Calcium oxide crucible for vacuum melting of high-temperature alloy and preparation method of calcium oxide crucible
The protective layer is formed through the combination of modified calcium oxide, aluminum oxide and other materials and chemical treatment, which solves the problems of insufficient hydration resistance and thermal shock resistance of existing calcium oxide crucibles, significantly extends the service life of the crucible and improves the performance of high-temperature alloys. performance.
Patent Information
- Application Number
- CN202410950546.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing calcium oxide crucible has insufficient resistance to hydration and thermal shock during vacuum melting of high-temperature alloys, resulting in a short service life of the crucible and possible alloy contamination.
Using a crucible composed of modified calcium oxide, alumina, modified binder and defoaming agent, a dense protective layer is formed through chemical treatment of magnesium dihydrogen phosphate and organic silicon, combined with lignin modified binder to improve hydration resistance and thermal shock resistance, and the integrity of the protective layer is ensured through grouting.
It significantly improves the hydration resistance and thermal shock resistance of the calcium oxide crucible, prolongs its service life, avoids contamination of high-temperature alloys caused by corrosion or decomposition of crucible materials, and improves alloy performance.
Smart Images

Figure BDA0004947100270000101 
Figure BDA0004947100270000111
Abstract
Description
Technical Field
[0001] The invention belongs to the field of refractory materials, and in particular relates to a calcium oxide crucible used for vacuum smelting of high-temperature alloys and a preparation method thereof. Background Art
[0002] High-temperature alloys are widely used in the manufacture of high-end components due to their excellent creep resistance, fatigue resistance, oxidation resistance and thermal corrosion resistance. The sources of impurities mainly include master alloys, vacuum environments, crucibles, mold shells, ceramic cores and pouring systems. Therefore, the smelting and preparation of high-temperature alloys has a significant impact on the properties of the alloys.
[0003] At present, vacuum induction melting is the main method for preparing most high-temperature alloys. Crucibles are used as containers for vacuum induction melting of high-temperature alloys. Their performance and quality are very important for the preparation of high-temperature alloys. The use of crucibles with stable properties can greatly reduce the content of impurity elements in the alloy melting process, thereby ensuring the purity of the high-temperature alloy and making the high-temperature alloy have excellent performance to meet the use requirements.
[0004] There are three main types of crucibles for melting high-temperature alloys: MgO, CaO and Al2O3. Among them, CaO has the functions of removing S, P and reducing O content in molten steel, and has the advantages of high melting point, stable thermodynamic properties, low price and easy availability. However, the easy hydration property of calcium oxide limits its application.
[0005] Patent CN105859305B discloses a method for preparing a dry calcium oxide crucible that is resistant to hydration and thermal shock. The invention uses high-purity quicklime fines and additives composed of calcium fluoride, boric acid and other ingredients to make a mixture, which is finally formed after two pressings and two temperature-controlled sinterings. The obtained calcium oxide crucible has a high density and a small specific area, which enhances the ability to resist hydration; and the use of composite additives also increases the heat buffering capacity of the crucible, but the ability of the calcium oxide crucible to resist hydration still needs to be improved. Patent CN101058502A discloses a composition for making a crucible, comprising magnesium oxide, calcium oxide and calcium fluoride. The crucible made of the composition has the function of a crucible made of pure calcium oxide, and the hydration rate is about 1 / 10 of that of a pure calcium oxide crucible, but its thermal shock resistance may be insufficient. Summary of the invention
[0006] In order to overcome the above-mentioned deficiencies of the prior art, the present invention provides a calcium oxide crucible for vacuum melting of high-temperature alloys and a preparation method thereof. The calcium oxide crucible has excellent hydration resistance and thermal shock resistance, thereby extending the service life of the crucible and effectively avoiding contamination of the high-temperature alloy caused by erosion or decomposition of the crucible material, thereby improving the performance of the high-temperature alloy.
