Transparent photochromic hydrogel and preparation method thereof
By using TiO2 quantum dots and K-Ca-Nb-O/MoS2 quantum dots in the hydrogel for ultrasonic mixing and light polymerization, combined with cross-linking agents and monomers, the problem of transparency when the hydrogel is combined with photochromic materials is solved To solve the problem of sex loss, we have achieved a uniform and transparent photochromic hydrogel, which can achieve color change and recovery under light.
Patent Information
- Application Number
- CN202410944651.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-15
AI Technical Summary
It is difficult for existing hydrogels to maintain transparency when combined with photochromic materials. The thermal initiator often causes gel clusters and loses transparency.
TiO2 quantum dots and K-Ca-Nb-O/MoS2 quantum dots are used as photochromic materials. Through ultrasonic mixing and light polymerization, cross-linking agents and monomers are combined to form a uniform photochromic hydrogel, which shortens the gelation time. Glue time to prevent cluster formation.
A uniform and transparent photochromic hydrogel is achieved, the gelation time is shortened, the transparency of the hydrogel is maintained, and the color can be changed and restored under light.
Smart Images

Figure CN118725192A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a photochromic hydrogel and a preparation method thereof, and belongs to the field of hydrogel and photochromism. Background Art
[0002] Hydrogel is a hydrophilic polymer material with a three-dimensional network structure. It can swell in water but will not dissolve. It is widely used in the biomedical field, especially as implants, drug carriers, biosensors or contact lenses. At the same time, hydrogel also has good recyclability and environmental friendliness. The gel itself is non-toxic and does not pollute the environment. Therefore, hydrogels are also often used in life scenes, such as hydroponic plants, water babies, etc. However, most of these hydrogels are colorless and transparent, and have a single form.
[0003] On the other hand, photochromic materials undergo reversible photochemical reactions under light excitation, presenting two reversible states with different structures. They are widely used in automotive glass, laser printing, displays, ultra-high-density optical information storage, optoelectronic devices, stimulus-responsive materials, etc.
[0004] Therefore, the combination of hydrogel and photochromic to make a color-changing hydrogel has important application value. However, simply adding photochromic materials (generally nanopowder materials) during the hydrogel synthesis process will cause the hydrogel to be opaque and lose the important properties of the hydrogel because it cannot be completely dissolved or dispersed in water. Even if organic photochromic materials or quantum dot photochromic materials are used, although they can be dissolved or dispersed in water, they will still cause clusters during the hydrogel synthesis process due to thermal initiators (which take hours or days to solidify), ultimately causing the hydrogel to be opaque. Summary of the invention
[0005] In order to combine hydrogel and photochromism to form a uniform and transparent photochromic hydrogel, the present invention provides a transparent photochromic hydrogel and a preparation method thereof.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing a photochromic hydrogel, comprising the following steps:
[0008] (1) dispersing TiO2 quantum dot initiator and K-Ca-Nb-O / MoS2 quantum dots in ultrapure water and mixing them thoroughly in an ultrasonic environment until a uniform solution is formed;
[0009] (2) adding a crosslinking agent to the above solution, stirring at a certain stirring rate to uniformly disperse the crosslinking agent in the solution, and then adding a monomer, maintaining the same stirring rate to fully prepolymerize the monomer and the crosslinking agent;
[0010] (3) subjecting the above solution to a polymerization reaction under light to finally obtain a photochromic hydrogel.
[0011] Preferably, in step (1), the photochromic material K-Ca-Nb-O / MoS2 is immersed in a butylamine solution and stirred for 7 days to expand the K-Ca-Nb-O / MoS2 layered structure by substitution to obtain K-Ca-Nb-O / MoS2 quantum dots.
[0012] Preferably, in step (1), the particle size of TiO2 quantum dots and K-Ca-Nb-O / MoS2 quantum dots is less than 5 nm.
