Hexamer surfactant and synthesis method thereof

By reacting alkylphenol polyoxyethylene ether with hexachlorocyclotriphosphazene in an organic solvent, a hexameric surfactant with excellent properties was successfully prepared, which solved the problem of difficulty in synthesizing multimeric surfactants and achieved Hexameric surfactant with low critical micelle concentration and flame retardant properties suitable for a variety of applications.

CN118724964AInactive Publication Date: 2024-10-01CHANGZHOU UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410753380.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult to synthesize multimeric surfactants in the prior art, especially there are few reports on oligomeric surfactants above the trimer type, and there is a lack of surfactants based on polyphosphazene derivatives.

Method used

By reacting alkylphenol polyoxyethylene ether with active hydrogen and hexachlorocyclotriphosphazene in an organic solvent, alkylphenol polyoxyethylene having a six-membered ring skeleton of hexachlorocyclotriphosphazene phosphorus and nitrogen is prepared. The hexameric surfactant with ether organic groups realizes a one-step reaction under simple process conditions to obtain a hexameric surfactant with excellent performance.

Benefits of technology

A hexameric surfactant with a lower critical micelle concentration was realized, which has fire-extinguishing and flame-retardant properties and is suitable for emulsifiers, dispersants, flame retardants and fire-extinguishing agents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724964A_ABST
    Figure CN118724964A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of fine chemicals, and particularly relates to a hexameric surfactant and a synthesis method thereof. In an organic solvent, alkyl (phenol) polyoxyethylene ether with reactive hydrogen and phosphonitrilic chloride trimer are used as raw materials, and the hexaalkyl (phenol) polyoxyethylene ether cyclotriphosphazene surfactant is obtained through a one-step reaction in the presence of an acid application agent. The hexameric surfactant obtained by the synthesis method has the characteristics of high surface activity, flame retardance, rich nitrogen and phosphorus and the like, and can be used as an emulsifier, a fire extinguishing agent, a flame retardant and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of fine chemicals, and in particular relates to a hexameric surfactant and a synthesis method thereof. Background Art

[0002] Polyphosphazenes are a class of linear or cyclic polymers with nitrogen and phosphorus double bonds arranged alternately. Their properties are between those of inorganic and organic substances. Among them, hexachlorocyclotriphosphazene (HCCP) is one of the earliest synthesized polyphosphazene compounds. HCCP is a cyclic compound that exhibits some unique properties due to its special structure. On the one hand, the conjugation effect of the phosphorus and nitrogen main chains makes it have good thermal stability and chemical inertness. It is difficult to be oxidized and not easy to open the ring when placed in the air; on the other hand, the chlorine connected to phosphorus has very high chemical activity and is easily replaced by various nucleophilic reagents in a certain environment to obtain cyclophosphazene compounds containing various groups.

[0003] CN114685565A discloses a method for preparing a class of fluorine-containing phenoxy cyclotriphosphazene compounds, using hexachlorocyclotriphosphazene and m-trifluoromethylphenol as raw materials, and synthesizing hexa-m-trifluoromethylphenoxy cyclotriphosphazene through a simple process. The product not only has good heat stability and acid and alkali corrosion resistance, but also has high hydrophobicity, and can be used in flame retardant materials, coating materials or lubricating materials and other fields.

[0004] CN104725428B discloses a method for preparing melamine-modified polyaminocyclotriphosphazene, which is prepared by condensation, re-ammoniation and finally heating polycondensation using hexachlorocyclotriphosphazene and melamine as reaction substrates. The water solubility and hygroscopicity of the product are significantly reduced, and the thermal stability is significantly improved.

[0005] CN113024605A and CN117105986A disclose methods for preparing hexaphenoxy cyclotriphosphazene and hexaphenylamino cyclotriphosphazene, respectively, both of which are used as good flame retardants in the flame retardant field. CN111040185A discloses a method for preparing a multifunctional composite flame retardant CMSs-HCCP-CS, which uses carbon microspheres as cores and hexachlorocyclotriphosphazene as a connecting bridge, and grafts carboxymethyl chitosan with excellent antibacterial properties on the surface of carbon microspheres, thereby constructing a multifunctional composite flame retardant with both flame retardant and antibacterial effects.