[0007] The technical solution adopted by the present invention is:
[0008] A first aspect of the present invention provides a calcium oxide crucible for vacuum melting of high-temperature alloys, comprising the following raw materials, by weight: 90-100 parts of modified calcium oxide, 1.5-2.5 parts of aluminum oxide, 0.5-3 parts of modified adhesive, 0.1-0.5 parts of defoaming agent and 10-20 parts of anhydrous ethanol.
[0009] In some embodiments, the alumina is of p-type.
[0010] In some embodiments, the steps of modifying the adhesive are as follows:
[0011] A1. Stir alkali lignin, phenol and deionized water at 40-50° C. for 10-20 min to obtain a reactant;
[0012] A2, stirring phenol, NaOH solution and polyethylene glycol at 80-90° C. for 20-30 min, then adding formaldehyde, stirring for 40-60 min, then adding the reactant of step A1, continuing stirring for 3-5 h, cooling to 10-20° C. after the stirring is completed, filtering, and obtaining the modified adhesive.
[0013] In some embodiments, the mass ratio of alkali lignin, phenol and deionized water in step A1 is 1:(2-3):(3-4).
[0014] In some embodiments, the mass concentration of the NaOH solution in step A2 is 2-4%.
[0015] In some embodiments, the mass ratio of phenol, polyethylene glycol in step A2 to the reactant in step A1 is 1:(0.05-0.1):(1.1-1.3).
[0016] In some embodiments, the steps of modifying calcium oxide are as follows:
[0017] S1, prepare magnesium dihydrogen phosphate aqueous solution;
[0018] S2, preparing an organosilicon-anhydrous ethanol solution;
[0019] S3, screening calcium oxide, the particle size ratio of calcium oxide is: 1-4mm accounts for 20-30%, and <1mm accounts for 70-80%;
[0020] S4, stirring the calcium oxide in step S3 and the organosilicon-anhydrous ethanol solution in step S2 for 1-3 minutes, then subjecting them to ultrasonic treatment, subjecting them to ultrasonic treatment for 3-5 minutes, stirring them at 25-30° C. for 20-40 minutes, slowly pouring the magnesium dihydrogen phosphate aqueous solution in step S1 after the stirring, continuing to stir for 1-2 hours, filtering and drying after the stirring, so as to obtain the modified calcium oxide.
[0021] In some embodiments, the mass concentration of the magnesium dihydrogen phosphate aqueous solution in step S1 is 10-20%; the mass concentration of the organosilicon-anhydrous ethanol solution in step S2 is 1.5-2.5%.
[0022] A second aspect of the present invention provides a method for preparing a calcium oxide crucible for vacuum melting of high-temperature alloys, comprising the following steps:
[0023] (1) Material preparation: first, the modified adhesive and anhydrous ethanol are stirred at a speed of 300-400 rpm for 20-40 min, then modified calcium oxide, defoaming agent and aluminum oxide are added, and the mixture is stirred at a speed of 50-80 rpm for 10-20 min to obtain sand material;
[0024] (2) Casting: The sand material of step (1) is poured into a crucible model made of gypsum, and after low-temperature drying at 50-100° C., the sand material is demoulded and taken out to obtain a crucible blank;
[0025] (3) Firing: The crucible blank of step (2) is vacuum dried and then placed in a kiln for firing to obtain the calcium oxide crucible for vacuum smelting of high-temperature alloys.
[0026] In some embodiments, the firing process in step (3) is: heating to 100-120°C at 20-30°C / h and keeping warm for 20-24h; then heating to 580-620°C at 20-30°C / h and keeping warm for 7-9h; then heating to 1150-1250°C at 35-45°C / h and keeping warm for 2-4h; finally heating to 1500-1700°C at 55-65°C / h and keeping warm for 2-4h.
