Ytterbium-based coordination polymer as well as synthesis method and application thereof

Through the fluorescence sensing performance of the ytterbium-based coordination polymer {Yb(H2O)2(4-CPCA)[H(4-CPCA)]H2O}n, the problem of trace amounts of scandium ions and iron ions in the existing technology has been solved. It solves detection problems and achieves fast, convenient and low-cost detection results, and is suitable for the field of fluorescence sensing.

CN118725331APending Publication Date: 2024-10-01SICHUAN XUANYANG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410947953.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing technology cannot achieve fast, convenient and low-cost detection of trace amounts of scandium ions and iron ions in food and environmental samples. Existing methods are costly, require complex instruments and a lot of manpower, and cannot achieve on-site real-time detection.

Method used

Develop an ytterbium-based coordination polymer {Yb(H2O)2(4-CPCA)[H(4-CPCA)]H2O}n, which uses its fluorescence sensing performance to detect metal ions by coordinating with the rare earth metal Yb. It is prepared by solvothermal reaction method and has the characteristics of simplicity, convenient operation and high yield.

Benefits of technology

It achieves high-sensitivity detection of Sc3+ and Fe3+ ions, has good fluorescence properties and stability, is suitable for the field of fluorescence sensing, can quickly and accurately detect metal ions in complex environments, and reduces detection costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725331A_ABST
    Figure CN118725331A_ABST
Patent Text Reader

Abstract

The invention discloses an ytterbium-based coordination polymer as well as a synthesis method and application thereof, and the ytterbium-based coordination polymer takes Yb (III) as a central metal ion and is respectively coordinated with seven oxygen atoms to form a twisted pentagonal bipyramid structure. And the adjacent Yb (III) are bridged through 4-CPCA < 2-> to form a one-dimensional chain structure. The one-dimensional chains are further stacked through intermolecular acting force to form a three-dimensional supramolecular structure. Due to good fluorescent property and stability, the fluorescent probe can be applied to the field of fluorescent sensing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new materials, and in particular to an ytterbium-based coordination polymer and a synthesis method and application thereof. Background Art

[0002] Heavy metals are among the most dangerous pollutants in the ecosystem. Among them, metal scandium and metal iron have special properties, such as active chemical properties and good water solubility. However, excessive intake of these metals has irreversible harm to the human body, and the development of methods that can detect trace amounts of scandium and iron ions in food and environmental samples has become a current research hotspot. Nowadays, there are many methods for detecting heavy metal ions, such as spectrophotometry, inductively coupled plasma mass spectrometry, neutron activation analysis, and high performance liquid chromatography. However, these methods are costly, require large instruments and complex pretreatment, consume a lot of manpower and material resources, and cannot achieve real-time detection on site. Therefore, it is urgent to develop a highly sensitive, fast, convenient and low-cost method.

[0003] Coordination polymers are an infinite chain or network formed by the connection of inorganic metal ions or metal clusters with organic ligands. Due to its unique advantages such as high specific surface area, adjustable pore size, and active site construction, it can be widely used in gas adsorption separation, catalysis, and optoelectronic devices. And when the coordination polymer is used as a fluorescent sensor, the detection information can be expressed by the change of the light signal. It has the advantages of strong selectivity, high sensitivity, simple operation, and rapidity. In recent years, it has been increasingly used for constant analysis and detection. Among them, rare earth complexes as one of the branches have many advantages. First, its emission spectrum is narrow, which can reduce background interference and improve the accuracy of detection; secondly, rare earth coordination polymers have long-life fluorescence, which makes them have advantages in time resolution and in vivo analysis. And the fluorescence quantum yield of rare earth coordination polymers is high, which can produce relatively strong fluorescence signals; finally, under most conditions, rare earth coordination polymers have high chemical stability, which makes them applicable to complex environments. These characteristics make rare earth complexes a hot research object in recent years. Nowadays, rare earth complexes can be used as fluorescent probes to play an important role in the detection of metal ions, organic molecules and antibiotics.