[0013] Preferably, in step (1), the mass ratio of K-Ca-Nb-O / MoS2 quantum dots to TiO2 quantum dots is 1:1.
[0014] Preferably, in step (2), the crosslinking agent is N,N'-bis(acrylamide)cystamine, and the mass ratio of the crosslinking agent to the initiator is 1:5.
[0015] Preferably, in step (2), stirring is performed at a stirring rate of 200 rad / min.
[0016] Preferably, in step (2), the monomer is acrylamide, and the mass ratio of the monomer to the cross-linking agent is 1000:1.
[0017] Preferably, in step (3), ultraviolet light is used for illumination.
[0018] Preferably, in step (3), the polymerization reaction time is 1 to 10 min, preferably 5 min.
[0019] In a second aspect, the present invention provides a photochromic hydrogel prepared by the method described in the first aspect.
[0020] In a third aspect, the present invention proposes a use of a photochromic hydrogel prepared by the method described in the first aspect, wherein the photochromic hydrogel is placed under sunlight or irradiated with ultraviolet light indoors, and the hydrogel undergoes photochromic changes under light irradiation, and can restore its original color under no light conditions.
[0021] Compared with the prior art, the advantages of the present invention are:
[0022] 1) combining the hydrogel and the photochromic to form a uniform and transparent photochromic hydrogel;
[0023] 2) Use photoinitiator quantum dots to shorten the hydrogel gelation time to a few minutes, thereby suppressing the clustering of quantum dot photochromic materials (which causes the hydrogel to be opaque). BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a photo of the photochromic hydrogel prepared using titanium dioxide quantum dots as a photoinitiator in Example 1.
[0025] Figure 2 This is a photograph of the photochromic hydrogel prepared with titanium dioxide quantum dots as photoinitiators in Example 1 after being irradiated with light.
[0026] Figure 3 This is a photo of the photochromic hydrogel prepared at a stirring speed of 1000 rad / min in Example 2.
[0027] Figure 4 This is a photo of the photochromic hydrogel prepared using large-particle titanium dioxide as a photoinitiator in Example 3.
[0028] Figure 5 This is a photo of the photochromic hydrogel prepared using g-C3N4 quantum dots as initiator in Example 4.
[0029] Figure 6 These are photos of the photochromic hydrogel made of non-quantum dot K-Ca-Nb-O / MoS2 in Example 5 before (a) and after (b) illumination.
[0030] Figure 7 These are photos of the colloidal solution of TiO2 quantum dots and K-Ca-Nb-O / MoS2 quantum dots in Example 1 (1) and the mixed solution of large-particle titanium dioxide and K-Ca-Nb-O / MoS2 quantum dots in Example 3 (2). DETAILED DESCRIPTION
[0031] It should be noted that the terms such as "upper", "lower", "left", "right", "middle", etc. cited in this specification are only for the convenience of description and are not used to limit the scope of implementation. Changes or adjustments to their relative relationships should be regarded as the scope of implementation of this application without substantially changing the technical content.
[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the term "and / or" used herein includes any and all combinations of one or more of the associated listed items.
[0033] If the specific conditions are not specified in the examples, the conventional conditions or the conditions recommended by the manufacturer are followed. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially. The photochromic material K-Ca-Nb-O / MoS2 is prepared according to the method described in patent 202211310270.3.
[0034] As used herein, the term "about" is used to provide flexibility and imprecision associated with a given term, measurement or value. The degree of flexibility for a particular variable can be easily determined by one skilled in the art.
[0035] As used herein, the term "at least one of" is intended to be synonymous with "one or more of." For example, "at least one of A, B, and C" expressly includes only A, only B, only C, and combinations of each thereof.