[0027] In order to ensure the stability of calcium oxide during the crucible forming process, the present invention first performs an anti-hydration treatment on it, and uses a magnesium dihydrogen phosphate solution to allow the dihydrogen phosphate groups near the hydroxyl active sites on the surface of the calcium oxide to form a single molecule of dihydrogen phosphate through chemical bonds, and the remaining hydroxyl groups will be in the H + The reaction generates dihydrogen phosphate with the participation of , and at the same time, the dihydrogen phosphate molecules are tightly combined through dehydration condensation, thereby forming a dense shell-like protective layer on the surface of calcium oxide to achieve anti-hydration effect. In order to achieve an ideal protective layer effect, the present invention first grafts organic silicon on the surface of calcium oxide, and uses Si-OH bonds to replace the original hydroxyl groups on the surface of calcium oxide to react with magnesium dihydrogen phosphate to form a complete protective layer, thereby solving the problem that water in the original magnesium dihydrogen phosphate solution inhibits the formation of the protective layer.
[0028] The magnesium dihydrogen phosphate selected in the present invention has a modification effect on the one hand; on the other hand, the doped magnesium element can also improve the sintering temperature of calcium oxide, promote the growth of calcium oxide grains and make the product dense, reduce the channels for water to enter, and improve the anti-hydration ability.
[0029] Since the present invention first forms a protective layer on the surface of calcium oxide, in order to ensure that the protective layer can play its expected effect, in the selection of the crucible forming method, the pressure forming method can easily cause the protective layer to be destroyed, resulting in new unprotected cross-sections and thus hydration. Therefore, the present invention adopts the grouting forming method.
[0030] Binder is an important component of grouting material, which provides early working performance and mechanical strength for the slurry, and can also affect the performance of refractory castables at high temperatures. Since the slurry of the present invention is a calcium oxide system, and particles of 1-4 mm are prone to cause the particles to float and segregate in this molding method, and separate from the slurry, the present invention uses phenolic resin as a binder to improve the segregation of small particles.
[0031] In some embodiments, the defoaming agent is a silicone defoaming agent.
[0032] Since the crucible needs to withstand extreme working conditions during the high-temperature alloy smelting process, and will cool rapidly during the alloy casting process, it is greatly affected by temperature shock. Under the condition of rapid changes in ambient temperature, the strength of the crucible will drop significantly, resulting in surface peeling or even fracture, so the crucible is required to have excellent thermal shock resistance. The present invention solves the problem of increased pores and poor thermal shock resistance caused by the appearance of a large number of bubbles due to the poor fluidity of the liquid phenolic resin by adding a defoaming agent.
[0033] However, the binder and defoamer will undergo carbonization reaction at medium and high temperature stages to form a part of amorphous carbon, which is easily oxidized at high temperature to form a large amount of carbon-containing gas, which will increase the porosity of the crucible and ultimately lead to poor thermal shock resistance of the crucible. The present invention modifies the adhesive by using lignin to replace a part of phenol, ensuring that the lignin is partially soluble in ethanol while retaining some granular substances, thereby promoting the generation of a large amount of new carbon when the raw material is carbonized. The new carbon has primary bonds and has adsorption force on inorganic elements, and can combine carbon with inorganic phosphorus elements. On the one hand, the protective layer of the modified calcium oxide can provide a skeleton for the new carbon when the raw material is carbonized, allowing carbon to be deposited on the skeleton to form an organic grid structure. The structure can absorb or release stress at the crack tip through bridging and crack deflection mechanisms, thereby improving the fracture toughness and thermal shock resistance of the crucible. On the other hand, the protective layer of the modified calcium oxide catalyzes the in-situ formation of a carbon nanostructure inside the crucible during the heat treatment of the raw material. The in-situ formed carbon nanostructure is not only stable crystalline carbon, but also helps to react with Si of the silane layer to form β-SiC whiskers, thereby further improving the strength of the crucible. In addition, the present invention optimizes the adhesion of the crucible material making process and promotes the solidification and demoulding of the crucible by adding a small amount of ρ-type alumina to react with a certain amount of water contained in the modified adhesive.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] 1. The present invention provides a calcium oxide crucible for vacuum melting of high-temperature alloys. Its excellent hydration resistance and thermal shock resistance extend the service life of the crucible, and can also effectively avoid the contamination of the high-temperature alloy caused by the falling of the crucible material, thereby improving the performance of the high-temperature alloy.
