Glass treatment method
By forming a dense non-hydrophilic protective layer on the glass surface, the problem of insufficient hydrophobicity of the glass is solved, the rapid evacuation of water droplets and the drainage of rainwater are achieved, and the hydrophobic performance of the glass is improved, making it suitable for the automotive field.
Patent Information
- Application Number
- CN202310319643.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
Existing glass has insufficient hydrophobicity when using wipers on rainy days, making it difficult to drain rainwater and affecting safety.
By forming a dense non-hydrophilic protective layer on the glass surface, including ultrasonic cleaning, depositing a transition metal silicon bonding layer, a diamond-like carbon layer and a fluoride ion doping layer in a vacuum chamber, fluoride ion diffusion is used to form chemical bonds to improve hydrophobicity performance.
Significantly improves the hydrophobic properties of the glass, allowing water droplets to evacuate quickly, making it suitable for industrial use. It especially improves rainwater drainage efficiency in automotive applications.
Abstract
Description
Technical Field
[0001] The invention relates to the field of glass manufacturing, and in particular to a glass processing method. Background Art
[0002] Glass has different requirements for different application scopes and fields. For example, in the automotive field, the hydrophobicity of glass is required to be high. When the car is driving on rainy days, the outer surface of the glass must be cleaned with wipers. Whether the rainwater can be wiped clean not only has quality requirements for the wipers, but also has high requirements for the glass. If the hydrophobicity of the glass is not good, and the quality of the wipers has deteriorated due to long-term use, the accumulated water will not be removed smoothly, affecting safety.
[0003] Therefore, there is an urgent need to provide a glass processing method to improve the hydrophobicity of glass. Summary of the invention
[0004] The object of the present invention is to provide an improved glass processing method, which forms a dense hydrophilic protective layer on the surface of the glass, thereby improving the hydrophobic performance of the glass and effectively assisting the discharge and evacuation of rainwater.
[0005] To achieve the above object, the present invention provides a method for treating glass, comprising the following steps:
[0006] Ultrasonic cleaning of glass;
[0007] In a vacuum chamber containing silane and argon, depositing a transition metal silicon bonding layer on the surface of the glass;
[0008] Depositing a diamond-like carbon layer on the transition metal silicon bonding layer in a vacuum chamber containing methane and hydrogen; and
[0009] A fluoride ion doping layer is formed on the diamond-like carbon layer.
[0010] Compared with the prior art, the present invention first performs ultrasonic cleaning on the glass, which is beneficial to the subsequent deposition process. Under different vacuum chamber conditions, a transition metal silicon bonding layer is first formed, then a dense diamond-like carbon layer is formed, and finally a fluoride ion doping layer is formed on the diamond-like carbon layer. The fluoride ions diffuse to the surface of the diamond-like carbon layer to form chemical bonds. The diamond-like carbon layer and the fluoride ion doping layer have lower surface energy aggregation, so that the combination is more firm. At the same time, the fluoride ion doping layer has a strong hydrophobic property, which can make the water droplets on the glass surface disperse and discharge outward as quickly as possible.
[0011] Preferably, the ultrasonic cleaning is performed using N-methylpyrrolidone immersion and isopropyl alcohol as a cleaning solution.
[0012] Preferably, the temperature of the cleaning solution is 30-40° C., and the ultrasonic cleaning time is 30-40 minutes.
[0013] Preferably, forming the transition metal silicon bonding layer specifically includes: introducing the silane and the argon gas into the vacuum chamber at a first flow rate, the gas pressure in the vacuum chamber is 5-10Pa, and the bias voltage is -400 to -500V.
[0014] Preferably, the thickness of the transition metal silicon bonding layer is 80-100 nanometers.
[0015] Preferably, forming the diamond-like carbon layer specifically includes: introducing the methane and the hydrogen into the vacuum chamber at a second flow rate greater than the first flow rate, the gas pressure in the vacuum chamber is 20-30 Pa, and the bias voltage is -400 to -500V.
[0016] Preferably, the thickness of the diamond-like carbon layer is 500-600 nanometers.
[0017] Preferably, forming the fluoride ion doped layer specifically includes: introducing CF4 gas into the vacuum chamber, adjusting the power supply to 8-10KW, controlling the gas pressure in the vacuum chamber to 0.5-0.8Pa, and doping fluoride ions on the interface of the diamond-like carbon layer to form the fluoride ion doped layer.
[0018] Preferably, the amount of CF4 gas used is 80-100 sccm.
[0019] Preferably, the thickness of the fluoride ion doping layer is 20-50 nanometers. DETAILED DESCRIPTION
[0020] The glass treatment method of the present invention is further described below in conjunction with the embodiments, but the present invention is not limited thereby. The method of the present invention is intended to provide an improved glass treatment method, forming a dense non-hydrophilic protective layer on the surface of the glass, thereby improving the hydrophobic property of the glass and effectively assisting the drainage and evacuation of rainwater.
[0021] In one embodiment of the glass processing method of the present invention, the following steps are included:
[0022] Ultrasonic cleaning of glass;
[0023] In a vacuum chamber containing silane and argon, depositing a transition metal silicon bonding layer on the surface of the glass;
[0024] Depositing a diamond-like carbon layer on the transition metal silicon bonding layer in a vacuum chamber containing methane and hydrogen; and
[0025] A fluoride ion doping layer is formed on the diamond-like carbon layer.