[0004] Based on this, a pyridazinecarboxylic acid derivative H2 (4-CPCA) was selected as an organic ligand to coordinate with the rare earth metal Yb to obtain a Yb coordination polymer. The coordination polymer was used to perform fluorescence detection of various metal ions and to evaluate the fluorescence sensing performance of the Yb coordination polymer. Summary of the invention

[0005] This Summary is provided to introduce some concepts in a simplified form that are further described below in the Detailed Description. This Summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used as an aid in determining the scope of the claimed subject matter.

[0006] The present invention provides a coordination polymer for fluorescence sensing, and the present invention proposes the following technical solution:

[0007] Ytterbium-based coordination polymer, molecular formula: {Yb(H2O)2(4-CPCA)[H(4-CPCA)]H2O} n , wherein 4-CPCA is an organic ligand, Yb(III) is a central metal ion; n is a non-zero natural number, representing that the ytterbium-based coordination polymer is infinitely arranged alternately with the molecular formula to form a crystal; the crystal belongs to the orthorhombic system, the Pna21 space group, and the unit cell parameter is α=90°, β=90°, γ=90°,

[0008]

[0009] Preferably, 4-CPCA is 1-(4-carboxyphenyl)-4-oxo-1,4-dihydropyridazine-3-carboxylic acid, the chemical formula of which is: 12 H8N2O5.

[0010] The present invention also provides a method for synthesizing an ytterbium-based coordination polymer, which is characterized by comprising the following steps:

[0011] Step 1: adding YbCl3·6H2O and H2(4-CPCA) into H2O solvent and mixing them evenly to obtain a mixed solution, adjusting the pH value of the mixed solution to 5.3-6.4, and reacting at a constant temperature of 118-122°C for 70-74h to obtain a reaction product;

[0012] Step 2: Cool the reaction product obtained in step 1 to crystallize to obtain a crystallized product, and rinse, filter and dry the crystallized product in sequence to obtain an ytterbium-based coordination polymer.

[0013] Preferably, in step 1, one or more of the following characteristics are met:

[0014] The pH value of the mixed solution is 5.43;

[0015] The reaction temperature is 120°C;

[0016] The reaction time is 72h.

[0017] Preferably, the alkali used to adjust the mixed solution is a sodium hydroxide solution with a concentration of 0.3 mol / L.

[0018] Preferably, the H2(4-CPCA) is 1-(4-carboxyphenyl-4-oxopyridazine)-3-carboxylic acid, and the structural formula of the H2(4-CPCA) is:

[0019]

[0020] Preferably, the feed ratio of YbCl3·6H2O, H2(4-CPCA) and H2O solvent is 1 mmol:1 mmol:4 ml.

[0021] Preferably, in step 2, one or two of the following characteristics are met:

[0022] Rinse with deionized water;

[0023] The filtration is performed under reduced pressure, and the drying process is performed in an oven at a constant temperature of 50 to 70° C. for 2 to 4 hours.

[0024] Preferably, in step 2, the drying process is carried out in an oven at 60°C for 3 hours.

[0025] The present invention also provides an application of an ytterbium-based coordination polymer, characterized in that the ytterbium-based coordination polymer is applied to a fluorescent sensor.

[0026] Due to the adoption of the above technical solution, the beneficial effects achieved by the present invention are:

[0027] In the present invention, Yb(III) is used as the central metal ion, and is coordinated with seven oxygen atoms to form a distorted pentagonal bipyramidal structure. Adjacent Yb(III) are connected by 4-CPCA 2- The one-dimensional chains are further stacked through intermolecular forces to form a three-dimensional supramolecular structure. Due to its good fluorescence properties and stability, it can be used in the field of fluorescence sensing.

[0028] The invention adopts a one-pot solvent thermal reaction to prepare the ytterbium-based fluorescent sensor, and the preparation method has the advantages of simple process, convenient operation, high yield, good reproducibility, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is a single molecule image of the Yb coordination polymer;

[0030] Figure 2 This is the three-dimensional supramolecular stacking diagram of the Yb coordination polymer;

[0031] Figure 3 is the IR spectrum of the Yb coordination polymer;

[0032] Figure 4 is the XRD pattern of the Yb coordination polymer;

[0033] Figure 5 It is the solid-state fluorescence spectrum of the Yb coordination polymer;