[0036] 2. The present invention grafts organic silicon onto the surface of calcium oxide and utilizes Si-OH bonds to replace the original hydroxyl groups on the surface of calcium oxide to react with magnesium dihydrogen phosphate to form a complete protective layer, thereby solving the problem that water in the magnesium dihydrogen phosphate solution easily reacts with calcium oxide.
[0037] 3. The protective layer formed by modifying calcium oxide in the present invention can not only prevent its hydration during the crucible forming process, but also form a carbon nanostructure in situ inside the crucible with the modified adhesive during the sintering process, thereby improving the strength of the crucible. DETAILED DESCRIPTION
[0038] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0039] In order to facilitate those skilled in the art to implement the present invention, some raw materials and manufacturers of the embodiments and comparative examples are described as follows:
[0040] Alkali lignin was purchased from Tianjin Shengfujiang Chemical Sales Co., Ltd.;
[0041] Polyethylene glycol was purchased from Jiangsu Dena Chemical Co., Ltd. with the specification of PEG-300;
[0042] The defoamer was purchased from Jiangsu Scott Technology Co., Ltd., model number XP-30A.
[0043] Preparation Example 1
[0044] The preparation steps of modified calcium oxide-A are as follows:
[0045] S1, preparing a 12wt% aqueous solution of magnesium dihydrogen phosphate;
[0046] S2, preparing a hexadecyltrimethoxysilane-anhydrous ethanol solution with a concentration of 1.5wt%;
[0047] S3. Screen calcium oxide, the particle size ratio of calcium oxide is: 1-4 mm accounts for 25%, and <1 mm accounts for 75%;
[0048] S4, stirring 1500g of the calcium oxide in step S3 and 1950mL of the hexadecyltrimethoxysilane-anhydrous ethanol solution in step S2 for 3min, then subjecting to ultrasonic treatment, stirring at 30°C for 30min after ultrasonic treatment for 4min, slowly pouring in 300mL of the magnesium dihydrogen phosphate aqueous solution in step S1 after the stirring, continuing stirring for 1.5h, filtering while washing with anhydrous ethanol after the stirring, and drying at 50°C for 12h to obtain the modified calcium oxide-A.
[0049] Preparation Example 2
[0050] The preparation steps of modified calcium oxide-B are as follows:
[0051] S1, preparing a 12wt% aqueous solution of magnesium dihydrogen phosphate;
[0052] S2. Screen calcium oxide, the particle size ratio of calcium oxide is: 1-4 mm accounts for 25%, and <1 mm accounts for 75%;
[0053] S3, stirring 100g of the calcium oxide from step S2 and 270mL of the magnesium dihydrogen phosphate aqueous solution from step S1 for 2min, then subjecting to ultrasonic treatment, subjecting to ultrasonic treatment for 4min, stirring at 25°C for 1.5h, filtering with suction and washing with anhydrous ethanol after the stirring, and vacuum drying after the filtering, to obtain the modified calcium oxide-B.
[0054] Preparation Example 3
[0055] The preparation steps of modified calcium oxide-C are as follows:
[0056] S1, preparing a hexadecyltrimethoxysilane-anhydrous ethanol solution with a concentration of 1.5wt%;
[0057] S2. Screen calcium oxide, the particle size ratio of calcium oxide is: 1-4 mm accounts for 25%, and <1 mm accounts for 75%;
[0058] S3. Add 100 g of the calcium oxide obtained in step S2 to 1400 g of the hexadecyltrimethoxysilane-anhydrous ethanol solution obtained in step S1, and stir at 40° C. for 1.5 h. After stirring, filter and vacuum dry to obtain the modified calcium oxide-C.