[0036] Concentration, amount and other numerical data can be presented in range format herein.It should be understood that such range format is only used for convenience and simplicity, and should be flexibly interpreted as not only including the numerical value clearly described as range limit, but also including all single numerical values or sub-ranges contained in the range, just as each numerical value and sub-range are clearly described.For example, the numerical range of about 1 to about 4.5 should be interpreted as not only including the limit value of 1 to about 4.5 clearly described, but also including single numerals (such as 2,3,4) and sub-ranges (such as 1 to 3,2 to 4, etc.).The same principle is applicable to the scope of only narrating a numerical value, such as "less than about 4.5", which should be interpreted as including all the above-mentioned values and ranges.In addition, no matter how the breadth of the described range or feature is, this explanation should be applicable.
[0037] In order to combine the hydrogel and the photochromic to form a uniform and transparent photochromic hydrogel, the present invention uses a highly light-transmitting hydrogel as a substrate, disperses the quantum dot photochromic material therein, and can achieve photochromic under light irradiation, and can restore the original color under the condition of no light. The present invention uses initiator quantum dot light and photochromic quantum dots, both of which are less than 5nm in size, and can be evenly dispersed in water to form a transparent colloidal solution, and then uses the photoinitiator quantum dots to accelerate the rapid solidification of the precursor. At this time, the gel time is greatly shortened to a few minutes, so the photochromic quantum dot clusters can be effectively reduced, and finally a uniform and transparent photochromic hydrogel is formed. Based on the two characteristics of high light transmittance and photochromism, the present invention can be used to make handicrafts such as photochromic contact lenses (similar to traditional sunglasses), color-changing water babies, etc.
[0038] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0039] Example 1 (initiator is titanium dioxide quantum dots (<5nm), coagulation time 5min)
[0040] The synthesis method of titanium dioxide quantum dots (<5nm) is as follows: add 30mL of ethanol and a stirrer to a beaker, then place it on a magnetic stirrer and set the stirrer speed to 500rad / min; slowly add 0.5mL of 15% titanium trichloride solution and 0.5mL of prepared 6mol / L hydrochloric acid solution to the ethanol with a pipette; after stirring for two minutes, seal the beaker with a PE film, and then place the beaker in a digital constant temperature stirring water bath at 75°C for 6h; take out the centrifuge and wash with deionized water to obtain titanium dioxide quantum dots.
[0041] The photochromic material quantum dots K-Ca-Nb-O / MoS2 were prepared as follows: 50 mg of K-Ca-Nb-O / MoS2 was soaked in butylamine solution (5 mL), stirred for 7 days, and the K-Ca-Nb-O / MoS2 layered structure was expanded by substitution to obtain a single-layer K-Ca-Nb-O / MoS2 quantum dot.
[0042] Preparation of photochromic hydrogel: Disperse the initiator TiO2 quantum dots (10 mg) and the photochromic material quantum dots K-Ca-Nb-O / MoS2 (10 mg) in ultrapure water (10 mL). Place the mixture in an ultrasonic bath and mix thoroughly until a uniform colloidal solution (such as Figure 7 1 tube). Add 2 mg of cross-linking agent N,N'-bis(acryl)cystamine to the above colloidal solution, stir at a stirring rate of 200 rad / min, so that the cross-linking agent is evenly dispersed in the colloidal solution. Add 2 g of monomer acrylamide to the above solution, maintain the same stirring rate, stir until the solution is clear, and fully prepolymerize the monomer and the cross-linking agent. The above precursor solution is polymerized under a xenon lamp for 5 minutes to obtain a photochromic hydrogel. During the polymerization process, the hydrogel will photochromic under the action of ultraviolet light. In order to facilitate practical applications, the photochromic hydrogel can be dried and dehydrated for use.
[0043] How to use photochromic hydrogel: Indoors, soak the dried and dehydrated photochromic hydrogel in pure water for several hours to restore it to a gel state, and obtain a colorless and transparent photochromic hydrogel, such as Figure 1 When the hydrogel is irradiated with a xenon lamp, the hydrogel instantly undergoes photochromic changes, as shown in FIG. Figure 2 As shown, it quickly returns to colorless and transparent under no light conditions (such as Figure 1 shown).