[0006] Surfactants are an important class of fine chemicals, known as "industrial MSG", and can be used in technology and production departments such as washing, cosmetics, petroleum, food, and chemistry. Traditional single-chain surfactants are amphiphilic molecules with one hydrophilic group and one lipophilic group. Oligomeric surfactants covalently connect two or more single-chain surfactants near the hydrophilic group through chemical bonds. Compared with single-chain surfactants, oligomeric surfactants have higher surface activity, better foaming performance, lower critical micelle concentration, richer aggregation behavior and many other more excellent properties. At present, the research on oligomeric surfactants is mainly focused on dimerization (Gemini) and trimerization. Due to the difficulty of synthesis, there are relatively few reports on oligomeric surfactants above the trimerization type.

[0007] The prior art discloses various flame retardants based on phosphazenes, but surfactants based on polyphosphazene derivatives have not been reported. Summary of the invention

[0008] In order to overcome the current situation that polymeric surfactants are difficult to synthesize, the present invention synthesizes a hexameric surfactant based on polyphosphazene. The hexameric surfactant synthesized by the present invention has both high surface activity and better emulsification, dispersing, flame retardant and fire extinguishing properties.

[0009] The hexameric surfactant of the present invention has both the phosphorus-nitrogen six-membered ring inorganic ring skeleton of hexachlorocyclotriphosphazene and the alkyl (phenol) polyoxyethylene ether organic group, and its general structural formula is as follows:

[0010]

[0011] R=C m H 2m+1 - or C m H 2m+1 (C6H4)-, m≥8, n≥3.

[0012] The synthesis process of the invention is simple, and the starting materials are alkyl (phenol) polyoxyethylene ether with active hydrogen and hexachlorocyclotriphosphazene. The specific synthesis method is: in an organic solvent, an acid binding agent, alkylphenol polyoxyethylene ether and hexachlorocyclotriphosphazene are put into a reaction container, heated and stirred to react, and after a period of time, the salt is removed by filtering, and the solvent is removed to finally obtain the product.

[0013] The organic solvent includes but is not limited to tetrahydrofuran, acetone and benzene.

[0014] Acid binding agents include but are not limited to NaH, KOH, NaOH, and triethylamine.

[0015] The reaction raw material alkylphenol polyoxyethylene ether includes but is not limited to octylphenol polyoxyethylene ether, nonylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether (AEO-3, AEO-7, AEO-9).

[0016] The molar ratio of the acid-binding agent, alkylphenol polyoxyethylene ether and hexachlorocyclotriphosphazene is 6:6:1. The reaction temperature is 45-65°C and the reaction time is 4-8h. After the reaction is completed, the salt is removed by filtration and the solvent is removed by reduced pressure distillation to obtain the target product.

[0017] Beneficial effects of the present invention:

[0018] The present invention is the first to react alkyl polyoxyethylene ether or fatty alcohol polyoxyethylene ether with surface activity with HCCP, and prepares hexaalkylphenol polyoxyethylene ether cyclotriphosphazene in only one step under mild conditions, thereby obtaining a hexameric surfactant with excellent performance. The hexameric surfactant not only has a lower critical micelle concentration, but also has certain fire extinguishing and flame retardant properties, and can be used as an emulsifier, dispersant, flame retardant and fire extinguishing agent. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 .Infrared spectrum of hexa(octylphenol polyoxyethylene ether) cyclotriphosphazene;

[0020] Figure 2 . Comparison of surface tension curves of hexa(octylphenol polyoxyethylene ether)cyclotriphosphazene and octylphenol polyoxyethylene ether;

[0021] Figure 3 .Infrared spectrum of hexa(nonylphenol polyoxyethylene ether) cyclotriphosphazene;

[0022] Figure 4 .Surface tension curve of hexa(nonylphenol polyoxyethylene ether) cyclotriphosphazene;

[0023] Figure 5 .Infrared spectrum of hexa-(lauryl polyoxyethylene ether-7) cyclotriphosphazene;

