Prime powder as well as preparation method and application thereof

By controlling the temperature and humidity environment, the firing powder is directly generated in situ, which solves the problem of safety hazards of copper azotetrazole in the firing powder in the existing technology, and realizes the production and use of lead-free and barium-free green detonating powder. Improved safety and environmental protection.

CN118724664APending Publication Date: 2024-10-01NANJING UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310333661.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing detonators contain a large amount of heavy metal oxides such as lead and barium, which are toxic and pose safety risks. It is difficult to achieve lead-free and barium-free green detonators. Copper azotetrazole is sensitive to impact and friction during preparation and use, causing safety risks. , it is difficult to avoid explosion accidents.

Method used

By controlling the temperature and relative humidity of the reaction environment, solid mixed raw materials are used to directly generate the firing agent in situ, eliminating the mixing and pressing process, reducing the friction and impact sensitivity of copper azotetrazolium, and improving safety.

Benefits of technology

It realizes the safe production and use of triggering chemicals, reduces the safety hazards of copper azotetrazolium in the field of triggering chemicals, avoids pollution to people and the environment, and provides a green and environmentally friendly alternative to explosive chemicals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a primer composition as well as a preparation method and application thereof, the preparation method of the primer composition creatively adopts an in-situ preparation method, a solid mixed raw material is placed in a specific container, and the target primer composition is obtained by directly reacting the solid mixed raw material in the container by controlling the temperature, relative humidity and other conditions of the environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to azotetrazolyl copper or a composition containing the azotetrazolyl copper, and also provides a corresponding preparation method and application. Background Art

[0002] The firing charge is the basic charge of various impact ignition devices. It is a mixed agent that causes deflagration after being stimulated by the initial impulse energy. The firing charge needs to meet the requirements of suitable mechanical sensitivity, good ignition ability, reliable action, safe manufacturing and use. The commonly used detonators for firing charges include lead nitride, tetrazene and lead styphnate. Based on the above commonly used detonators, when used as firing charges, they usually also need to have combustibles and oxidants as essential components. In addition, they may also contain desensitizers, sensitizers and other components. After the firing charge is triggered by the outside world, a hot spot is generated. The detonator decomposes to cause the combustion reaction of the combustible and the oxidant, and the flame formed is used to ignite the pyrotechnics. Therefore, as the first-level charge stimulated by mechanical energy, the firing charge has extremely high mechanical sensitivity and is sensitive to impact and friction. It is often produced by small-batch drum mixing in production, and the intermediate process requires manual participation: such as weighing, taking and placing medicine trays, and shipping medicine trays, which makes the safety risk in the production and transportation process higher and poses greater harm to equipment and workers. In addition, the widely used firing powder contains a large amount of lead, barium and titanium, and the oxides of these heavy metals are toxic. In order to meet the requirements of environmental protection, lead-free and barium-free firing powder has been sought in the past two decades.

[0003] Based on this, azotetrazole energetic compounds have become a research hotspot. Some azotetrazole energetic compounds do not contain oxygen in their molecular structure, but have high energy and high bombardment velocity. Compared with aminotetrazole energetic compounds, azotetrazole energetic compounds are relatively sensitive and more environmentally friendly than the currently widely used detonators, and are expected to become new green detonators. However, with the application of azotetrazole energetic compounds in high explosives and pyrotechnic agents, it was found that due to their high sensitivity, azotetrazole complexes still exist when used as detonators for firing agents, etc., but due to the impact and friction during the mixing and pressing process, explosions or combustion may occur, resulting in accidents. Based on this, the friction sensitivity and impact sensitivity of azotetrazole energetic compounds as detonators have gradually become research hotspots for their improvement.

[0004] In order to solve the above safety issues, it is necessary to seek new ways to achieve a harmonious unity between the energy and stability of the complex. Based on the high-energy nitrogen-containing azotetrazole compounds, domestic and foreign researchers have appropriately reduced the nitrogen content of the azotetrazole complex by introducing auxiliary ligands to achieve the unity of high energy and insensitivity. Through systematic research, the structure and performance of the complex have been optimized. Tao Guo-hong et al. (non-patent literature 1) have made a new approach to achieve a harmonious unity between the energy and stability of the complex by introducing auxiliary ligands based on the high-energy nitrogen-containing azotetrazole compounds. 2-The auxiliary ligands o-phenanthroline (o-phen) and 2,2'-bipyridyl (2,2'-bipyridyl) were introduced to enhance the stability of the complex by moderately reducing the nitrogen content; Zhang Tonglai et al. (Non-patent Literature 2) studied the Mn 2+ 、Cd 2+ 、Ni 2+ The coordination compound is a coordination compound with DAT, C1OT, N, etc. as the central ion and DAT, C1OT, N, etc. as the ligands. The energy and insensitivity of energetic complexes are unified by introducing auxiliary ligands to synthesize mixed complexes. In addition, Xie Xingbing, Zhu Shunguan, et al. (non-patent document three) disclosed a relatively complex preparation method, in which the target compound [Cu(NH3)4]ATZ-2H20 is synthesized in two steps. First, 5-aminotetrazole is used as the raw material, and it is oxidized to generate 5,5-azotetrazole sodium (NaATZ) by Thiele alkaline oxidation method; the second step is to use NaATZ aqueous solution as the base liquid, add ammonia water and soluble copper salt to carry out coordination reaction to generate the target product crystal. On the basis of the high-energy nitrogen compound of azotetrazole, the nitrogen content of the azotetrazole complex is appropriately reduced by introducing auxiliary ligands to achieve the unity of high energy and insensitivity. Through systematic research, the structure and performance of the complex are optimized, and it is hoped that it will have practical application value in the field of pyrotechnics.

[0005] However, the lone pair of electrons on the ring-forming N atom in the 5,5'-azotetrazolyl ion structure provides the necessary conditions for its coordination with metal ions, making it a very excellent high-nitrogen energetic ligand. The research on azotetrazolyl energetic compounds has been carried out for many years, but most of them involve the synthesis of new compounds, process optimization, and performance modification. Regarding the research on azotetrazolyl metal salts, current reports generally involve alkaline earth metals, alkali metals, and some trivalent metal complexes, mainly manganese, cobalt, nickel, zinc, lead and other metal salts of azotetrazolyl.

[0006] In 2009, Yan Zhijun et al. (Non-patent Document 4) synthesized the dihydrate of copper azotetrazole. Compared with other metal salts of azotetrazole, this salt has better explosive properties, but it is extremely sensitive to impact, friction, and static electricity stimulation, especially after the copper azotetrazole loses its crystal water, which makes it a huge safety hazard in the process of preparation, storage and use, and still cannot avoid the safety problems in the mixing and pressing process of the detonator.