[0034] Figure 6 The Yb coordination polymer is added with different volumes of Sc 3+ Fluorescence spectrum after solution (0.1 mmol / L);

[0035] Figure 7 It is a Yb coordination polymer in Sc 3+ Linear fitting graph of fluorescence change value in solution;

[0036] Figure 8 The Yb coordination polymer is added with different volumes of Fe 3+ Fluorescence spectrum after solution (0.1 mmol / L);

[0037] Fig. 9 It is a Yb coordination polymer in Fe 3+ Linear fitting graph of fluorescence change value in solution;

[0038] Fig.10 Yb coordination polymer to Sc 3+ and Fe 3+ Anti-interference effect of specific fluorescence changes. DETAILED DESCRIPTION

[0039] The preferred embodiments described below are for example only, and those skilled in the art may think of other obvious variations. The basic principles of the present invention defined in the following description may be applied to other embodiments, variations, improvements, equivalents, and other technical solutions that do not deviate from the spirit and scope of the present invention.

[0040] Example 1

[0041] This embodiment provides a method for preparing a Yb coordination polymer.

[0042] S1. 1 mmol of YbCl3·6H2O and 1 mmol of H2(4-CPCA) were added into a glass scintillation vial containing 4 mL of H2O solvent and mixed to obtain a mixed solution. The pH value of the mixed solution was adjusted to 5.43 with a 0.3 mol / L sodium hydroxide solution. The mixed solution was subjected to a solvothermal isothermal reaction at 120° C. for 72 h to obtain a reaction product.

[0043] Wherein, H2(4-CPCA) is 1-(4-carboxyphenyl-4-oxopyridazine)-3-carboxylic acid, and the structural formula of H2(4-CPCA) is:

[0044]

[0045] S2. Cool the reaction product obtained in S1 and crystallize it to obtain a crystallized product. Rinse the crystallized product with deionized water, and then filter it under reduced pressure to obtain transparent block crystals. Place the transparent block crystals in an oven at a temperature of 60° C. and keep the temperature constant for 3 hours to obtain a product with a yield of about 84.6%.

[0046] Figure 1 is the single molecule image of product 1, Figure 2 is the three-dimensional supramolecular diagram of product 1, according to Figure 1 and Figure 2 It can be seen that the molecular formula of the product is {Yb(H2O)2(4-CPCA)[H(4-CPCA)]H2O} n , that is, Yb coordination polymer.

[0047] from Figure 1 and Figure 2 It can be seen that the Yb coordination polymer prepared in this example is composed of Yb 3+ is the central metal ion, which is coordinated with seven oxygen atoms to form a distorted pentagonal bipyramid structure. 3+ Between 4-CPCA 2- The one-dimensional chains are further stacked through intermolecular forces to form a three-dimensional supramolecular structure.

[0048] Coordination polymer {Yb(H2O)2(4-CPCA)[H(4-CPCA)]H2O} n It crystallizes in space group Pna21 and belongs to the orthorhombic system. Its asymmetric structural unit includes 1 Yb 3+ , 3 deprotonated H2(4-CPCA) molecules and 2 H2O molecules. Central metal ion Yb 3+ It coordinates with 7 oxygen atoms to form a distorted pentagonal bipyramidal structure. Five of the oxygen atoms (O1, O3, O6, O8, O9) come from three chelate-coordinated H2 (4-CPCA), and two oxygen atoms (O11, O12) come from two monodentate-coordinated H2O molecules. 3+ Between 4-CPCA 2- The one-dimensional chains are further stacked through intermolecular forces to form a three-dimensional supramolecular structure.

[0049] Because of its good fluorescence properties and good stability, it can be used in the field of fluorescence sensing.

[0050] Example 2

[0051] This embodiment provides a method for preparing a Yb coordination polymer.

[0052] S1. Add 1 mmol of YbCl3·6H2O and 1 mmol of H2(4-CPCA) into a glass scintillation vial containing 4 mL of H2O solvent and mix well to obtain a mixed solution. Adjust the pH value of the mixed solution to 5.3 with a 0.3 mol / L sodium hydroxide solution. Perform a solvothermal isothermal reaction of the mixed solution at 118°C for 72 hours to obtain a reaction product.