[0059] Preparation Example 4
[0060] The preparation steps of modified adhesive-A are as follows:
[0061] A1. Stir 20 g of alkali lignin, 50 g of phenol and 60 g of deionized water at 40-50° C. for 10-20 min to obtain a reactant;
[0062] A2. Stir 100 g of phenol, 200 g of 3% NaOH solution and 75 g of polyethylene glycol at 85° C. for 30 min, then add 140 g of formaldehyde, stir for 60 min, then add 120 g of the reactant of step A1, and continue stirring for 4 h to obtain the modified adhesive-A.
[0063] Preparation Example 5
[0064] The steps for preparing the adhesive are as follows:
[0065] 118 g of phenol, 200 g of a 3% NaOH solution and 75 g of polyethylene glycol were stirred at 85° C. for 30 min, and then 140 g of formaldehyde was added and stirred for 4 h to obtain the adhesive.
[0066] Preparation Example 6
[0067] The preparation steps of modified adhesive-B are as follows:
[0068] The difference between this preparation example and preparation example 4 is that 12 g of alkali lignin was used in step A1.
[0069] Preparation Example 7
[0070] The preparation steps of modified adhesive-C are as follows:
[0071] The difference between this preparation example and preparation example 4 is that 28 g of alkali lignin was used in step A1.
[0072] Preparation Example 8
[0073] The preparation steps of modified adhesive-D are as follows:
[0074] The difference between this preparation example and preparation example 4 is that 70 g of phenol was used in step A2.
[0075] Preparation Example 9
[0076] The preparation steps of modified adhesive-E are as follows:
[0077] The difference between this preparation example and preparation example 4 is that 135 g of phenol was used in step A2.
[0078] Preparation Example 10
[0079] The preparation steps of modified adhesive-F are as follows:
[0080] The difference between this preparation example and preparation example 4 is that the mass concentration of the NaOH solution in step A2 is 1%.
[0081] Preparation Example 11
[0082] The preparation steps of modified adhesive-G are as follows:
[0083] The difference between this preparation example and preparation example 4 is that the mass concentration of the NaOH solution in step A2 is 5%.
[0084] Example 1
[0085] A calcium oxide crucible for vacuum melting of high-temperature alloys comprises the following raw materials, measured by weight: 95 parts of modified calcium oxide-A, 2 parts of ρ-alumina, 2 parts of modified adhesive-A, 0.3 parts of XP-30A and 15 parts of anhydrous ethanol.
[0086] The preparation method of the calcium oxide crucible in this embodiment comprises the following steps:
[0087] (1) Material preparation: first, the modified binder-A and anhydrous ethanol were stirred at a speed of 350 rpm for 30 min, and then the modified calcium oxide-A, XP-30A and ρ-alumina were added, and the stirring was continued at a speed of 60 rpm for 15 min to obtain the sand material;
[0088] (2) Casting: The sand material of step (1) is poured into a crucible model made of gypsum, and after low-temperature drying at 80° C. for 24 h, the sand material is demoulded and taken out to obtain a crucible blank;
[0089] (3) Firing: The crucible blank of step (2) is vacuum dried at a temperature of 60°C for 4 hours, and then placed in a kiln for firing, heating to 110°C at a rate of 25°C / h and keeping warm for 24 hours; then heating to 300°C at a rate of 25°C / h and keeping warm for 8 hours; then heating to 1200°C at a rate of 40°C / h and keeping warm for 3 hours; finally heating to 1600°C at a rate of 60°C / h and keeping warm for 3 hours, thereby obtaining the calcium oxide crucible for vacuum smelting of high-temperature alloys.
[0090] Example 2
[0091] A calcium oxide crucible for vacuum melting of high-temperature alloys comprises the following raw materials, measured by weight: 90 parts of modified calcium oxide-A, 1.5 parts of ρ-alumina, 1 part of modified adhesive-A, 0.1 parts of XP-30A and 12 parts of anhydrous ethanol.