[0007] Therefore, if the safety issues of explosives such as copper azotetrazole in the preparation and use process can be solved, and their excellent explosive performance and green and environmentally friendly characteristics can be utilized, they will replace traditional pyrotechnic agents containing toxic and harmful elements such as lead, cadmium, and chlorine, and provide research ideas for the miniaturization of weapon systems.

[0008] Non-patent literature 1: TAO Guo-hong, Twamley B, Shreeve J M. Energetic nitrogen rich Cu(II) and Cd(II)5,5'-azobis(tetrazolate) complexes[J]. Inorg.Chem.2009,48,20,9918–9923.

[0009] Non-patent literature 2: Huang Huisheng, Zhang Tonglai, Zhang Jianguo, et al. Theoretical study on the structure and properties of energetic complexes of cobalt, nickel and copper with nitric acid carbohydrazide [J]. Acta Chimica Sinica, 2010, 68(4): 289-293.

[0010] Non-patent literature 3: Xie Xingbing, Zhu Shunguan, Chen Pengyuan, Tang Xiangbin, Tao Peipei, Synthesis and properties of tetraamminecopper(II) dihydrate azotetrazolyl[J]. Journal of Explosives and Propellants, 2014, 37(6): 31-34.

[0011] Non-patent literature 4: Yan Zhijun, Jiao Baojuan, Gao Shengli. Synthesis of a novel energetic complex CuATZ·2H2O[J]. Applied Chemistry, 2009, 26(4): 483-485. Summary of the invention

[0012] 1. Problem to be solved

[0013] One of the purposes of the present invention is to provide a novel method for preparing a firing charge, wherein the method creatively adopts a solid mixed raw material, and directly generates the firing charge in situ by controlling the temperature, relative humidity and other conditions of the reaction environment, thereby eliminating the mixing and pressing process required for copper azotetrazole as a detonating agent to be used as a firing charge, thereby improving safety;

[0014] Based on one of the purposes of the present invention, the present invention also provides a firing charge, and a primer or detonator containing the firing charge.

[0015] 2. Technical solution

[0016] In order to solve the above problems, the technical solution adopted by the present invention is as follows:

[0017] According to one of the purposes of the present invention, the present invention provides a method for preparing a firing agent, wherein the raw materials of the firing agent include:

[0018] Sodium azotetrazolyl;

[0019] a source of copper; and,

[0020] Adhesives;

[0021] The addition amount of the sodium azotetrazolyl and copper source is calculated according to the molar ratio of the azotetrazolyl anion to the divalent copper ion of (1-2): (2-1);

[0022] Calculated based on the total amount of sodium azotetrazolyl and copper source added, the amount of the binder added accounts for 0.5 to 8 wt% of the total amount added;

[0023] The preparation of the firing medicine comprises the following steps:

[0024] 1) mixing the component raw materials and filling the mixed component raw materials into a container;

[0025] 2) placing the container in an environment with a temperature of 20 to 80 degrees Celsius and a relative humidity of not less than 40% for 0.5 to 72 hours to form the firing charge.

[0026] According to the method for preparing a firing agent of any embodiment of the first aspect of the first object of the present invention, in step 1), the molar ratio of the azotetrazolyl anion to the divalent copper ion is 1:(2-1); or the molar ratio of the azotetrazolyl anion to the divalent copper ion is 2:(2-1); or the molar ratio of the azotetrazolyl anion to the divalent copper ion is (1-2):1; or the molar ratio of the azotetrazolyl anion to the divalent copper ion is (1-2):2.

[0027] According to the method for preparing a firing agent of any embodiment of the first aspect of the first object of the present invention, in step 1), based on the total amount of sodium azotetrazolyl and copper source added, the amount of the adhesive added accounts for 3-6wt% of the total amount added, and most preferably 5wt%.

[0028] According to the method for preparing the firing agent of any embodiment of the first aspect of the first object of the present invention, the sodium azotetrazolyl can pass through a sieve of not less than 40 meshes.

[0029] According to the method for preparing the firing agent of any embodiment of the first aspect of the first object of the present invention, the mesh number of the sieve through which the sodium azotetrazolyl can pass can be any value taken from any of the following numerical ranges: 40-500 mesh, 40-300 mesh, 40-200 mesh, 40-100 mesh, 40-80 mesh, 80-500 mesh, 80-400 mesh, 80-300 mesh, 80-200 mesh, 80-100 mesh, 100-500 mesh, 100-400 mesh, 100-300 mesh, 100-200 mesh.

[0030] According to the method for preparing the percussion charge of any embodiment of the first aspect of the first object of the present invention, the copper source can pass through a sieve of not less than 40 meshes.

[0031] According to the method for preparing a percussion charge of any embodiment of the first aspect of the first object of the present invention, the mesh number of the sieve through which the copper source can pass can be any value taken from any one of the following numerical ranges: 40-500 mesh, 40-300 mesh, 40-200 mesh, 40-100 mesh, 40-80 mesh, 80-500 mesh, 80-400 mesh, 80-300 mesh, 80-200 mesh, 80-100 mesh, 100-500 mesh, 100-400 mesh, 100-300 mesh, 100-200 mesh.

[0032] According to the method for preparing the firing agent of any embodiment of the first aspect of the first object of the present invention, the particle size of the sodium azotetrazolyl oxide is no more than 400 microns.

[0033] According to the method for preparing the firing agent of any embodiment of the first aspect of the first object of the present invention, the particle size of the sodium azotetrazole can be any value taken from any group of numerical ranges: 400-10 microns, 400-50 microns, 400-100 microns, 400-150 microns, 400-200 microns, 400-250 microns, 400-300 microns, 400-350 microns, 300-10 microns, 300-50 microns, 300-100 microns, 300-150 microns, 300-200 microns, 300-250 microns, 200-10 microns, 200-50 microns, 200-100 microns, 200-150 microns.

[0034] According to the method for preparing the firing charge of any embodiment of the first aspect of the first object of the present invention, the particle size of the copper source does not exceed 400 microns.

[0035] According to the method for preparing the percussion charge of any embodiment of the first aspect of the first object of the present invention, the particle size of the copper source can be any value taken from any one of the following numerical ranges: 400-10 microns, 400-50 microns, 400-100 microns, 400-150 microns, 400-200 microns, 400-250 microns, 400-300 microns, 400-350 microns, 300-10 microns, 300-50 microns, 300-100 microns, 300-150 microns, 300-200 microns, 300-250 microns, 200-10 microns, 200-50 microns, 200-100 microns, 200-150 microns.