[0053] S2. Cool the reaction product obtained in S1 to crystallize to obtain a crystallized product, rinse the crystallized product with deionized water, and then filter under reduced pressure to obtain transparent block crystals, place the transparent block crystals in an oven at a temperature of 50° C. and keep the temperature constant for 4 hours to obtain a product Yb coordination polymer with a yield of about 82.2%.

[0054] Example 3

[0055] This embodiment provides a method for preparing a Yb coordination polymer.

[0056] S1. 1 mmol of YbCl3·6H2O and 1 mmol of H2(4-CPCA) were added into a glass scintillation vial containing 4 mL of H2O solvent and mixed to obtain a mixed solution. The pH value of the mixed solution was adjusted to 5.91 with a 0.3 mol / L sodium hydroxide solution. The mixed solution was subjected to a solvothermal isothermal reaction at 122° C. for 70 h to obtain a reaction product.

[0057] S2. Cool the reaction product obtained in S1 to crystallize to obtain a crystallized product, rinse the crystallized product with deionized water, and then filter under reduced pressure to obtain transparent block crystals, place the transparent block crystals in an oven at a temperature of 70° C. and keep the temperature constant for 2 hours to obtain a product Yb coordination polymer with a yield of about 82.8%.

[0058] Example 4

[0059] This embodiment provides a method for preparing a Yb coordination polymer.

[0060] S1. Add 1 mmol of YbCl3·6H2O and 1 mmol of H2(4-CPCA) into a glass scintillation vial containing 4 mL of H2O solvent and mix well to obtain a mixed solution. Adjust the pH value of the mixed solution to 6.23 with a 0.3 mol / L sodium hydroxide solution. Perform a solvothermal isothermal reaction of the mixed solution at 120°C for 74 hours to obtain a reaction product.

[0061] S2. Cool the reaction product obtained in S1 and crystallize it to obtain a crystallized product. Rinse the crystallized product with deionized water, and then filter it under reduced pressure to obtain transparent block crystals. Place the transparent block crystals in an oven at a temperature of 60° C. and keep the temperature constant for 3 hours to obtain a product Yb coordination polymer with a yield of about 83.6%.

[0062] Example 5

[0063] This embodiment provides a method for preparing a Yb coordination polymer.

[0064] S1. Add 1 mmol of YbCl3·6H2O and 1 mmol of H2(4-CPCA) into a glass scintillation vial containing 4 mL of H2O solvent and mix well to obtain a mixed solution. Adjust the pH value of the mixed solution to 6.4 with a 0.3 mol / L sodium hydroxide solution. Perform a solvothermal isothermal reaction of the mixed solution at 120°C for 72 hours to obtain a reaction product.

[0065] S2. Cool the reaction product obtained in S1 and crystallize it to obtain a crystallized product. Rinse the crystallized product with deionized water, and then filter it under reduced pressure to obtain transparent block crystals. Place the transparent block crystals in an oven at a temperature of 60° C. and keep the temperature constant for 3 hours to obtain a product Yb coordination polymer with a yield of about 82.4%.

[0066] Effect Example

[0067] The final product Yb coordination polymer prepared in Example 1 was characterized.

[0068] (1) Crystal structure determination of Yb coordination polymer

[0069] A single crystal with a size of 0.42×0.4×0.35 was selected under a microscope and X-ray diffraction experiments were carried out at room temperature.

[0070] Diffraction data were collected on a Bruker-Apex II X-ray single crystal diffractometer using Mo-Kα radiation monochromatized by a graphite monochromator. Diffraction points were collected in ω-2θ scanning mode. All data were corrected by factors and empirical absorption. The crystal structure was solved by a direct method using a program. Hydrogen atoms were determined by difference Fourier synthesis and fixed in the calculated optimal position. All non-hydrogen atoms and their anisotropic thermal parameters were corrected based on the full matrix least squares method using the SHELX-97 program. The main crystallographic measurement data of the Yb coordination polymer are shown in Tables 1 and 2. The important bond length and bond angle data of the Yb coordination polymer are shown in Table 2. The crystal structure is shown in Figure 1 As shown, the three-dimensional supramolecular structure of the coordination polymer is Figure 2 shown.

