Therefore, in the case of paying attention to the impact on the environment, it is preferred that they are not actually contained except for being inevitably mixed in. Thus, the optical glass does not actually contain substances that pollute the environment. Therefore, even if special environmental countermeasures are not taken, the optical glass of the present invention can be manufactured, processed and discarded.

[0064] In order to achieve environmental friendliness, the high-refractive and high-dispersion optical glass of the present invention preferably does not contain As2O3 and PbO.

[0065] The "does not contain" and "0%" recorded in this article mean that the compound, molecule or element is not intentionally added as a raw material to the high-refractive and high-dispersion optical glass of the present invention; however, as raw materials and / or equipment for producing optical glass, there will be certain impurities or components that are not intentionally added, which will be contained in small amounts or trace amounts in the final optical glass, and this situation is also within the scope of protection of the patent of this invention.

[0066] Next, the properties of the high-refractive and high-dispersion optical glass of the present invention will be described.

[0067] <Refractive Index and Abbe Number>

[0068] The refractive index of optical glass (n d ) and the Abbe number (ν d ) Tested according to the method specified in GB / T 7962.1-2010.

[0069] In some embodiments, the refractive index (n d ) has a lower limit of 1.97, a preferred lower limit of 1.98, and a more preferred lower limit of 1.99.

[0070] In some embodiments, the refractive index (n d ) has an upper limit of 2.10, a preferred upper limit of 2.05, and a more preferred upper limit of 2.02.

[0071] In some embodiments, the Abbe number (ν d ) has a lower limit of 25, a preferred lower limit of 26, a more preferred lower limit of 27, and a further preferred lower limit of 28.

[0072] In some embodiments, the Abbe number (ν d ) has an upper limit of 34, a preferred upper limit of 33, a more preferred upper limit of 32, and a further preferred upper limit of 31.

[0073] <density>

[0074] The density (ρ) of optical glass is tested according to the method specified in GB / T7962.20-2010.

[0075] In some embodiments, the density (ρ) of the high refractive and high dispersion optical glass of the present invention is 5.20 g / cm 3 Below, preferably 5.10 g / cm 3 Below, more preferably 5.00 g / cm3 the following.

[0076] <Coefficient of Thermal Expansion>

[0077] Thermal expansion coefficient of optical glass (α -30 / 70℃ )The data at -30~70℃ were tested according to the method specified in GB / T7962.16-2010.

[0078] In some embodiments, the thermal expansion coefficient (α) of the high-refractive and high-dispersion optical glass of the present invention is -30 / 70℃ ) is 85×10 -7 / K or less, preferably 80×10 -7 / K or less, more preferably 75×10 -7 / K or less.

[0079] <Water resistance stability>

[0080] Water resistance stability of optical glass (D W )(Powder method) Tested according to the method specified in GB / T 17129.

[0081] In some embodiments, the water resistance stability (D W ) is 2 or more, preferably 1.

[0082] <Acid resistance stability>

[0083] Acid resistance stability of optical glass (D A )(Powder method) Tested according to the method specified in GB / T 17129.

[0084] In some embodiments, the acid resistance stability (D A ) is 2 or more, preferably 1.

[0085] <Weather resistance>

[0086] The test method for weather resistance (CR) of optical glass is as follows: place the sample in a test chamber with a saturated water vapor environment of 90% relative humidity, alternately cycle at 40-50°C every 1h, and cycle for 15 cycles. The weather resistance category is divided according to the change in turbidity before and after the sample is placed. The weather resistance classification is shown in Table 1:

[0087] Table 1.

[0088]

[0089] In some embodiments, the weather resistance (CR) of the high-refractive and high-dispersion optical glass of the present invention is Class 2 or higher, preferably Class 1.

[0090] <Knoop hardness>

[0091] Knoop hardness of optical glass (H K ) Test according to the test method specified in GB / T7962.18-2010.