[0036] According to the method for preparing the firing charge of any embodiment of the first aspect of the first object of the present invention, the raw materials of the firing charge further include: a reducing agent and / or an oxidizing agent;

[0037] The amount of the reducing agent added is 6 to 30 wt % of the total amount of the sodium azotetrazolyl and the copper source added;

[0038] The added amount of the oxidant accounts for 65-85 wt % of the total amount of the sodium azotetrazolyl and the copper source.

[0039] According to the method for preparing the firing charge of any embodiment of the first aspect of the first object of the present invention, the reducing agent comprises any one or both of zirconium powder and aluminum powder;

[0040] According to the method for preparing a firing charge of any embodiment of the first aspect of the first object of the present invention, the component raw materials of the firing charge include zirconium powder, and the added amount of the zirconium powder accounts for 0-20wt% of the total added amount; the preferred added amount is 0-15wt%, more preferably 6-10wt%, and even more preferably 8-10wt%.

[0041] According to the method for preparing a firing charge of any embodiment of the first aspect of the first object of the present invention, the component raw materials of the firing charge include aluminum powder, and the added amount of the aluminum powder accounts for 0 to 30 wt% of the total added amount; the preferred added amount is 8 to 30 wt%, more preferably 13 to 30 wt%, and even more preferably 20 to 30 wt%.

[0042] According to the method for preparing the firing agent of any embodiment of the first aspect of the first object of the present invention, the raw materials of the firing agent further include:

[0043] The oxidant includes any one, two or three of copper oxide, iron oxide and bismuth oxide.

[0044] According to the method for preparing the firing charge of any embodiment of the first aspect of the first object of the present invention, the raw material of the firing charge comprises copper oxide, and the addition amount of the copper oxide accounts for 0 to 80 wt% of the total addition amount; preferably, the addition amount is 60 to 80 wt%, more preferably 70 to 80 wt%, and even more preferably 74 to 80 wt%;

[0045] According to the method for preparing the firing charge of any embodiment of the first aspect of the first object of the present invention, the raw material of the firing charge comprises iron oxide, and the amount of the iron oxide added accounts for 0 to 80 wt% of the total amount added; preferably, the amount added is 70 to 80 wt%, more preferably 70 to 75 wt%, and even more preferably 74 wt%;

[0046] According to the method for preparing a firing charge of any embodiment of the first aspect of the first object of the present invention, the component raw materials of the firing charge include bismuth oxide, and the added amount of the bismuth oxide accounts for 0-80wt% of the total added amount; the preferred added amount is 70-80wt%, and more preferably 75wt%.

[0047] According to the method for preparing the percussion charge of any embodiment of the first aspect of the first object of the present invention, the oxidant and the reducing agent can pass through a sieve of not less than 60 meshes.

[0048] According to the method for preparing the percussion charge of any embodiment of the first aspect of the first object of the present invention, the mesh number of the sieve through which the oxidant and the reductant can pass can be any value taken from any group of numerical ranges below: 60-500 mesh, 60-300 mesh, 60-200 mesh, 60-100 mesh, 60-80 mesh, 80-500 mesh, 80-400 mesh, 80-300 mesh, 80-200 mesh, 80-100 mesh, 100-500 mesh, 100-400 mesh, 100-300 mesh, 100-200 mesh.

[0049] According to the method for preparing the firing agent of any embodiment of the first aspect of the first object of the present invention, the particle size of the oxidizing agent and the reducing agent does not exceed 300 microns.

[0050] According to the method for preparing the firing agent of any embodiment of the first aspect of the first object of the present invention, the particle size of the oxidant and the reductant can be any value within any of the following numerical ranges: 300-10 microns, 300-50 microns, 300-100 microns, 300-150 microns, 300-200 microns, 300-250 microns, 200-10 microns, 200-50 microns, 200-100 microns, 200-150 microns.

[0051] According to the method for preparing the firing agent of any embodiment of the first aspect of the first object of the present invention, in step 2), the container is placed at a temperature of 20 to 60 degrees Celsius; preferably, the container is placed at a temperature of 20 to 40 degrees Celsius; and / or,

[0052] In step 2), the container is placed in an environment with a relative humidity of not less than 60%; preferably, the container is placed in an environment with a relative humidity of not less than 70%.

[0053] According to the method for preparing the firing agent of any embodiment of the first aspect of the first object of the present invention, in step 1), the mixed component raw materials are compacted;

[0054] and / or

[0055] The mixed component raw materials are processed by a vibration compaction method.

[0056] According to the method for preparing the firing agent of any embodiment of the first aspect of the first object of the present invention,

[0057] The mixed component raw materials are compacted at a pressure of not less than 50 MPa;

[0058] Preferably, the mixed component raw materials are compacted using a pressure of 50 to 150 MPa.

[0059] According to the method for preparing the percussion charge of any embodiment of the first aspect of the first object of the present invention, the pressure can be any value within any of the following numerical ranges: 50-200MPa, 50-175MPa, 50-150MPa, 50-125MPa, 50-100MPa, 50-75MPa, 80-200MPa, 80-175MPa, 80-150MPa, 80-125MPa, 80-100MPa.

[0060] According to the method for preparing the firing agent of any embodiment of the first aspect of the first object of the present invention, the copper source includes one or more of copper sulfate, copper nitrate, copper chloride and hydrates thereof.

[0061] According to the method for preparing the firing agent of any embodiment of the first aspect of the first object of the present invention, the adhesive comprises one or more of 901 glue, hydroxypropyl methylcellulose, and polyvinyl alcohol.

[0062] According to the method for preparing the firing agent of any embodiment of the first aspect of the first object of the present invention, in step 2), the container is placed in an environment with a temperature of 20 to 80 degrees Celsius and a relative humidity of not less than 40% to form a product containing azotetrazole copper;

[0063] Wherein, the processing time is 0.5 to 72 hours;

[0064] According to the method for preparing the percussion medicine of any embodiment of the first aspect of the first object of the present invention, the temperature at which the container is placed can be any value taken from any of the following numerical ranges: 20-80 degrees Celsius, 20-75 degrees Celsius, 20-70 degrees Celsius, 20-65 degrees Celsius, 20-60 degrees Celsius, 20-55 degrees Celsius, 20-50 degrees Celsius, 20-45 degrees Celsius, 20-40 degrees Celsius, 20-35 degrees Celsius, 25-30 degrees Celsius, 25-35 degrees Celsius, 25-40 degrees Celsius, 25-45 degrees Celsius, 25-50 degrees Celsius, 25-55 degrees Celsius, 25-60 degrees Celsius, 25-65 degrees Celsius, 25-70 degrees Celsius; the preferred range is 20-45 degrees Celsius, 20-40 degrees Celsius, 20-35 degrees Celsius, 25-30 degrees Celsius, 25-35 degrees Celsius, 25-40 degrees Celsius, 25-45 degrees Celsius.