[0024] Figure 6 .Surface tension curve of hexa-(lauryl polyoxyethylene ether-7) cyclotriphosphazene;

[0025] Figure 7 .Infrared spectrum of hexa-(lauryl polyoxyethylene ether-9) cyclotriphosphazene;

[0026] Figure 8 .Surface tension curve of hexa(lauryl polyoxyethylene ether-9) cyclotriphosphazene. DETAILED DESCRIPTION

[0027] The present invention is exemplarily described below in conjunction with specific embodiments, but the embodiments are given only as examples and are not considered to be the entire technical solution of the present invention, nor are they intended to limit the overall technical solution of the present invention. Anything with the same or similar technical features, simple changes or replacements, falls within the scope of protection of the present invention.

[0028] Example 1

[0029] 0.432g NaH, 11.679g octylphenol polyoxyethylene ether and 20mL tetrahydrofuran were mixed and added to a three-necked flask, and placed in an oil bath pot at 45°C with nitrogen protection for 1h. 1.043g hexachlorocyclotriphosphazene was dissolved in 25mL tetrahydrofuran and transferred to a constant pressure dropping funnel, and slowly dripped into the three-necked flask. After the addition was completed, the reaction was continued at 45°C for 3h. After the reaction was completed, the salt was filtered and removed, and the filtrate was finally subjected to reduced pressure distillation to remove the tetrahydrofuran solvent to obtain hexa-(octylphenol polyoxyethylene ether) cyclotriphosphazene.

[0030] The conversion rate of octylphenol polyoxyethylene ether was determined based on the hydroxyl value of the product before and after the reaction. The determination of hydroxyl value was carried out according to the third part of GB / T12008 "Plastic Polyether Polyols": Determination of Hydroxyl Value. The conversion rate of octylphenol polyoxyethylene ether was calculated to be 49.38%.

[0031] The product was separated by column chromatography and characterized by nuclear magnetic resonance: 1H NMR (400MHz, CDCl3) δ7.30-7.19 (m, 1H), 6.81 (d, J = 8.8 Hz, 1H), 4.17-4.05 (m, 1H), 3.90-3.80 (m, 1H), 3.74-3.56 (m, 14H), 1.68 (s, 1H), 1.32 (s, 3H), 0.69 (s, 4H), 0.06 (s, 2H).

[0032] The average molecular weight was determined to be 4234 by gel permeation chromatography.

[0033] The infrared characterization of the product is as follows Figure 1 shown.

[0034] Comparison of surface tension curves of product and raw material Figure 2 shown.

[0035] Example 2

[0036] Mix 1.043g hexachlorocyclotriphosphazene and 20mL tetrahydrofuran and add to a three-necked flask for later use. Mix 1.010g KOH, 11.679g octylphenol polyoxyethylene ether and 10mL deionized water and add to another three-necked flask, place in an oil bath pot at 60℃ for reaction for 3h, add 30mL of benzene as a water-carrying agent to the three-necked flask containing octylphenol polyoxyethylene ether, raise the oil bath temperature to 90℃ for vacuum distillation, then mix the obtained substance after distillation with 30mL tetrahydrofuran and transfer to a constant pressure dropping funnel, slowly drip into the three-necked flask containing hexachlorocyclotriphosphazene, and continue to react at 60℃ for 5h after the dropwise addition is completed. After the reaction is completed, filter and remove salt, and finally vacuum distill the filtrate to remove the tetrahydrofuran solvent to obtain hexa-(octylphenol polyoxyethylene ether) cyclotriphosphazene.

[0037] The conversion rate of octylphenol polyoxyethylene ether was determined based on the hydroxyl value of the product before and after the reaction. The determination of hydroxyl value was carried out according to the third part of GB / T12008 "Plastic Polyether Polyols": Determination of Hydroxyl Value. The conversion rate of octylphenol polyoxyethylene ether was calculated to be 64.37%.

[0038] Example 3

[0039] 11.679g of octylphenol polyoxyethylene ether, 1.043g of hexachlorocyclotriphosphazene, 5mL of triethylamine and 40mL of benzene solution were mixed and added to a three-necked flask, and placed in an oil bath at 65°C for 6h. After the reaction was completed, the salt was removed by filtration, and the filtrate was finally subjected to reduced pressure distillation to remove the benzene solvent to obtain hexa(octylphenol polyoxyethylene ether)cyclotriphosphazene.