[0092] In some embodiments, the Knoop hardness (H) of the high refractive and high dispersion optical glass of the present invention is K ) is 670×10 7 Pa or more, preferably 680×10 7 Pa or more, more preferably 690×10 7 Pa or above.

[0093] <Young's modulus>

[0094] Young's modulus (E) is calculated using the following formula using ultrasonic testing of the longitudinal wave velocity and transverse wave velocity.

[0095]

[0096]

[0097] Where:

[0098] E is Young's modulus, Pa;

[0099] G is the shear modulus, Pa;

[0100] V T is the shear wave velocity, m / s;

[0101] V S is the longitudinal wave velocity, m / s;

[0102] ρ is the glass density, g / cm 3 .

[0103] In some embodiments, the lower limit of the Young's modulus (E) of the high refractive and high dispersion optical glass of the present invention is 11500×10 7 Pa, the preferred lower limit is 12000×10 7 Pa, and the more preferred lower limit is 12500×10 7 Pa, and the lower limit is preferably 13000×10 7 Pa.

[0104] In some embodiments, the upper limit of the Young's modulus (E) of the high refractive and high dispersion optical glass of the present invention is 15500×10 7 Pa, the upper limit is preferably 15000×10 7 Pa, and the upper limit is more preferably 14500×10 7Pa, and the upper limit is preferably 14000×10 7 Pa.

[0105] <Abrasion>

[0106] Abrasiveness of optical glass (F A ) refers to the value obtained by multiplying the ratio of the wear volume of the sample to the wear volume (volume) of the standard sample (H-K9 glass) by 100 under exactly the same conditions, and is expressed by the following formula:

[0107]

[0108] Where:

[0109] V—volume wear of the sample being tested;

[0110] V0—Volume loss of standard sample;

[0111] W—mass wear loss of the sample being tested;

[0112] W0—standard sample mass wear;

[0113] ρ—density of the sample being tested;

[0114] ρ0—standard sample density.

[0115] In some embodiments, the abrasion degree (F A ) has a lower limit of 80, a preferred lower limit of 85, and a more preferred lower limit of 90.

[0116] In some embodiments, the abrasion degree (F A ) has an upper limit of 125, a preferred upper limit of 115, and a more preferred upper limit of 105.

[0117] <Bubble Degree>

[0118] The bubble degree of optical glass is tested according to the method specified in GB / T7962.8-2010.

[0119] In some embodiments, the bubble degree of the high refractive and high dispersion optical glass of the present invention is above grade A, preferably above grade A0, and more preferably above grade A1. 00 class.

[0120] [Method for producing optical glass]

[0121] The manufacturing method of the high-refractive and high-dispersion optical glass of the present invention is as follows: the glass of the present invention is produced using conventional raw materials and processes, including but not limited to using oxides, hydroxides, complex salts (such as carbonates, nitrates, sulfates, etc.), boric acid, etc. as raw materials, and after mixing according to conventional methods, the prepared furnace materials are put into a melting furnace (such as platinum or platinum alloy crucible) at 1200-1450°C for melting, and after clarification and homogenization, a homogeneous molten glass without bubbles and undissolved substances is obtained, and the molten glass is cast in a mold and annealed. Those skilled in the art can appropriately select raw materials, process methods and process parameters according to actual needs.

[0122] [Glass preforms and optical components]

[0123] The glass preform can be made from the high-refractive and high-dispersion optical glass by direct drop molding, grinding, or hot press molding. That is, the molten optical glass can be directly drop molded into a glass precision preform, or the glass preform can be made by mechanical processing such as grinding and grinding, or the preform for molding is made from the optical glass, and then the preform is hot-pressed and then ground to make the glass preform. It should be noted that the means for preparing the glass preform are not limited to the above means.

[0124] As described above, the high-refractive and high-dispersion optical glass of the present invention is useful for various optical elements and optical designs, among which it is particularly preferred to form a preform from the optical glass of the present invention, and use the preform to perform re-hot pressing, precision stamping, etc. to produce optical elements such as lenses and prisms.