[0065] According to the method for preparing the percussion charge of any embodiment of the first aspect of the first object of the present invention, the relative humidity can be any value taken from any one of the following numerical ranges: 40-100, 40-95, 40-90, 40-85, 40-80, 40-75, 40-70, 40-65, 40-60, 40-55, 40-50, 50-100, 50-95, 50-90, 50-85, 50-80, 50-75, 50-70, 50-65, 50-60, 50-55, 60-100, 60-95, 60-85. 0-90, 60-85, 60-80, 60-75, 60-70, 60-65, 70-100, 70-95, 70-90, 70-85, 70-80, 70-75, 80-100, 80-95, 80-90, 80-85; a more preferred range is 70-100, 70-95, 70-90, 70-85, 70-80, 70-75, 80-100, 80-95, 80-90, 80-85; the most preferred range is 80-100, 80-95, 80-90, 80-85.

[0066] According to the method for preparing the percussion powder of any embodiment of the first aspect of the first object of the present invention, the processing time can be any value taken from any one of the following numerical ranges: 0.5-72h, 0.5-36h, 0.5-18h, 0.5-9h, 1-72h, 1-36h, 1-18h, 1-9h, 2-72h, 2-36h, 2-18h, 2-9h, 3-72h, 3-36h, 3-18h, 3-9h, 4-72h, 4-36h, 4-18h, 4-9h, 6-72h, 6-36h, 6-18h, 6-9h, 8-72h, 8-36h, 8-18h, 8-9h.

[0067] Based on the first object of the present invention and any of the above technical solutions, the second object of the present invention is to provide a firing charge, characterized in that the firing charge comprises:

[0068] Copper azotetrazolyl, and

[0069] Sodium salt;

[0070] The content of the sodium salt is 18-60 wt %.

[0071] According to the firing charge of any embodiment of the first aspect of the second object of the present invention, the firing charge comprises sodium azotetrazolyl.

[0072] According to the percussion charge of any embodiment of the first aspect of the second object of the present invention, the percussion charge includes a reducing agent, and the reducing agent is zirconium powder.

[0073] Based on the first object of the present invention and its technical solution, or based on the second object of the present invention and its technical solution, the third object of the present invention is to provide a percussion cap or detonator containing the firing powder.

[0074] Based on the first object of the present invention and its technical solution, or based on the second object of the present invention and its technical solution, or based on the third object of the present invention and its technical solution, the fourth object of the present invention is to provide an in-situ application method of a firing agent.

[0075] Beneficial Effects

[0076] (1) The method for preparing the firing charge provided by the present invention can realize the direct in-situ generation of the firing charge in containers such as percussion cap shells, primer shells, detonator shells, etc.

[0077] (2) The preparation method of the firing agent provided by the present invention eliminates the mixing and pressing process, and can realize the safe application of copper azotetrazolyl as a detonating agent in the firing agent field, which greatly reduces the potential safety hazards in the preparation and application of copper azotetrazolyl as a detonating agent in the firing agent field.

[0078] (3) The preparation method of the firing agent provided by the present invention avoids the pollution to humans and the environment during the production and use of copper azotetrazole. DETAILED DESCRIPTION

[0079] The present disclosure may be more easily understood by reference to the following description in conjunction with examples, all of which constitute a part of the present disclosure. It should be understood that the present disclosure is not limited to the specific products, methods, conditions or parameters described and / or illustrated herein. Further, the terms used herein are only used for the purpose of describing specific embodiments by way of example and are not intended to be limiting unless otherwise indicated.

[0080] It should also be understood that, for the sake of clarity, certain features of the present disclosure may be described herein in the context of separate embodiments, but may also be provided in combination with each other in a single embodiment. That is, unless clearly incompatible or specifically not included, each separate embodiment is considered to be combinable with any other embodiment, and the combination is considered to represent another different embodiment. Conversely, for the sake of simplicity, the various features of the present disclosure described in the context of a single embodiment may also be provided individually or in any sub-combination. Finally, although a particular embodiment may be described as part of a series of steps or part of a more general structure, each step or substructure itself may also be considered to be an independent embodiment.

[0081] Unless otherwise indicated, it should be understood that each individual element in a list and each combination of individual elements in the list will be interpreted as a different embodiment. For example, a list of embodiments represented as "A, B, or C" should be interpreted to include embodiments "A", "B", "C", "A or B", "A or C", "B or C", or "A, B, or C".

[0082] In the present disclosure, the singular forms of the articles "a", "an", and "the" also include the corresponding plural references, and a reference to a specific value includes at least that specific value unless the context clearly indicates otherwise. Thus, for example, a reference to "a substance" is a reference to at least one of that substance and equivalents thereof.

[0083] The terms including ordinal numbers such as "first" and "second" can be used to explain various components or fluids, but these components and fluids are not limited by these terms. Therefore, without departing from the teachings of the present disclosure, these terms are only used to distinguish the component / fluid from another component / fluid.

[0084] When items are described by using conjunction terms such as “… and / or…”, the description should be understood to include any one of the associated listed items and all combinations of one or more thereof; for example, A and / or B should be interpreted as an embodiment including “A” but not including “B”, an embodiment including “B” but not including “A”, and an embodiment including “A” and “B”.

[0085] In general, the use of the term "about" indicates an approximate value that may vary depending on the desired properties obtained by the disclosed subject matter, and will be interpreted in a context-dependent manner based on function. Therefore, one of ordinary skill in the art will be able to interpret a certain degree of difference on a case-by-case basis. In some cases, the number of significant figures used when expressing a particular value can be a representative technique for determining the difference allowed by the term "about". In other cases, a gradient in a range of values ​​can be used to determine the range of differences allowed by the term "about". Further, all ranges in this disclosure are inclusive and combinable, and reference to the values ​​stated in the range includes each value within the range.

[0086] Throughout the specification of this application document, when a certain part is described as “including” a certain constituent element, unless otherwise clearly described to the contrary, it does not mean that other constituent elements are excluded but that other constituent elements may also be included.

[0087] Throughout the specification of the present invention, when a certain step is recorded as being "above" or "before" other steps, it not only includes the case where a certain step has a direct time series relationship with other steps, but also includes the same rights as the case where a certain step has an indirect time series relationship where the time series of the order of two steps is changed, such as a mixing step after each step.

[0088] Throughout the specification of the present invention, when it is recorded as "according to any embodiment of the ... aspect of the ... object of the present invention...", unless otherwise clearly stated to the contrary, it does not mean that the constituent elements of the described scheme that appear before and after it are excluded, but that other constituent elements may also be included.