[0071] Table 1

[0072]

[0073]

[0074] Table 2

[0075]

[0076] (2) Infrared (IR) spectrum characterization:

[0077] Figure 3 This is the IR spectrum of Yb coordination polymer and H2(4-CPCA). The infrared spectrum of the sample collected data from 500 to 4000 cm -1 , using KBr pellets, Figure 3 It can be seen that 1507~1598cm -1 The three peaks between are the stretching vibration peaks of the benzene ring, 3600cm -1 The peak at 1654 cm is the stretching vibration peak of the OH bond in the water molecule. -1 The carbonyl stretching vibration peak is at 1600cm -1 The strong peak at accurately indicates the presence of CN.

[0078] (3) Phase purity characterization of Yb coordination polymers:

[0079] The powder XRD characterization results of the Yb coordination polymer using a Bruker / D8Advance X-ray diffractometer showed that it had reliable phase purity, such as Figure 4 shown.

[0080] (4) Fluorescence sensing performance of Yb coordination polymers:

[0081] Since heavy metal ions are often distributed in water, it is important to study the effects of Yb coordination polymers on Sc in aqueous solution. 3+ and Fe 3+ The fluorescence sensing performance of ions is more convenient.

[0082] The photoluminescence (PL) properties of the Yb coordination polymer were studied at room temperature, and fluorescence sensing experiments were performed in aqueous suspension. Figure 5 is the solid-state fluorescence spectrum of the Yb coordination polymer. Figure 5 It can be seen that the maximum emission peak of the Yb coordination polymer is 445nm.

[0083] 2 mg of Yb coordination polymer powder sample was immersed in 4 mL of water to dissolve, and then ultrasonicated for 20 min to obtain a stable suspension. Na +, K + , Pb 2+ 、Cd 2+ 、Zn 2+ , Mn 2+ , Ba 2+ , Hg 2+ , Ca 2+ 、Co 2+ 、Ag + 、Ni 2+ , Cu 2+ 、Eu 3+ 、Sm 3+ 、Nd 3+ , Gd 3+ , Pr 3+ 、Dy 3+ ,La 3+ 、Ho 3+ 、Lu 3+ Metal cation suspension solutions were used for qualitative and anti-interference studies. 3 μL of the metal cation suspension solution prepared above with a concentration of 0.01 mol / L was added each time for quantitative titration studies, and the fluorescence spectra were recorded and collected under excitation at a wavelength of 348 nm.

[0084] The fluorescence emission intensity of the Yb coordination polymer at an excitation wavelength of 348 nm is as follows: Figure 6 As shown in the figure, the changes in luminescence intensity caused by various metal ions are compared. 3+ The addition of Fe 3+ The addition of 2-nitropropene causes fluorescence quenching effect.

[0085] In order to study the Yb coordination polymer as a fluorescent probe for detecting Sc 3+ and Fe 3+ Based on the experimental data obtained, Figure 6 The Yb coordination polymer is added with different volumes of Sc 3+ Fluorescence spectrum of solution (0.1 mmol / L), Figure 7 It is a Yb coordination polymer in Fe 3+ The linear fitting diagram of the fluorescence change value in the solution is Figure 6 and Figure 7 It can be seen that the fluorescence intensity of the Yb coordination polymer at 425 nm increases with the Sc 3+ The effect of ion concentration increases and forms a good linear relationship within a certain concentration range (R 2 =0.9961).

[0086] Figure 8 The Yb coordination polymer is added with different volumes of Fe 3+ The fluorescence spectrum of the solution (0.1 mmol / L) after Fe3+ With the increase of concentration, the fluorescence intensity of the coordination polymer gradually weakened. Fig. 9 It is a Yb coordination polymer in Fe 3+ Linear fitting diagram of fluorescence change value in solution; Stern-Volmer equation (I0-I) / I=K sv φ(I0 and I are respectively added Fe 3+ Fluorescence intensity before and after, φ is Fe 3+ Volume fraction, K sv is the quenching constant) and its linear correlation coefficient R 2 =0.9983.