[0026] The present invention firstly performs ultrasonic cleaning on the glass, which is beneficial to the subsequent deposition process. Under different vacuum chamber conditions, a transition metal silicon bonding layer is first formed, then a dense diamond-like carbon layer is formed, and finally a fluoride ion doping layer is formed on the diamond-like carbon layer. The fluoride ions diffuse to the surface of the diamond-like carbon layer to form chemical bonds. The diamond-like carbon layer and the fluoride ion doping layer have lower surface energy aggregation, so the combination is more firm. At the same time, the fluoride ion doping layer has a strong hydrophobic property, which can make the water droplets on the glass surface disperse and discharge outward as quickly as possible.
[0027] Specifically, in ultrasonic cleaning, ultrasonic cleaning is used, NMP (N-methylpyrrolidone immersion and IPA (isopropyl alcohol) are used as cleaning solutions, preferably, the temperature of the cleaning solution is 30-40° C., and the ultrasonic cleaning time is 30-40 minutes. More preferably, it is then rinsed with deionized water.
[0028] Next, the glass is placed in a vacuum chamber for deposition of each layer. First, a transition metal silicon bonding layer is deposited. Specifically, silane and argon are introduced into the vacuum chamber at a first flow rate, the gas pressure in the vacuum chamber is controlled to be 5-10 Pa, and the bias voltage is -400 to -500 V. Under this condition, a transition metal silicon bonding layer is deposited with a thickness of 80-100 nanometers.
[0029] Next, the residual gas in the vacuum chamber is exhausted, and methane and hydrogen are introduced into the vacuum chamber. The gas flow rate is greater than the first flow rate mentioned above. The gas pressure in the vacuum chamber is controlled to be 20-30 Pa, and the bias voltage is -400 to -500 V. Under this condition, a diamond-like carbon layer is deposited with a thickness of 500-600 nanometers. It should be noted that the thickness of the diamond-like carbon layer should be relatively large to ensure sufficient density.
[0030] After the deposition of the diamond-like carbon layer is completed, the residual gas in the vacuum chamber is exhausted, and about 80-100 sccm of CF4 gas is introduced into the vacuum chamber for the radio frequency source to generate plasma. Fluoride ions diffuse into the diamond-like carbon layer and form chemical bonds with carbon. In particular, in order to protect the diamond-like carbon layer from being removed, no bias is applied during the process of doping fluoride ions. Specifically, after CF4 is introduced, the power supply is adjusted to 8-10KW, the air pressure in the vacuum chamber is controlled to 0.5-0.8Pa, and fluoride ions are doped on the interface of the diamond-like carbon layer to form a fluoride ion doping layer.
[0031] Thus, through the method of the present invention, a transition metal silicon bonding layer, a diamond-like carbon layer and a fluoride ion doping layer are sequentially formed on the surface of the glass. The transition metal silicon bonding layer makes the subsequent layers more bonded, and the diamond-like carbon layer and the fluoride ion doping layer have lower surface energy accumulation, which not only makes the bonding stronger, but also the fluoride ion doping layer has a strong hydrophobic property, which can make the water droplets on the surface of the glass disperse and drain outward as soon as possible, which is conducive to improving the hydrophobic property of the glass, thereby being more suitable for industrial use.
[0032] The above disclosure is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. Therefore, equivalent changes made according to the scope of the patent application of the present invention are still within the scope covered by the present invention.
Claims
1. A method for treating glass, characterized in that: The following steps are involved: Ultrasonic cleaning of glass; In a vacuum chamber containing silane and argon, depositing a transition metal silicon bonding layer on the surface of the glass; Depositing a diamond-like carbon layer on the transition metal silicon bonding layer in a vacuum chamber containing methane and hydrogen; and A fluoride ion doping layer is formed on the diamond-like carbon layer.
2. The glass processing method according to claim 1, characterized in that: The ultrasonic cleaning is performed using N-methylpyrrolidone immersion and isopropyl alcohol as cleaning solutions.
3. The glass processing method according to claim 2, characterized in that: The temperature of the cleaning solution is 30-40° C., and the time of the ultrasonic cleaning is 30-40 minutes.
4. The glass processing method according to claim 1, characterized in that: Forming the transition metal silicon bonding layer specifically includes: introducing the silane and the argon gas into the vacuum chamber at a first flow rate, the gas pressure in the vacuum chamber is 5-10Pa, and the bias voltage is -400 to -500V.
5. The glass processing method according to claim 4, characterized in that: The thickness of the transition metal silicon bonding layer is 80-100 nanometers.
6. The glass processing method according to claim 4, characterized in that: Forming the diamond-like carbon layer specifically includes: introducing the methane and the hydrogen into the vacuum chamber at a second flow rate greater than the first flow rate, the gas pressure in the vacuum chamber is 20-30 Pa, and the bias voltage is -400 to -500V.
7. The glass processing method according to claim 6, characterized in that: The thickness of the diamond-like carbon layer is 500-600 nanometers.
8. The glass processing method according to claim 1, characterized in that: The formation of the fluoride ion doped layer specifically includes: introducing CF4 gas into the vacuum chamber, adjusting the power supply to 8-10KW, controlling the gas pressure in the vacuum chamber to 0.5-0.8Pa, and doping fluoride ions on the interface of the diamond-like carbon layer to form the fluoride ion doped layer.
9. The glass processing method according to claim 8, characterized in that: The amount of CF4 gas used is 80-100 sccm.
10. The glass processing method according to claim 8, characterized in that: The thickness of the fluoride ion doping layer is 20-50 nanometers.