[0089] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs; the terms used herein and / or include any and all combinations of one or more of the associated listed items.

[0090] In order to demonstrate the technical solutions and advantages of the present invention, the technical solutions in the embodiments of the present invention will be fully described below.

[0091] [1] The method for preparing the firing agent of the present invention comprises the following steps:

[0092] 1) mixing solid component raw materials, and filling the mixed solid component raw materials into a container;

[0093] The component raw materials include sodium azotetrazolyl and a copper source; further, the addition amount of the sodium azotetrazolyl and the copper source is calculated according to the molar ratio of the azotetrazolyl anion to the divalent copper ion of (1-2): (2-1); optionally, the molar ratio of the azotetrazolyl anion to the divalent copper ion is 1: (2-1); or the molar ratio of the azotetrazolyl anion to the divalent copper ion is 2: (2-1); or the molar ratio of the azotetrazolyl anion to the divalent copper ion is (1-2): 1; or the molar ratio of the azotetrazolyl anion to the divalent copper ion is (1-2): 2; or the molar ratio of the azotetrazolyl anion to the divalent copper ion is (1-2): 2; the ideal result is that the molar ratio of the azotetrazolyl anion to the divalent copper ion that actually participates in the reaction can be kept infinitely close to 1: 1.

[0094] The component raw materials also include a binder; based on the total amount of sodium azotetrazolyl and copper source added, the amount of the binder added accounts for 0.5-8wt% of the total amount added.

[0095] In addition, the component raw materials may further include a reducing agent and / or an oxidizing agent; the amount of the reducing agent added accounts for 6 to 30 wt% of the total amount of the sodium azotetrazolyl and copper source added; the amount of the oxidizing agent added accounts for 65 to 85 wt% of the total amount of the sodium azotetrazolyl and copper source added.

[0096] The sodium azotetrazolyl in the component raw material is used to provide anionic azotetrazolyl. Further, the particle size of the sodium azotetrazolyl needs to be micrometer level, preferably not more than 400 micrometers, more preferably not more than 420 micrometers, or, the sodium azotetrazolyl as the component raw material can be sieved through a sieve, and the sodium azotetrazolyl can at least pass through a sieve of 40 mesh.

[0097] The copper source in the component raw material is used to provide copper ions. Therefore, there is no particular limitation on the type of the copper source, and examples thereof include copper salts such as copper sulfate, copper nitrate, copper chloride and its hydrate. Further, the particle size of the copper source needs to be micrometer level, preferably not more than 400 micrometers, more preferably not more than 420 micrometers, or, the copper source as the component raw material can be sieved through a sieve, and the copper source can at least pass through a 40-mesh sieve.

[0098] As a binder in the component raw materials, one of its functions is to facilitate granulation and bonding. There is no special limitation on the type of the binder, but for environmental protection considerations, water-soluble glue is preferably used, for example, any one of 901 glue, hydroxypropyl methylcellulose, polyvinyl alcohol, etc., which are non-toxic and environmentally friendly.

[0099] As a reducing agent in the component raw material, one of its functions is to improve the sensitivity. As for the types of the reducing agent, for example, there can be mentioned: any one or two of zirconium powder and aluminum powder; the amount of zirconium powder added accounts for 0-20wt% of the total amount added; the preferred amount added is 0-15wt%, more preferably 6-10wt%, and more preferably 8-10wt%; the amount of aluminum powder added accounts for 0-30wt% of the total amount added; the preferred amount added is 8-30wt%, more preferably 13-30wt%, and more preferably 20-30wt%. Furthermore, the particle size of the reducing agent needs to be micron level, preferably not more than 300 microns, more preferably not more than 200 microns, or, as a component raw material, the reducing agent can be sieved through a sieve, and the reducing agent can at least pass through a 60-mesh sieve. In addition,

[0100] As an oxidant in the component raw material, one of its functions is to improve sensitivity. For the types of the oxidant, for example, any one, two or three of copper oxide, iron oxide and bismuth oxide can be cited; the amount of copper oxide added accounts for 0-80wt% of the total amount added; the preferred amount added is 60-80wt%, more preferably 70-80wt%, and more preferably 74-80wt%; the amount of iron oxide added accounts for 0-80wt% of the total amount added; the preferred amount added is 70-80wt%, more preferably 70-75wt%, and more preferably 74wt%; the amount of bismuth oxide added accounts for 0-80wt% of the total amount added; the preferred amount added is 70-80wt%, more preferably 70-75wt%, and more preferably 74wt%; the amount of bismuth oxide added accounts for 0-80wt% of the total amount added; the preferred amount added is 70-80wt%, and more preferably 75wt%. Further, the particle size of the oxidant needs to be micron-level, preferably not more than 300 microns, and more preferably not more than 200 microns, or, as a component raw material, the oxidant can be sieved through a sieve, and the oxidant can at least pass through a 60-mesh sieve.

[0101] As the "container", the basic requirement it meets is that it can accommodate the corresponding amount of component raw materials; under this premise, it can be further clarified that the better choice for the "container" is a "container" that is directly used to hold or contain the "gunpowder or firing powder" when the later copper azotetrazole is used as "gunpowder or firing powder", such as primer shells and detonators.

[0102] 2) placing the container in an environment with a certain temperature and humidity for treatment;

[0103] The temperature of the environment is 20 to 80 degrees Celsius, preferably 20 to 60 degrees Celsius, and may also be 25 to 35 degrees Celsius;

[0104] The humidity of the environment, measured by relative humidity, has a relative humidity of not less than 40%, and the "relative humidity" as mentioned herein specifically refers to the percentage of the water vapor pressure in the air to the saturated water vapor pressure at the same temperature; the calculation method is U = E / E ω , where U is the relative humidity, E is the water vapor pressure at that temperature (Pa), and E ω is the saturated water vapor pressure (Pa) at that temperature; its detection methods include dry-wet bulb method, telescopic method, electrolysis method, electronic humidity sensor, etc. In the present invention, an electronic humidity sensor is used for inspection. Regarding the selection of humidity, if it is to improve the preparation efficiency or reduce the ambient temperature, it is preferred that the environment has a relative humidity of not less than 60%, and it is most preferred that the environment has a relative humidity of not less than 80%.

[0105] The treatment time is 0.5 to 72 hours.