[0092] The preparation method of the calcium oxide crucible in this embodiment comprises the following steps:
[0093] (1) Material preparation: firstly, the modified binder-A and anhydrous ethanol were stirred at a speed of 300 rpm for 40 min, and then the modified calcium oxide-A, XP-30A and ρ-alumina were added, and the stirring was continued at a speed of 50 rpm for 20 min to obtain the sand material;
[0094] (2) Casting: The sand material of step (1) is poured into a crucible model made of gypsum, and after low-temperature drying at 60° C. for 30 h, the sand material is demoulded and taken out to obtain a crucible blank;
[0095] (3) Firing: The crucible blank of step (2) is vacuum dried at a temperature of 60°C for 4 hours, and then placed in a kiln for firing, heating to 100°C at a rate of 20°C / h and keeping the temperature for 24 hours; then heating to 580°C at a rate of 20°C / h and keeping the temperature for 9 hours; then heating to 1150°C at a rate of 35°C / h and keeping the temperature for 4 hours; finally heating to 1500°C at a rate of 55°C / h and keeping the temperature for 4 hours, thereby obtaining the calcium oxide crucible for vacuum smelting of high-temperature alloys.
[0096] Example 3
[0097] A calcium oxide crucible for vacuum melting of high-temperature alloys comprises the following raw materials, measured by weight: 100 parts of modified calcium oxide-A, 2.5 parts of ρ-alumina, 3 parts of modified adhesive-A, 0.5 parts of XP-30A and 20 parts of anhydrous ethanol.
[0098] The preparation method of the calcium oxide crucible in this embodiment comprises the following steps:
[0099] (1) Material preparation: firstly, the modified binder-A and anhydrous ethanol were stirred at a speed of 400 rpm for 20 min, and then the modified calcium oxide-A, XP-30A and ρ-alumina were added, and the stirring was continued at a speed of 80 rpm for 10 min to obtain the sand material;
[0100] (2) Casting: The sand material of step (1) is poured into a crucible model made of gypsum, and after low-temperature drying at 90° C. for 20 h, the sand material is demoulded and taken out to obtain a crucible blank;
[0101] (3) Firing: The crucible blank of step (2) is vacuum dried at a temperature of 60°C for 4 hours, and then placed in a kiln for firing, heating to 120°C at a rate of 30°C / h and keeping the temperature for 20 hours; then heating to 620°C at a rate of 30°C / h and keeping the temperature for 7 hours; then heating to 1250°C at a rate of 45°C / h and keeping the temperature for 2 hours; finally heating to 1700°C at a rate of 65°C / h and keeping the temperature for 2 hours, thereby obtaining the calcium oxide crucible for vacuum smelting of high-temperature alloys.
[0102] Example 4
[0103] This embodiment provides a calcium oxide crucible for vacuum melting of high-temperature alloys and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that modified calcium oxide-A is replaced by an equal portion of modified calcium oxide-B.
[0104] Example 5
[0105] This embodiment provides a calcium oxide crucible for vacuum melting of high-temperature alloys and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that modified calcium oxide-A is replaced by an equal portion of modified calcium oxide-C.
[0106] Example 6
[0107] This embodiment provides a calcium oxide crucible for vacuum melting of high-temperature alloys and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified adhesive-A is replaced by an equal portion of the modified adhesive-B.
[0108] Example 7
[0109] This embodiment provides a calcium oxide crucible for vacuum melting of high-temperature alloys and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified adhesive-A is replaced by an equal portion of the modified adhesive-C.
[0110] Example 8
[0111] This embodiment provides a calcium oxide crucible for vacuum melting of high-temperature alloys and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified adhesive-A is replaced by an equal portion of the modified adhesive-D.
[0112] Example 9
[0113] This embodiment provides a calcium oxide crucible for vacuum melting of high-temperature alloys and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified adhesive-A is replaced by an equal portion of the modified adhesive-E.
[0114] Example 10
[0115] This embodiment provides a calcium oxide crucible for vacuum melting of high-temperature alloys and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified adhesive-A is replaced by an equal portion of the modified adhesive-F.