[0040] The conversion rate of octylphenol polyoxyethylene ether was determined based on the hydroxyl value of the product before and after the reaction. The determination of hydroxyl value was carried out according to the third part of GB / T12008 "Plastic Polyether Polyols": Determination of Hydroxyl Value. The conversion rate of octylphenol polyoxyethylene ether was calculated to be 44.31%.

[0041] Example 4

[0042] 11.556g of nonylphenol polyoxyethylene ether, 0.432g of NaH and 20mL of benzene were mixed and added to a three-necked flask, and placed in an oil bath pot at 45°C with nitrogen protection for 1h. 1.043g of hexachlorocyclotriphosphazene and 25mL of benzene were mixed and transferred to a constant pressure dropping funnel and slowly dripped into the three-necked flask. After the addition was completed, the temperature was raised to 65°C and reacted for 4h. After the reaction was completed, the salt was filtered and removed, and the filtrate was finally subjected to reduced pressure distillation to remove the benzene solvent to obtain hexa-(nonylphenol polyoxyethylene ether) cyclotriphosphazene.

[0043] The conversion rate of nonylphenol polyoxyethylene ether was determined based on the hydroxyl values ​​of the products before and after the reaction. The determination of hydroxyl value was carried out according to the third part of GB / T12008 "Plastic Polyether Polyols": Determination of Hydroxyl Value. The conversion rate of nonylphenol polyoxyethylene ether was calculated to be 45.18%.

[0044] The product was separated by column chromatography and characterized by nuclear magnetic resonance: 1H NMR (400MHz, CDCl3) δ7.33-7.21 (m, 1H), 6.84 (d, J = 8.6 Hz, 1H), 4.13 (t, J = 4.8 Hz, 2H), 3.86 (t, J = 4.9 Hz, 1H), 3.80-3.58 (m, 20H), 1.71 (s, 1H), 1.35 (s, 3H), 0.72 (s, 5H).

[0045] The average molecular weight was determined to be 4451 by gel permeation chromatography.

[0046] The infrared characterization of the product is as follows Figure 3 shown.

[0047] The surface tension of the product changes with concentration. Figure 4 shown.

[0048] Example 5

[0049] 11.556g of nonylphenol polyoxyethylene ether, 1.043g of hexachlorocyclotriphosphazene, 5mL of triethylamine and 40mL of acetone were mixed and added to a three-necked flask, and placed in an oil bath at 45°C for 6h. After the reaction was completed, the salt was removed by filtration, and the filtrate was finally subjected to reduced pressure distillation to remove the acetone solvent to obtain hexa-(nonylphenol polyoxyethylene ether) cyclotriphosphazene.

[0050] The conversion rate of nonylphenol polyoxyethylene ether was determined based on the hydroxyl values ​​of the products before and after the reaction. The determination of hydroxyl value was carried out according to the third part of GB / T12008 "Plastic Polyether Polyols": Determination of Hydroxyl Value. The conversion rate of nonylphenol polyoxyethylene ether was calculated to be 57.52%.

[0051] Example 6

[0052] Mix 1.043g of hexachlorocyclotriphosphazene and 20mL of acetone and add them to a three-necked flask for later use. Mix 0.720g of NaOH, 8.905g of lauryl alcohol polyoxyethylene ether-7 (AEO-7) and 10mL of deionized water and add them to another three-necked flask. Place it in an oil bath pot and react at 45°C for 3h. Add 30mL of benzene as a water-carrying agent to the three-necked flask containing AEO-7, raise the oil bath temperature to 90°C for vacuum distillation, then mix the distilled substance with 30mL of acetone and transfer it to a constant pressure dropping funnel, slowly drip it into the three-necked flask containing hexachlorocyclotriphosphazene, and after the addition is completed, react at 45°C for 5h. After the reaction is completed, filter and remove salt, and finally vacuum distill the filtrate to remove the acetone solvent to obtain hexa-(lauryl alcohol polyoxyethylene ether-7) cyclotriphosphazene.