[0106] Further examples include:

[0107] The temperature of the environment can be 20 degrees Celsius, the relative humidity of the environment can be 60%, and the treatment time can be 72 hours;

[0108] The temperature of the environment can be 30 degrees Celsius, the relative humidity of the environment can be 60%, and the treatment time can be 60 hours;

[0109] The temperature of the environment can be 40 degrees Celsius, the relative humidity of the environment can be 60%, and the treatment time can be 48 hours;

[0110] The temperature of the environment can be 60 degrees Celsius, the relative humidity of the environment can be 60%, and the treatment time can be 24 hours;

[0111] The temperature of the environment can be 80 degrees Celsius, the relative humidity of the environment can be 60%, and the treatment time can be 12 hours;

[0112] The temperature of the environment can be 30 degrees Celsius, the relative humidity of the environment can be 80%, and the treatment time can be 12 hours;

[0113] The temperature of the environment may be 40 degrees Celsius, the relative humidity of the environment may be 90%, and the treatment time may be 8 hours.

[0114] In addition, it should be noted that, depending on the actual need to produce and use the target product "detonator" in situ, a compaction step can be selectively added between the preparation steps 1) and 2) of the detonator, as follows: the mixed solid component raw materials filled into the container need to have a certain density, and the density can be selected according to the actual application requirements or other factors. For example, when the copper azotetrazole is used as an explosive, the pressing step can be performed as required to achieve the density requirement.

[0115] There is no special requirement for the method of making the mixed solid component raw materials filled into the container have a certain density. For example, it can be compacted by rolling, tamping or vibration. The intensity of the compaction can be selected within the pressure range of 50 to 150 MPa, preferably 100 MPa.

[0116] Before the "compacting process", the "solid component raw materials" are preferably subjected to a "mixing" process. The "mixing" method is not particularly limited, and any known method that can help the materials to be mixed more evenly can be used, for example: mixing using a pharmaceutical mixer (also called a pharmaceutical mixer); or mixing using a high-speed mixer.

[0117] In addition, it should be noted that in order to improve certain aspects of the performance of the primer or detonator, such as mechanical sensitivity, ignition ability, etc., ingredients such as combustibles, oxidants, desensitizers, sensitizers or adhesives may be added to the solid component raw materials in the preparation process of the aforementioned firing powder, especially in step 1) of the preparation process.

[0118] [2] Based on the preparation method provided by the present invention, the present invention can also provide a firing charge, wherein the firing charge is essentially a composition containing azotetrazolyl copper explosive. The content of the azotetrazolyl copper explosive is 10-70wt%, and in addition, the composition also includes a corresponding sodium salt.

[0119] The content of copper azotetrazolyl in the composition depends on the particle size, dosage, ratio, and process parameters of the raw material components; the type of the metal sodium salt in the composition depends on the use of the raw material (copper source);

[0120] For example, if the copper source is copper sulfate, the content of the azotetrazolyl copper obtained can be controlled to be 10-61 wt %, and the corresponding sodium salt is sodium sulfate.

[0121] If the copper source is copper chloride, the content of the azotetrazolyl copper obtained can be controlled to be 10-66wt%, and the corresponding sodium salt is sodium chloride.

[0122] If the copper source is copper nitrate, the content of the azotetrazolyl copper obtained can be controlled to be 10-57wt%, and the corresponding sodium salt is sodium nitrate.

[0123] However, the content of copper azotetrazolyl is usually less than 70wt%. For example, the amount and ratio of sodium azotetrazolyl and copper source used to prepare copper azotetrazolyl solid component raw materials, if the copper source is excessive, the sodium azotetrazolyl can be guaranteed to have a higher conversion rate, if the sodium azotetrazolyl is excessive, the copper salt can be guaranteed to have a higher conversion rate, and the sensitivity of the product can be adjusted by controlling the excess raw materials;

[0124] For example, the particle size of the sodium azotetrazolyl is below 60 mesh; the particle size of the copper source is below 60 mesh.

[0125] For example, in step 2), the ambient temperature, ambient humidity and treatment time for the reaction are:

[0126] The temperature of the environment is 20±2 degrees Celsius, the relative humidity of the environment is 40±2%, and the treatment time is 48 hours; the content of copper azotetrazole in the obtained product is not less than 10wt%;

[0127] The temperature of the environment is 30±2 degrees Celsius, the relative humidity of the environment is 80±2%, and the treatment is 12 hours; the content of copper azotetrazole in the obtained product is not less than 15wt%;

[0128] The temperature of the environment is 30±2 degrees Celsius, the relative humidity of the environment is 80±2%, and the treatment is 24 hours; the content of copper azotetrazole in the obtained product is not less than 20wt%;

[0129] The temperature of the environment is 40±2 degrees Celsius, the relative humidity of the environment is 90±2%, and the treatment is 12 hours; the content of copper azotetrazole in the obtained product is not less than 30wt%;

[0130] The content of copper azotetrazolyl in the product can be characterized by the following idea: the sample to be tested is fully dissolved with water, and the remaining insoluble part is copper azotetrazolyl.

[0131] [4] Based on the method for preparing the firing charge provided by the present invention, the method for achieving the safe use of the firing charge as a detonator and further obtaining a percussion cap or a detonator is as follows:

[0132] According to the preparation step 1) of the firing charge, the solid component raw materials (sodium tetrazolyl chloride and copper source) are directly mixed and filled into a cap shell or a detonator;

[0133] According to the preparation step 2) of the firing powder, the cap shell or detonator is placed in a corresponding environment for reaction.

[0134] What needs to be clarified at this point is that it is recommended to add a compaction step between the preparation steps 1) and 2) of the aforementioned detonating agent, as follows: the mixed solid component raw materials filled into the container need to have a certain density, and the size of the density can be selected according to the actual application requirements or other factors. For example, when the copper azotetrazole is used as a detonating agent, the pressing step can be carried out as required to achieve the density requirement.

[0135] There is no special requirement for the method of making the mixed solid component raw materials filled into the container have a certain density. For example, it can be compacted by rolling, tamping or vibration. The intensity of the compaction can be selected within the pressure range of 50 to 150 MPa, preferably 100 MPa.

[0136] Before the "compacting process", the "solid component raw materials" are preferably "mixed". The "mixing" method is not particularly limited, and any known method that can help the materials mix more evenly can be used, for example: mixing using a pharmaceutical mixer (also called a pharmaceutical mixer); or mixing using a high-speed mixer.

[0137] In addition, it should be noted that in order to improve certain aspects of the performance of the primer or detonator, such as mechanical sensitivity, ignition ability, etc., ingredients such as combustibles, oxidants, desensitizers, sensitizers or adhesives may be added to the solid component raw materials in the preparation process of the aforementioned firing powder, especially in step 1) of the preparation process.

[0138] Example 1 (Preparation method example)

[0139] Weigh a certain proportion of the raw materials sodium azotetrazolyl and copper sulfate;

[0140] Add the mixture into the mixing tank, start the mixer and mix for 30 minutes before discharging;

[0141] Pressing the mixed component raw materials into a reaction container;

[0142] Place the reaction container in a constant temperature and humidity chamber for reaction;

[0143] After being taken out, the mixture is dried to obtain a product composition, wherein the product composition contains copper azotetrazole.