[0125] The glass preform and optical element of the present invention are both formed by the high-refractive and high-dispersion optical glass of the present invention. The glass preform of the present invention has the excellent properties of the high-refractive and high-dispersion optical glass; the optical element of the present invention has the excellent properties of the high-refractive and high-dispersion optical glass, and can provide various optical elements such as lenses and prisms with high optical value.

[0126] Examples of the lens include various lenses having spherical or aspherical lens surfaces, such as a concave meniscus lens, a convex meniscus lens, a biconvex lens, a biconcave lens, a plano-convex lens, and a plano-concave lens.

[0127] [Optical instruments]

[0128] The optical element formed by the high-refractive and high-dispersion optical glass of the present invention can be used to manufacture optical instruments such as photographic equipment, video equipment, projection equipment, display equipment, vehicle-mounted equipment, and monitoring equipment.

[0129] Example

[0130] <High refractive and high dispersion optical glass example>

[0131] In order to further clearly illustrate and describe the technical solution of the present invention, the following non-limiting examples are provided.

[0132] This embodiment adopts the above optical glass manufacturing method to obtain high refractive and high dispersion optical glasses having the compositions shown in Tables 2 to 4. In addition, the properties of each glass are measured by the test method described in the present invention, and the measurement results are shown in Tables 2 to 4.

[0133] Table 2.

[0134]

[0135]

[0136] Table 3.

[0137]

[0138]

[0139] Table 4.

[0140]

[0141]

[0142] <Glass Preform Example>

[0143] The glass obtained from high-refractive and high-dispersion optical glass Examples 1 to 24# is used, for example, by grinding processing, or by molding methods such as re-hot pressing, precision stamping, etc., to make preforms of various lenses, prisms, etc., such as concave meniscus lenses, convex meniscus lenses, double convex lenses, double concave lenses, plano-convex lenses, and plano-concave lenses.

[0144] <Optical Element Embodiment>

[0145] The preforms obtained in the above-mentioned glass preform embodiments are annealed to reduce the internal stress of the glass and fine-tune the refractive index so that the optical properties such as the refractive index reach the desired values.

[0146] Next, each preform is ground and polished to produce various lenses and prisms such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses. The surface of the obtained optical element may be coated with an anti-reflection film.

[0147] <Optical Instrument Embodiment>

[0148] The optical element obtained by the above-mentioned optical element embodiment is optically designed to form an optical component or optical assembly by using one or more optical elements, and can be used in, for example, imaging equipment, sensors, microscopes, medical technology, digital projection, communications, optical communication technology / information transmission, optics / lighting in the automotive field, lithography technology, excimer lasers, wafers, computer chips, and integrated circuits and electronic devices including such circuits and chips.

Claims

1. High refractive and high dispersion optical glass, characterized in that: Its components, expressed in weight percentage, include: SiO2+B2O3: 8-30%; La2O3+Y2O3+Gd2O3: 45-75%; ZrO2: 2-15%; Nb2O5: 1-15%; TiO2: 6-20%, of which (SiO2+B2O3) / Y2O3 is 0.2-3.

5.

2. The high-refractive and high-dispersion optical glass according to claim 1, characterized in that: Its components are expressed in weight percentage, and also contain: Ta2O5: 0-5%; and / or RO: 0-10%; and / or Rn2O: 0-8%; and / or WO3: 0-5%; and / or ZnO: 0-10%; and / or Al2O3: 0-8%; and / or Yb2O3: 0-10%; and / or GeO2: 0-5%; and / or clarifier: 0-2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

3. High refractive and high dispersion optical glass, characterized in that: Contains ZrO2, Nb2O5, TiO2, and its components, expressed in weight percentage, contain 8-30% SiO2+B2O3 and 45-75% La2O3+Y2O3+Gd2O3, wherein (SiO2+B2O3) / Y2O3 is 0.2-3.5, and the refractive index of the high-refractive and high-dispersion optical glass is above 1.97, the Abbe number is 25-34, and the thermal expansion coefficient is α -30 / 70℃ 85×10 -7 / K or less, and the bubble degree is above grade A.