[0053] The conversion rate of AEO-7 was determined based on the hydroxyl value of the product before and after the reaction. The determination of hydroxyl value was carried out according to GB / T 12008 "Plastic Polyether Polyols" Part 3: Determination of Hydroxyl Value. The conversion rate of AEO-7 was calculated to be 58.47%.

[0054] The product was separated by column chromatography and characterized by nuclear magnetic resonance: 1H NMR (400MHz, CDCl3) δ7.30–7.23 (m, 1H), 6.84 (d, J = 8.8 Hz, 1H), 4.13 (t, J = 4.9 Hz, 1H), 3.90–3.83 (m, 1H), 3.75 (dt, J = 5.9, 2.5 Hz, 2H), 3.72–3.64 (m, 14H), 1.71 (s, 1H), 1.35 (s, 3H), 0.72 (s, 5H), 0.09 (s, 2H).

[0055] The average molecular weight was determined to be 4143 by gel permeation chromatography.

[0056] The infrared characterization of the product is as follows Figure 5 shown.

[0057] The surface tension of the product changes with concentration. Figure 6 shown.

[0058] Example 7

[0059] 10.491g of lauryl alcohol polyoxyethylene ether-9 (AEO-9), 1.043g of hexachlorocyclotriphosphazene, 5mL of triethylamine and 40mL of tetrahydrofuran solution were mixed and added into a three-necked flask, and placed in an oil bath pot at 45°C for 6h. After the reaction was completed, the salt was filtered and removed, and finally the filtrate was subjected to reduced pressure distillation to remove the tetrahydrofuran solvent to obtain hexa-(lauryl alcohol polyoxyethylene ether-9) cyclotriphosphazene.

[0060] The conversion rate of AEO-9 was determined based on the hydroxyl value of the product before and after the reaction. The determination of hydroxyl value was carried out according to GB / T 12008 "Plastic Polyether Polyols" Part 3: Determination of Hydroxyl Value. The conversion rate of AEO-9 was calculated to be 57.18%.

[0061] The average molecular weight was determined to be 4212 by gel permeation chromatography.

[0062] The infrared characterization of the product is as follows Figure 7 shown.

[0063] The surface tension of the product changes with concentration. Figure 8 shown.

[0064] Comparative Example 1

[0065] 0.432g NaH, 4.364g hexadecanol and 20mL tetrahydrofuran were mixed and added to a three-necked flask, and placed in an oil bath pot at 45°C with nitrogen protection for 1h. 1.043g hexachlorocyclotriphosphazene was dissolved in 25mL tetrahydrofuran and transferred to a constant pressure dropping funnel, and slowly dripped into the three-necked flask. After the addition was completed, the reaction was continued at 45°C for 3h. After the reaction was completed, the salt was removed by filtration, and the filtrate was finally subjected to reduced pressure distillation to remove the tetrahydrofuran solvent to obtain hexa-(hexadecanol)cyclotriphosphazene.

[0066] The conversion rate of hexadecanol was determined based on the hydroxyl values ​​of the products before and after the reaction. The determination of hydroxyl value was carried out in accordance with Part 3 of GB / T 12008 "Plastic Polyether Polyols": Determination of Hydroxyl Value. The conversion rate of hexadecanol was calculated to be 17.48%.

[0067] Application Example 1

[0068] Hexa-(octylphenol polyoxyethylene ether) cyclotriphosphazene was prepared into ethanol solutions with mass concentrations of 1%, 5%, 10%, 15%, and 20%. Five canvases with a size of 300mm*89mm were taken, and each canvas was soaked in a concentration for 30 minutes and then dried. A vertical combustion test was conducted on the soaked canvas, and the mass before and after combustion was recorded and the residual carbon rate was calculated. The results are shown in Table 1. It can be seen that after adding hexa-(octylphenol polyoxyethylene ether) cyclotriphosphazene, the residual carbon rate of the canvas after vertical combustion increased significantly, proving that it has a good flame retardant effect.