[0144] [Specific process parameters used in the preparation of sample 1]:

[0145] Sodium azotetrazolyl: copper sulfate (weight ratio) = 55:45; (the molar ratio of anionic azotetrazolyl: copper ion is 1:1);

[0146] The sodium azotetrazolyl chloride is sieved through a 60-mesh sieve before use, and the sieve residue is taken;

[0147] The copper sulfate is sieved through a 60-mesh sieve before use, and the sieve residue is taken;

[0148] The pressure of the mixed raw materials into the reaction vessel is 100MPa;

[0149] The reaction container directly selects the cap shell;

[0150] The temperature of the thermostat is 30 degrees Celsius and the relative humidity is greater than 85%;

[0151] The reaction time is 12h.

[0152] [Specific process parameters used in the preparation of sample 2]:

[0153] Sodium azotetrazolyl: copper sulfate (weight ratio) = 55:45; (anion azotetrazolyl: copper ion molar ratio is 1:1)

[0154] The sodium azotetrazolyl chloride is sieved through a 40-mesh sieve before use, and the sieve residue is taken;

[0155] The copper sulfate is passed through a 40-mesh sieve before use, and the sieve residue is taken;

[0156] The pressure of the mixed raw materials into the reaction vessel is 100MPa;

[0157] The reaction container directly selects the cap shell;

[0158] The temperature of the thermostat is 30 degrees Celsius and the relative humidity is greater than 85%;

[0159] The reaction time is 12h.

[0160] [Specific process parameters used in the preparation of comparative sample 1]:

[0161] Basically the same as [Sample 2], the only difference is that the sodium azotetrazolyl oxide particles are larger, and are sieved through a 10-mesh sieve before use, and the sieve residue is taken;

[0162] The copper sulfate particles are relatively large and are sieved through a 10-mesh sieve before use to obtain the material under the sieve.

[0163] [Specific process parameters used in the preparation of sample 3]:

[0164] Sodium azotetrazolyl: copper sulfate (weight ratio) = 55:45; (anion azotetrazolyl: copper ion molar ratio is 1:1)

[0165] The sodium azotetrazolyl chloride is sieved through a 60-mesh sieve before use, and the sieve residue is taken;

[0166] The copper sulfate is sieved through a 60-mesh sieve before use, and the sieve residue is taken;

[0167] The pressure of the mixed raw materials into the reaction vessel is 80MPa;

[0168] The reaction container directly selects the cap shell;

[0169] The temperature of the thermostat is 30 degrees Celsius and the relative humidity is greater than 85%;

[0170] The reaction time is 12h.

[0171] [Specific process parameters used in the preparation of sample 4]:

[0172] Sodium azotetrazolyl: copper sulfate (weight ratio) = 55:45; (anion azotetrazolyl: copper ion molar ratio is 1:1)

[0173] The sodium azotetrazolyl chloride is sieved through a 60-mesh sieve before use, and the sieve residue is taken;

[0174] The copper sulfate is sieved through a 60-mesh sieve before use, and the sieve residue is taken;

[0175] The pressure of the mixed raw materials into the reaction vessel is 100MPa;

[0176] The reaction container directly selects the cap shell;

[0177] The temperature of the thermostat is 20 degrees Celsius and the relative humidity is greater than 85%;

[0178] The reaction time is 48h.

[0179] [Specific process parameters used in the preparation of comparative sample 2]:

[0180] Basically the same as [Sample 4], the only difference is that the temperature of the thermostatic box is 10 degrees Celsius, and the sieve is sieved with a 10-mesh sieve before use, and the sieve is taken;

[0181] The copper sulfate particles are relatively large and are sieved through a 10-mesh sieve before use to obtain the material under the sieve.

[0182] [Specific process parameters used in the preparation of comparative sample 3]:

[0183] Basically the same as [Sample 4], the only difference is that the reaction time is 12h.

[0184] [Specific process parameters used in the preparation of comparative sample 4]:

[0185] Basically the same as [Sample 4], the only difference is that the relative humidity does not exceed 50%.

[0186] [Specific process parameters used in the preparation of sample 5]:

[0187] Sodium azotetrazolyl: copper sulfate (weight ratio) = 55:45; (anion azotetrazolyl: copper ion molar ratio is 1:1)

[0188] The sodium azotetrazolyl chloride is sieved through a 60-mesh sieve before use, and the sieve residue is taken;

[0189] The copper sulfate is sieved through a 60-mesh sieve before use, and the sieve residue is taken;

[0190] The pressure of the mixed raw materials into the reaction vessel is 100MPa;

[0191] The reaction container directly selects the cap shell;

[0192] The temperature of the thermostat is 30 degrees Celsius and the relative humidity is greater than 75%;

[0193] The reaction time is 48h.

[0194] [Specific process parameters used in the preparation of sample 6]:

[0195] Sodium azotetrazolyl: copper sulfate (weight ratio) = 55:45; (anion azotetrazolyl: copper ion molar ratio is 1:1)

[0196] The sodium azotetrazolyl chloride is sieved through a 60-mesh sieve before use, and the sieve residue is taken;

[0197] The copper sulfate is sieved through a 60-mesh sieve before use, and the sieve residue is taken;

[0198] The pressure of the mixed raw materials into the reaction vessel is 100MPa;

[0199] The reaction container directly selects the cap shell;

[0200] The temperature of the thermostat is 30 degrees Celsius and the relative humidity is greater than 85%;

[0201] The reaction time is 4h.

[0202] [Specific process parameters used in the preparation of sample 7]:

[0203] Sodium azotetrazolyl: copper sulfate (weight ratio) = 55:45; (anion azotetrazolyl: copper ion molar ratio is 1:1)

[0204] The sodium azotetrazolyl chloride is sieved through a 60-mesh sieve before use, and the sieve residue is taken;

[0205] The copper sulfate is sieved through a 60-mesh sieve before use, and the sieve residue is taken;

[0206] The pressure of the mixed raw materials into the reaction vessel is 100MPa;

[0207] The reaction container directly selects the cap shell;

[0208] The temperature of the thermostat is 20 degrees Celsius and the relative humidity is greater than 40%;

[0209] The reaction time is 48h.