4. The high-refractive and high-dispersion optical glass according to claim 3, characterized in that: Its components are expressed in weight percentage and contain: ZrO2: 2-15%; and / or Nb2O5: 1-15%; and / or TiO2: 6-20%; and / or Ta2O5: 0-5%; and / or RO: 0-10%; and / or Rn2O: 0-8%; and / or WO3: 0-5%; and / or ZnO: 0-10%; and / or Al2O3: 0-8%; and / or Yb2O3: 0-10%; and / or GeO2: 0-5%; and / or clarifier: 0-2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

5. The high-refractive and high-dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage and meet one or more of the following eight conditions: 1) (La2O3+TiO2) / Nb2O5 is 3.0 to 30.0, preferably (La2O3+TiO2) / Nb2O5 is 4.0 to 25.0, more preferably (La2O3+TiO2) / Nb2O5 is 5.0 to 20.0, and further preferably (La2O3+TiO2) / Nb2O5 is 5.5 to 15.0; 2) Nb2O5 / Y2O3 is 0.1 to 2.0, preferably Nb2O5 / Y2O3 is 0.2 to 1.5, more preferably Nb2O5 / Y2O3 is 0.3 to 1.3, and further preferably Nb2O5 / Y2O3 is 0.3 to 1.0; 3) Y2O3 / TiO2 is 0.3 to 3.0, preferably Y2O3 / TiO2 is 0.4 to 2.0, more preferably Y2O3 / TiO2 is 0.5 to 1.5, and further preferably Y2O3 / TiO2 is 0.7 to 1.3; 4) (SiO2+B2O3) / Y2O3 is 0.4 to 3.0, preferably (SiO2+B2O3) / Y2O3 is 0.5 to 2.5, and more preferably (SiO2+B2O3) / Y2O3 is 0.7 to 1.8; 5) (Nb2O5+WO3+Gd2O3) / TiO2 is 0.1 to 3.0, preferably (Nb2O5+WO3+Gd2O3) / TiO2 is 0.2 to 2.5, more preferably (Nb2O5+WO3+Gd2O3) / TiO2 is 0.3 to 2.0, and further preferably (Nb2O5+WO3+Gd2O3) / TiO2 is 0.4 to 1.5; 6) (RO + ZnO) / Y2O3 is 1.0 or less, preferably (RO + ZnO) / Y2O3 is 0.8 or less, more preferably (RO + ZnO) / Y2O3 is 0.5 or less, and further preferably (RO + ZnO) / Y2O3 is 0.2 or less; 7) (RO + Gd2O3) / Y2O3 is less than 1.0, preferably (RO + Gd2O3) / Y2O3 is less than 0.8, more preferably (RO + Gd2O3) / Y2O3 is less than 0.6, and further preferably (RO + Gd2O3) / Y2O3 is less than 0.3; 8) (WO3+TiO2) / Y2O3 is 0.3 to 3.0, preferably (WO3+TiO2) / Y2O3 is 0.4 to 2.5, more preferably (WO3+TiO2) / Y2O3 is 0.5 to 2.0, and further preferably (WO3+TiO2) / Y2O3 is 0.7 to 1.5, The RO is one or more of MgO, CaO, SrO and BaO.