[0069] Table 1. Carbon residue rate of canvas with different concentrations of hexa(octylphenol polyoxyethylene ether) cyclotriphosphazene

[0070]

[0071] Application Example 2

[0072] The hexa-nonylphenol polyoxyethylene ether cyclotriphosphazene was prepared into ethanol solutions with a mass concentration of 1%, 5%, 10%, 15%, and 20%. Five canvases with a size of 300mm*89mm were taken, and each canvas was soaked in a concentration for 30 minutes and then dried. The soaked canvas was subjected to a vertical combustion test, and the mass before and after combustion was recorded and the residual carbon rate was calculated. The results are shown in Table 2. It can be seen that after the addition of hexa-(nonylphenol polyoxyethylene ether) cyclotriphosphazene, the residual carbon rate of the canvas after vertical combustion increased significantly, proving that it has a good flame retardant effect.

[0073] Table 2. Carbon residue rate of canvas with different concentrations of hexa-(nonylphenol polyoxyethylene ether) cyclotriphosphazene

[0074]

[0075] Application Example 3

[0076] Hexa-(hexadecanol) cyclotriphosphazene was prepared into ethanol solutions with mass concentrations of 1%, 5%, 10%, 15%, and 20%, and 5 pieces of canvas with a size of 300mm*89mm were taken. Each piece of canvas corresponded to a concentration and was soaked for 30 minutes and then dried. A vertical combustion test was conducted on the soaked canvas, and the mass before and after combustion was recorded and the residual carbon rate was calculated. The results are shown in Table 3. It can be seen that after adding hexa-(hexadecanol) cyclotriphosphazene, the residual carbon rate of the canvas after vertical combustion was slightly improved, proving that it only has a slight flame retardant effect.

[0077] Table 3. Carbon residue rate of canvas with different concentrations of hexa-(hexadecanol) cyclotriphosphazene

[0078]

Claims

1. A hexameric surfactant, characterized in that The hexameric surfactant has both a nitrogen-phosphorus six-membered ring inorganic skeleton and a polyoxyethylene ether organic group, and its general structural formula is as follows: R=C m H 2m+1 - or C m H 2m+1 (C6H4)-, m≥8, n≥3.

2. A method for synthesizing the hexameric surfactant according to claim 1, characterized in that: The synthesis method comprises the following steps: mixing alkyl (phenol) polyoxyethylene ether, hexachlorocyclotriphosphazene and an acid binding agent in an organic solvent, heating and stirring to react, then filtering to remove salt and removing the solvent, and finally obtaining a hexameric surfactant.

3. The method for synthesizing a hexameric surfactant according to claim 2, characterized in that: The alkylphenol polyoxyethylene ether is selected from octylphenol polyoxyethylene ether, nonylphenol polyoxyethylene ether and fatty alcohol polyoxyethylene ether.

4. The method for synthesizing a hexameric surfactant according to claim 2, characterized in that: The organic solvent is selected from tetrahydrofuran, acetone and benzene.

5. The method for synthesizing a hexameric surfactant according to claim 2, characterized in that: The acid binding agent is selected from NaH, KOH, NaOH and triethylamine.

6. The method for synthesizing a hexameric surfactant according to claim 2, characterized in that: The molar ratio of the acid binding agent, alkylphenol polyoxyethylene ether and hexachlorocyclotriphosphazene is 6:6:

1.

7. The method for synthesizing a hexameric surfactant according to claim 2, characterized in that: The reaction temperature is 45-65° C., and the reaction time is 4-8 hours.

8. Use of the hexameric surfactant according to claim 1, characterized in that: The hexameric surfactant is used as an emulsifier, dispersant, flame retardant and fire extinguishing agent.

Citation Information

Cited By

  • Method for synthesizing six-long-chain alkyl polyoxyethylene ether cyclotriphosphazene without solvent

    CN119219909A

  • Process for the solvent-free synthesis of hexa-long-chain-alkyl polyoxyethylene ether cyclotriphosphazene

    CN119219909B

  • Extreme-temperature-resistant nitrogen-phosphorus-silicon synergistic fire extinguishing agent suitable for lithium ion battery and preparation method of extreme-temperature-resistant nitrogen-phosphorus-silicon synergistic fire extinguishing agent

    CN121016125A