[0087] The limit of detection (LOD) is also an important indicator for measuring the strength of fluorescence detection. The limit of detection (LOD) can be calculated by the formula 3σ / K sv Calculated. (where σ is the standard deviation of the fluorescence intensity of 11 blank experiments without adding any ions to the test complex) Calculated by the detection limit formula: Yb coordination polymer to Sc 3+ The detection limit is: 1.05×10 -5 mo l·L -1 , for Fe 3+ The detection limit is: 5.24×10 -6 mo l·L -1 Compared with other coordination polymer fluorescence sensors, Yb coordination polymer has a lower detection limit and a wider linear detection range.

[0088] In order to further explore whether Yb coordination polymers can selectively detect Sc 3+ Ions and Fe 3+ ions, add 0.01 mmol / L Na + , K + , Pb 2+ 、Cd 2+ 、Zn 2+ , Mn 2+ , Ba 2+ , Hg 2+ , Ca 2+ 、Co 2+ 、Ag + 、N i 2+ , Cu 2+ 、Eu 3+ 、Sm 3+ 、Nd 3+ , Gd 3+ , Pr 3+ 、Dy 3+ ,La 3+ 、Ho 3+ 、Lu3+ After ultrasonic treatment to form a stable suspension, Yb coordination polymer ions were added. Under room temperature, the fluorescence emission spectra were detected at excitation wavelengths of 346 nm and 349 nm. The results are as follows Fig.10 As shown in Figure 2, it can be seen that even in the presence of other interfering metal ions, the Yb coordination polymer can still selectively detect Sc 3+ Ions and Fe 3+ ion.

[0089] The beneficial effects of this technical solution are:

[0090] In the present invention, Yb(III) is used as the central metal ion, and is coordinated with seven oxygen atoms to form a distorted pentagonal bipyramidal structure. Adjacent Yb(III) are connected by 4-CPCA 2- The one-dimensional chains are further stacked through intermolecular forces to form a three-dimensional supramolecular structure. Due to its good fluorescence properties and stability, it can be used in the field of fluorescence sensing.

[0091] The invention adopts a one-pot solvent thermal reaction to prepare the ytterbium-based fluorescent sensor, and the preparation method has the advantages of simple process, convenient operation, high yield, good reproducibility, etc.

[0092] The coordination polymer of the present invention has strong fluorescence detection capability and strong anti-interference ability.

[0093] The embodiments described in the above paragraphs may be combined with one or more of the specifically described alternatives. In particular, the claimed embodiments may contain references to more than one other embodiment. The claimed embodiments may specify further limitations of the claimed subject matter.

[0094] Without departing from the scope of the present invention, many changes may be made to the illustrated embodiments of the present invention. Such modifications are within the scope of the present invention. The embodiments presented herein have been described in conjunction with specific embodiments, which are illustrative and not restrictive in all respects. Alternative embodiments and modifications will be apparent to those of ordinary skill in the art, but will not depart from the scope of the present invention.

[0095] From the foregoing it can be seen that the present invention is well adapted to achieve all of the above objects and goals, as well as other advantages that are obvious and inherent to the structure. It should be understood that certain features and sub-combinations are useful and can be used without reference to other features and sub-combinations. This is within the scope of the present invention.

[0096] In the foregoing detailed description, reference is made to the accompanying drawings which form a part of the specification, wherein the same reference numerals always represent the same components, and wherein embodiments that may be implemented are illustrated by way of illustration. It should be understood that other embodiments may be utilized and structural or logical changes may be made without departing from the scope of the present disclosure. Therefore, the foregoing detailed description is not restrictive, and the scope of the embodiments is defined by the appended claims and their equivalents.

[0097] Various aspects of the illustrative embodiments have been described using terms commonly used by those skilled in the art to convey the substance of their work to others skilled in the art. However, it will be apparent to those skilled in the art that alternative embodiments may be implemented using only some of the described aspects. For purposes of explanation, specific numbers, materials, and configurations are set forth in order to provide a thorough understanding of the illustrative embodiments. However, it will be apparent to those skilled in the art that alternative embodiments may be implemented without the specific details. In other cases, well-known features have been omitted or simplified in order not to obscure the illustrative embodiments.