[0116] Embodiment 11
[0117] This embodiment provides a calcium oxide crucible for vacuum melting of high-temperature alloys and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified adhesive-A is replaced by an equal portion of the modified adhesive-G.
[0118] Comparative Example 1
[0119] This comparative example provides a calcium oxide crucible for vacuum melting of high-temperature alloys and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified adhesive-A is replaced by an equal amount of adhesive.
[0120] Performance Test:
[0121] 1. Hydration resistance test
[0122] ① First, the crucible provided in each embodiment is dried at 110° C., and the drying is completed when the mass of the sample no longer changes, and then cooled to room temperature to obtain a sample;
[0123] ② Weigh the dried sample using an analytical balance and record the data, then place it in a constant temperature and humidity chamber to test its anti-hydration performance;
[0124] ③The data of the constant temperature and humidity chamber are set as follows: constant temperature 21°C, constant humidity 98%;
[0125] ④The time is controlled within 30h;
[0126] ⑤ The hydration resistance of the samples is divided into four levels, as follows:
[0127] Level 1 refers to those with no significant changes;
[0128] The surface of the sample is powdered, which is level 2;
[0129] The specimen edge disintegrated, which was grade 3;
[0130] The specimen with severe edge collapse is rated as Level 4.
[0131] 2. Thermal shock resistance test
[0132] This test is carried out according to the air rapid cooling method in the national standard GB / T 30873-2014. When the sample bursts during the rapid heating and cooling process and the bending stress test can no longer be performed, the number of repetitions is recorded, where the bending stress is 0.3MPa.
[0133] The results are shown in Table 1.
[0134] Table 1 Performance test results of different embodiments
[0135]
[0136]
[0137] It can be seen from the data in Table 1 that the calcium oxide crucibles of Examples 1-3 have good hydration resistance and thermal shock resistance, indicating that they have a long service life and have little negative impact on the melting process of high-temperature alloys; it can be seen from Examples 1 and 4-5 that for calcium oxide, it is necessary to use silicone to protect the surface before modifying it with magnesium dihydrogen phosphate, otherwise the calcium oxide is easily hydrated during the modification process and then fails, ultimately resulting in the formation of a crucible that cannot play a role in melting alloys.
[0138] It can be seen from Example 1 and Comparative Example 1 that improving the fluidity of the adhesive can enhance the thermal shock resistance of the crucible. The possible reason is that the adhesive with poor fluidity is prone to a large number of bubbles during the crucible grouting process, and is prone to segregation during the crucible forming process, resulting in an increase in pores during the calcination process, making the density poor, and then causing it to crack or surface peeling during the high-temperature alloy smelting process; it can be seen from Example 1 and Examples 6-7 that when modifying the adhesive, it is necessary to control the ratio of lignin to ensure that the rolling friction is increased without causing additional pores, so as to effectively improve the thermal shock resistance; it can be seen from Example 1 and Examples 8-9 that the change in the ratio of raw materials will affect the bonding ability of the adhesive, and then affect the hydration resistance and thermal shock resistance of the crucible; it can be seen from Example 1 and Examples 10-11 that the concentration change of the NaOH solution will have a certain effect on the thermal shock resistance of the crucible, which may be due to the influence on the synthesis of the phenolic resin.
[0139] The embodiments and comparative examples described above do not impose any form of limitation on the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A calcium oxide crucible for vacuum melting of high temperature alloys, It is characterized in that The invention comprises the following raw materials by weight: 90-100 parts of modified calcium oxide, 1.5-2.5 parts of aluminum oxide, 0.5-3 parts of modified adhesive, 0.1-0.5 parts of defoaming agent and 10-20 parts of anhydrous ethanol.
2. The calcium oxide crucible for vacuum melting of high temperature alloys according to claim 1, It is characterized in that The aluminum oxide is of p-type.