6. The high-refractive and high-dispersion optical glass according to any one of claims 1 to 4, characterized in that: The components are expressed in weight percentage, wherein: SiO2+B2O3: 8-25%, preferably SiO2+B2O3: 10-20%; and / or La2O3+Y2O3+Gd2O3: 50-75%, more preferably La2O3+Y2O3+Gd2O3: 55-70%; and / or ZrO2: 3-12%, preferably ZrO2: 4-10%; and / or Nb2O5: 3-12%, preferably Nb2O5: 5-10%; and / or Ta2O5: 0-3%, preferably Ta2O5: 0-1%, more preferably no Ta2O5; and / or TiO2: 6-18%, preferably TiO2: 8-15; and / or RO: 0-5%, preferably RO: 0-2%, more preferably no RO; and / or Rn2O: 0-3%, preferably Rn2O: 0-2%, more preferably no Rn2O ; and / or WO3: 0-3%, preferably WO3: 0-2%, more preferably no WO3; and / or ZnO: 0-5%, preferably ZnO: 0-2%, more preferably no ZnO; and / or Al2O3: 0-4%, preferably Al2O3: 0-2%, more preferably no Al2O3; and / or Yb2O3: 0-5%, preferably Yb2O3: 0-2%, more preferably no Yb2O3; and / or GeO2: 0-3%, preferably GeO2: 0-1%, more preferably no GeO2; and / or clarifier: 0-1%, preferably clarifier: 0-0.5%, wherein RO is one or more of MgO, CaO, SrO, and BaO, Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

7. The high-refractive and high-dispersion optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, among which: SiO2: 1-15%, preferably SiO2: 2-10%, more preferably SiO2: 4-9%; and / or B2O3: 2-18%, preferably B2O3: 4-12%, more preferably B2O3: 5-10%; and / or La2O3: 35-65%, preferably La2O3: 40-60%, more preferably La2O3: 42-55%; and / or Y2O3: 5-25%, preferably Y2O3: 6-20%, more preferably Y2O3: 8-18%, further preferably Y2O3: 8-15%; and / or Gd2O3: 0-10%, preferably Gd2O3: 0-6%, more preferably Gd2O3: 0-4%.

8. The high-refractive and high-dispersion optical glass according to any one of claims 1 to 4, characterized in that: The refractive index n of the high-refractive and high-dispersion optical glass is d is 1.97 or more, preferably 1.98 or more, more preferably 1.99 or more; the Abbe number v d It is 25-34, preferably 26-33, more preferably 27-32, further preferably 28-31.

9. The high-refractive and high-dispersion optical glass according to any one of claims 1 to 4, characterized in that: The density ρ of the high-refractive and high-dispersion optical glass is 5.20 g / cm 3 Below, preferably 5.10 g / cm 3 Below, more preferably 5.00 g / cm 3 Below; and / or thermal expansion coefficient α -30 / 70℃ 85×10 -7 / K or less, preferably 80×10 -7 / K or less, more preferably 75×10 -7 / K or less; and / or water resistance stability D W 2 or more, preferably 1; and / or acid resistance stability D A 2 or more, preferably 1; and / or weather resistance CR is 2 or more, preferably 1; and / or Knoop hardness H K 670×10 7 Pa or more, preferably 680×10 7 Pa or more, more preferably 690×10 7 Pa or more; and / or Young's modulus E is 11500×10 7 Pa~15500×10 7 Pa, preferably 12000×10 7 Pa~15000×10 7 Pa, more preferably 12500×10 7 Pa~14500×10 7 Pa, more preferably 13000×10 7 Pa~14000×10 7 Pa; and / or the bubble degree is A grade or above, preferably A0 grade or above, more preferably A 00 Grade; and / or wear degree F A It is 80-125, preferably 85-115, and more preferably 90-105.

10. A glass preform, characterized in that: The optical glass is made of the high-refractive and high-dispersion optical glass described in any one of claims 1 to 9.

11. An optical element, characterized in that It is made of the high-refractive and high-dispersion optical glass described in any one of claims 1 to 9, or is made of the glass preform described in claim 10.

12. An optical instrument, characterized in that Contains the high-refractive and high-dispersion optical glass according to any one of claims 1 to 9, and / or contains the optical element according to claim 11.

Citation Information

Patent Citations

  • High-refraction and high- dispersion optical glass and method of manufacture

    CN101289276A

  • Optical glass

    CN102674691A

  • Optical glass with high refraction and high chromatic dispersion, optical element and optical instrument

    CN107445474A

  • Optical glass, glass prefab, optical component and optical instrument

    CN110028239A

  • Optical glass

    CN110128005A