[0098] In a manner that is most helpful for understanding the illustrative embodiments, various operations are described as multiple separate operations; however, the order of description should not be interpreted as implying that these operations are necessarily sequence-dependent. In particular, these operations do not need to be performed in the order presented. In addition, describing operations as separate operations should not be interpreted as requiring these operations to be performed independently and / or by separate entities. Describing entities and / or modules as separate modules should also not be interpreted as requiring modules to be separate and / or perform separate operations. In various embodiments, the operations, entities, data, and / or modules illustrated and / or described can be merged, decomposed into more sub-parts, and / or omitted.

[0099] The phrase "in one embodiment" or "in an embodiment" is used repeatedly. The phrase generally does not refer to the same embodiment; however, it may. The terms "comprising," "having," and "including" are synonymous unless the context dictates otherwise. The phrase "A / B" means "A or B." The phrase "A and / or B" means "(A), (B), or (A and B)." The phrase "at least one of A, B, and C" means "(A), (B), (C), (A and B), (A and C), (B and C), or (A, B, and C)."

Claims

1. Ytterbium-based coordination polymers, It is characterized in that Its molecular formula is {Yb(H 2 O) 2 (4-CPCA)[H(4-CPCA)]H 2 O} n , wherein 4-CPCA is an organic ligand; n is a non-zero natural number, representing that the ytterbium-based coordination polymer is infinitely arranged alternately to form a crystal with the molecular formula; the crystal belongs to the orthorhombic system, Pna2 1 The space group and unit cell parameters are α=90°, β=90°, γ=90°, 2. The ytterbium-based coordination polymer according to claim 1, It is characterized in that 4-CPCA is 1-(4-carboxyphenyl)-4-oxo-1,4-dihydropyridazine-3-carboxylic acid, with the chemical formula: C 12 H 8 N 2 O 5 .

3. Synthesis method of ytterbium-based coordination polymer, It is characterized in that The following steps are involved: Step 1: YbCl 3 6H 2 O and H 2 (4-CPCA) added to H 2 O solvent to obtain a mixed solution, adjusting the pH value of the mixed solution to 5.3-6.4, and reacting at a constant temperature of 118-122° C. for 70-74 hours to obtain a reaction product; Step 2: Cool the reaction product obtained in step 1 to crystallize to obtain a crystallized product, and rinse, filter and dry the crystallized product in sequence to obtain an ytterbium-based coordination polymer.

4. The method for synthesizing the ytterbium-based coordination polymer according to claim 3, It is characterized in that In step 1, one or more of the following characteristics are met: The pH value of the mixed solution is 5.43; The reaction temperature is 120°C; The reaction time is 72h.

5. The method for synthesizing the ytterbium-based coordination polymer according to claim 3, It is characterized in that The alkali used to adjust the mixed solution is a sodium hydroxide solution with a concentration of 0.3 mol / L.

6. The method for synthesizing the ytterbium-based coordination polymer according to claim 3, It is characterized in that The H 2 (4-CPCA) is 1-(4-carboxyphenyl-4-oxopyridazine)-3-carboxylic acid, wherein H 2 The structural formula of (4-CPCA) is:

7. The method for synthesizing the ytterbium-based coordination polymer according to claim 6, It is characterized in that The YbCl 3 6H 2 O, H 2 (4-CPCA) and H 2 The feed ratio of O solvent is 1mmol:1mmo l:4ml.

8. The method for synthesizing the ytterbium-based coordination polymer according to claim 3, It is characterized in that In step 2, one or both of the following characteristics must be met: Rinse with deionized water; The filtration is performed under reduced pressure, and the drying process is performed in an oven at a constant temperature of 50 to 70° C. for 2 to 4 hours.

9. The method for synthesizing the ytterbium-based coordination polymer according to claim 8, It is characterized in that In step 2, the drying process is carried out in an oven at a constant temperature of 60° C. for 3 h.

10. Application of ytterbium-based coordination polymers, It is characterized in that Application of the ytterbium-based coordination polymer in fluorescent sensing agents.

Citation Information

Cited By

  • Praseodymium (III) metal organic framework crystalline material as well as preparation method and application thereof

    CN120365581A