[0044] Example 2 (stirring speed 1000 rad / min)
[0045] Disperse the initiator TiO2 quantum dots (10 mg) and the photochromic material quantum dots K-Ca-Nb-O / MoS2 (10 mg) in ultrapure water (10 mL). Place the mixture in ultrasound and mix thoroughly until a uniform colloidal solution is formed. Place the mixture in ultrasound and mix thoroughly until a uniform colloidal solution is formed. Add 2 mg of cross-linker N,N'-bis(acryl)cystamine to the above colloidal solution and stir at a stirring rate of 1000 rad / min to evenly disperse the cross-linker in the colloidal solution. Add 2 g of monomer acrylamide to the above solution, maintain the same stirring rate, stir until the solution is clear, and allow the monomer and cross-linker to fully prepolymerize. The above precursor solution is polymerized under a xenon lamp for 5 minutes to obtain a photochromic hydrogel. Due to the high stirring speed (friction), the colloidal solution flocculates, and the final photochromic hydrogel is opaque. The results are as follows. Figure 3 shown.
[0046] Example 3 (the initiator is large-particle titanium dioxide (>10 nm), and the solidification time is 45 min)
[0047] The initiator was replaced with large-particle titanium dioxide (>10 nm, commercial TiO2, Degussa Co., Ltd.), and the initiator large-particle titanium dioxide (10 mg) and the photochromic material quantum dots K-Ca-Nb-O / MoS2 (10 mg) were dispersed in ultrapure water (10 mL). The mixed solution was placed in an ultrasonic and fully mixed to obtain a turbid and opaque mixed solution (such as Figure 7 2 mg of crosslinker N,N'-bis(acryl)cystamine was added to the mixed solution, and the mixture was stirred at a stirring rate of 200 rad / min to uniformly disperse the crosslinker in the mixed solution. 2 g of monomer acrylamide was then added to the solution, and the stirring rate was maintained at the same level, and the mixture was stirred until the solution was clear, so that the monomer and the crosslinker were fully prepolymerized. The precursor solution was polymerized under a xenon lamp for 45 min to obtain a photochromic hydrogel, as shown in FIG. Figure 4 shown.
[0048] Example 4 (the initiator is quantum dot g-C3N4, the coagulation time is 2h, resulting in flocculation)
[0049] The initiator is replaced with g-C3N4 quantum dots (Wenjian Fang, Junying Liu, Lei Yu, Zhi Jiang, Wenfeng Shangguan, Novel (Na, O) co-doped g-C3N4 with simultaneously enhanced absorption and narrowed bandgap for highly efficient hydrogen evolution, Applied Catalysis B: Environmental, 209, 2017, 631-636.), and the initiator g-C3N4 quantum dots (10 mg) and the photochromic material quantum dots K-Ca-Nb-O / MoS2 (10 mg) are dispersed in ultrapure water (10 mL). The mixed solution is placed in ultrasound and fully mixed until a uniform colloidal solution is formed. 2 mg of cross-linking agent N, N'-bis (acryl) cystamine is added to the above colloidal solution, and stirred at a stirring rate of 200 rad / min to make the cross-linking agent uniformly dispersed in the colloidal solution. Then add 2g of acrylamide monomer to the above solution, maintain the same stirring rate, and stir until the solution is clear, so that the monomer and the crosslinking agent are fully prepolymerized. The above precursor solution is polymerized under a xenon lamp for 2h to obtain a photochromic hydrogel, such as Figure 5 As shown, long-term illumination can also cause flocculation of the colloidal solution, and the final hydrogel is opaque.