[0210] [Specific process parameters used in the preparation of sample 8]:

[0211] Sodium azotetrazolyl: copper sulfate (weight ratio) = 55:45; (anion azotetrazolyl: copper ion molar ratio is 1:1)

[0212] The sodium azotetrazolyl chloride is sieved through a 60-mesh sieve before use, and the sieve residue is taken;

[0213] The copper sulfate is sieved through a 60-mesh sieve before use, and the sieve residue is taken;

[0214] The pressure of the mixed raw materials into the reaction vessel is 50MPa;

[0215] The reaction container directly selects the cap shell;

[0216] The temperature of the thermostat is 30 degrees Celsius and the relative humidity is greater than 85%;

[0217] The reaction time is 12h.

[0218] Example 2

[0219] The ignition test adopts the explosion probability method. In this embodiment, referring to "GJB 3196.13A-2005 Gun and Bullet Test Method Part 13: Primer Impact Sensitivity Test", the ignition sensitivity test is carried out using an explosion probability method, and a falling ball weight of 55g is used.

[0220] The formulations of various embodiments and comparative examples and their product properties are shown in Table 1.

[0221] Table 1 Samples and comparative samples and their properties

[0222]

[0223]

[0224] Example 3

[0225] According to different proportions, sodium tetrazolyl chloride (under 60 mesh), copper sulfate (under 60 mesh), adhesive, and zirconium powder (under 60 mesh) are added to the mixing tank, and the mixer is started to mix for 30 minutes, and the material is discharged. The mixed material is pressed into the cap shell, and the cap shell is placed in a constant temperature and humidity chamber with a temperature of 30 degrees Celsius and a relative humidity greater than 85% for in-situ reaction for 12 hours. After being taken out, it is dried and assembled into products (samples 9 to 16) for testing. The ignition test adopts the explosion probability method (refer to "GJB 3196.13A-2005 Bullet Test Method Part 13: Primer Impact Sensitivity Test"), and a falling ball weight of 55g is used.

[0226] The formulations of various embodiments and comparative examples and their product properties are shown in Table 2.

[0227] Table 2 Samples and comparative samples and their properties

[0228] Sodium azotetrazolyl / % Copper salt / % Zirconium powder / % Adhesive (added) / % Drop height / cm Firing rate Sample 9 55 45(Copper sulfate) 5 1(Hydroxypropyl methylcellulose) 240 100 / 100 Sample 10 55 45(Copper sulfate) 5 10(Hydroxypropyl methylcellulose) 240 100 / 100 Sample 11 65 35(Copper sulfate) 0 5(Hydroxypropyl methylcellulose) 240 100 / 100 Sample 12 40 60(Copper sulfate) 20 5(Hydroxypropyl methylcellulose) 240 100 / 100 Sample 13 55 45(Copper nitrate) 5 5(Hydroxypropyl methylcellulose) 240 100 / 100 Sample 14 55 45(Copper chloride) 5 5(Hydroxypropyl methylcellulose) 280 100 / 100 Sample 15 55 45(Copper sulfate) 5 5(Polyvinyl alcohol) 240 100 / 100 Sample 16 55 45(Copper sulfate) 5 5(901 glue) 280 100 / 100

[0229] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a firing agent, characterized in that: The component raw materials of the firing medicine include: Sodium azotetrazolyl; a source of copper; and, Adhesives; The addition amount of the sodium azotetrazolyl and copper source is calculated according to the molar ratio of the azotetrazolyl anion to the divalent copper ion of (1-2): (2-1); Calculated based on the total amount of sodium azotetrazolyl and copper source added, the amount of the binder added accounts for 0.5 to 8 wt% of the total amount added; The preparation of the firing medicine comprises the following steps: 1) mixing the component raw materials and filling the mixed component raw materials into a container; 2) placing the container in an environment with a temperature of 20 to 80 degrees Celsius and a relative humidity of not less than 40% for 0.5 to 72 hours to form the firing charge.

2. The method for preparing the firing agent according to claim 1, characterized in that: In step 1), the sodium azotetrazolyl can pass through a sieve of not less than 40 mesh; and / or, The particle size of the sodium azotetrazolyl oxide is no more than 400 microns.

3. The method for preparing the firing agent according to claim 2, characterized in that: The copper source can pass through a sieve of not less than 40 mesh; and / or, The particle size of the copper source does not exceed 400 microns.

4. The method for preparing the firing agent according to any one of claims 1 to 3, characterized in that: The component raw materials of the firing medicine also include: reducing and / or oxidizing agents; The reducing agent includes any one or both of zirconium powder and aluminum powder; The oxidant includes any one, two or three of copper oxide, iron oxide and bismuth oxide; The amount of the reducing agent added is 6 to 30 wt % of the total amount of the sodium azotetrazolyl and the copper source added; The added amount of the oxidant accounts for 65-85 wt % of the total amount of the sodium azotetrazolyl and the copper source.

5. The method for preparing the firing medicine according to claim 4, characterized in that: The oxidant or reductant can pass through a sieve of not less than 60 mesh; and / or, The particle size of the oxidizing agent or reducing agent does not exceed 300 microns.

6. The method for preparing the firing powder according to any one of claims 1 to 5, characterized in that: In step 2), the container is placed at a temperature of 20 to 60 degrees Celsius; preferably, the container is placed at a temperature of 20 to 40 degrees Celsius; and / or, In step 2), the container is placed in an environment with a relative humidity of not less than 60%; preferably, the container is placed in an environment with a relative humidity of not less than 70%.

7. The method for preparing the firing agent according to any one of claims 1 to 5, characterized in that: In step 1), the mixed component raw materials are compacted.

8. The method for preparing the firing medicine according to claim 7, characterized in that: The mixed component raw materials are compacted at a pressure of not less than 50 MPa; Preferably, the mixed component raw materials are compacted using a pressure of 50 to 150 MPa.

9. A firing charge, characterized in that: The firing charge is prepared by the method according to any one of claims 1 to 6.

10. The firing charge according to claim 9, characterized in that: The firing charge comprises: Copper azotetrazolyl, and Sodium salt; The content of the sodium salt is no more than 60 wt %, preferably 18-60 wt %.

11. A percussion cap or detonator, characterized in that: The percussion charge is contained in the percussion cap or detonator, and the percussion charge is prepared by the method according to any one of claims 1 to 8; and / or, In the firing charge, the content of copper azotetrazolyl accounts for no less than 10%; Preferably, the content of copper azotetrazolyl is not less than 35%.

12. An in-situ application method of a firing charge, characterized in that: The firing charge is prepared by the method according to any one of claims 1 to 8; wherein The container includes any one or more of a cap shell, a primer shell, and a detonator shell.

Citation Information

Patent Citations

  • Energetic coordination complex based on azo tetrazole azotetrazole and use thereof

    CN101434617A

  • Copper azotetrazole, composition containing copper azotetrazole as well as preparation method and application of copper azotetrazole