3. The calcium oxide crucible for vacuum melting of high temperature alloys according to claim 1, It is characterized in that The preparation steps of the modified adhesive are as follows: A1. Stir alkali lignin, phenol and deionized water at 40-50° C. for 10-20 min to obtain a reactant; A2, stirring phenol, NaOH solution and polyethylene glycol at 80-90° C. for 20-30 min, then adding formaldehyde, stirring for 40-60 min, then adding the reactant of step A1, continuing stirring for 3-5 h, cooling to 10-20° C. after the stirring is completed, filtering, and obtaining the modified adhesive.
4. The calcium oxide crucible for vacuum melting of high temperature alloys according to claim 3, It is characterized in that In the step A1, the mass ratio of alkali lignin, phenol and deionized water is 1:(2-3):(3-4).
5. The calcium oxide crucible for vacuum melting of high temperature alloys according to claim 3, It is characterized in that The mass concentration of the NaOH solution in step A2 is 2-4%.
6. The calcium oxide crucible for vacuum melting of high temperature alloys according to claim 5, It is characterized in that The mass ratio of phenol, polyethylene glycol in step A2 to the reactant in step A1 is 1:(0.05-0.1):(1.1-1.3).
7. The calcium oxide crucible for vacuum melting of high temperature alloys according to claim 1, It is characterized in that The preparation steps of the modified calcium oxide are as follows: S1, prepare magnesium dihydrogen phosphate aqueous solution; S2, preparing an organosilicon-anhydrous ethanol solution; S3, screening calcium oxide, the particle size ratio of calcium oxide is: 1-4mm accounts for 20-30%, and <1mm accounts for 70-80%; S4, stirring the calcium oxide in step S3 and the organosilicon-anhydrous ethanol solution in step S2 for 1-3 minutes, then subjecting them to ultrasonic treatment, subjecting them to ultrasonic treatment for 3-5 minutes, stirring them at 25-30° C. for 20-40 minutes, slowly pouring the magnesium dihydrogen phosphate aqueous solution in step S1 after the stirring, continuing to stir for 1-2 hours, filtering and drying after the stirring, so as to obtain the modified calcium oxide.
8. The calcium oxide crucible for vacuum melting of high temperature alloys according to claim 7, It is characterized in that The mass concentration of the magnesium dihydrogen phosphate aqueous solution in step S1 is 10-20%; the mass concentration of the organosilicon-anhydrous ethanol solution in step S2 is 1.5-2.5%.
9. A method for preparing a calcium oxide crucible for vacuum melting of high-temperature alloys according to any one of claims 1 to 8, It is characterized in that The steps of the preparation method are as follows: (1) Material preparation: first, the modified adhesive and anhydrous ethanol are stirred at a speed of 300-400 rpm for 20-40 min, then modified calcium oxide, defoaming agent and aluminum oxide are added, and the mixture is stirred at a speed of 50-80 rpm for 10-20 min to obtain sand material; (2) Casting: The sand material of step (1) is poured into a crucible model made of gypsum, and after low-temperature drying at 50-100° C., the sand material is demoulded and taken out to obtain a crucible blank; (3) Firing: The crucible blank of step (2) is vacuum dried and then placed in a kiln for firing to obtain the calcium oxide crucible for vacuum smelting of high-temperature alloys.
10. The method for preparing a calcium oxide crucible for vacuum melting of high temperature alloys according to claim 9, It is characterized in that The firing process in step (3) is as follows: heating to 100-120°C at 20-30°C / h and keeping warm for 20-24h; then heating to 580-620°C at 20-30°C / h and keeping warm for 7-9h; then heating to 1150-1250°C at 35-45°C / h and keeping warm for 2-4h; finally heating to 1500-1700°C at 55-65°C / h and keeping warm for 2-4h.
Citation Information
Patent Citations
Composition for manufacturing crucible and method thereof
CN101058502A
A method for preparing a dry-process calcium oxide crucible that is resistant to hydration and thermal shock.
CN105859305B