[0050] Example 5 (Hydrogel made using non-quantum dot K-Ca-Nb-O / MoS2)
[0051] The photochromic material was replaced with non-quantum dot K-Ca-Nb-O / MoS2, and the initiator TiO2 quantum dots (10 mg) and K-Ca-Nb-O / MoS2 (10 mg) were dispersed in ultrapure water (10 mL). The mixed solution was placed in ultrasound and mixed thoroughly. 2 mg of cross-linking agent N, N'-bis (acryl) cystamine was added to the above colloidal solution, and stirred at a stirring rate of 200 rad / min to uniformly disperse the cross-linking agent in the colloidal solution. Then 2 g of monomer acrylamide was added to the above solution, and the same stirring rate was maintained, and the solution was stirred until it was clear, so that the monomer and the cross-linking agent were fully prepolymerized. The above precursor solution was polymerized under a xenon lamp for 5 minutes to obtain a photochromic hydrogel, and the photochromic hydrogel was dried and dehydrated for use.
[0052] In the room, the dried and dehydrated photochromic hydrogel is immersed in pure water for several hours to restore it to a gel state, and a colorless photochromic hydrogel is obtained, such as Figure 6As shown in a, since K-Ca-Nb-O / MoS2 cannot be evenly dispersed in water, it will eventually cluster inside the hydrogel. When the hydrogel is irradiated with a xenon lamp, the K-Ca-Nb-O / MoS2 clusters in the hydrogel undergo photochromic changes, as shown in Figure 6 As shown in b.
Claims
1. A method for preparing a transparent photochromic hydrogel, characterized in that: The following steps are involved: (1) Dispersing TiO2 quantum dot initiator and K-Ca-Nb-O / MoS2 quantum dots in ultrapure water and mixing them thoroughly in ultrasound until a uniform solution is formed; Add a crosslinking agent to the above solution, stir at a certain stirring rate to make the crosslinking agent uniformly dispersed in the solution, then add a monomer, maintain the same stirring rate, and allow the monomer and the crosslinking agent to be fully prepolymerized; The above solution is subjected to polymerization reaction under light to obtain a transparent photochromic hydrogel.
2. The method according to claim 1, characterized in that The photochromic material K-Ca-Nb-O / MoS2 was immersed in a butylamine solution and stirred for 7 days. The K-Ca-Nb-O / MoS2 layered structure was expanded by substitution to obtain K-Ca-Nb-O / MoS2 quantum dots.
3. The method according to claim 1, characterized in that The particle sizes of TiO2 quantum dots and K-Ca-Nb-O / MoS2 quantum dots are both less than 5 nm.
4. The method according to claim 1, characterized in that The mass ratio of K-Ca-Nb-O / MoS2 quantum dots to TiO2 quantum dots is 1:
1.
5. The method according to claim 1, characterized in that The cross-linking agent is N,N'-bis(acryl)cystamine, and the mass ratio of the cross-linking agent to the initiator is 1:
5.
6. The method according to claim 1, characterized in that Stirring was performed at a stirring rate of 200 rad / min.
7. The method according to claim 1, characterized in that The monomer is acrylamide, and the mass ratio of the monomer to the cross-linking agent is 1000:
1.
8. The method according to claim 1, characterized in that The polymerization reaction time is 1 to 10 min, preferably 5 min.
9. A transparent photochromic hydrogel prepared by the method according to any one of claims 1 to 8.
10. Use of a transparent photochromic hydrogel prepared by the method according to any one of claims 1 to 8, characterized in that: The hydrogel undergoes photochromic changes when exposed to light and can restore its original color in the absence of light.
Citation Information
Patent Citations
Quantum dot-doped polyion liquid-polyacrylamide interpenetrating network hydrogel and preparation method thereof
CN105524288A
Photonic crystal hydrogel microsphere for rapidly detecting pesticides, toxins and nano-particles, and preparation method and application thereof
CN107490576A
Low-molybdenum-content photochromic material and synthesis method thereof
CN115558484A
Tungstate quantum dot-based hydrogel color-changing device with electrochromism and photochromism and preparation method of tungstate quantum dot-based hydrogel color-changing device
CN116540464A
Bimodal information storage anti-counterfeiting material and preparation method thereof
CN117304743A