Three-dimensional array in-situ polymerization MPEGA / ATP composite gel electrolyte and preparation method thereof

The preparation of MPEGA/ATP composite gel electrolyte through in-situ polymerization of three-dimensional arrays solves the problems of low ionic conductivity and low mechanical properties of gel electrolytes, and achieves the formation of high ionic conductivity and stable transmission channels, which is suitable for lithium ions. Battery Preparation.

CN118725401AInactive Publication Date: 2024-10-01HARBIN UNIV OF SCI & TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410817560.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing gel electrolytes suffer from low ionic conductivity, low mechanical properties, and uneven lithium metal accumulation, which limits their application in lithium-ion batteries.

Method used

A three-dimensional array in-situ polymerization MPEGA/ATP composite gel electrolyte is prepared by uniformly dispersing polyoxyethylene PEO and attapulgite ATP in deionized water, freezing in liquid nitrogen and then freeze-drying to form a three-dimensional array porous membrane, and Initiate polymerization under UV light, add polyethylene glycol diacrylate PEGDA, poly(ethylene glycol) diacrylate MPEGA and 1-hydroxycyclohexylphenone HPCK to form a composite gel electrolyte to improve its ionic conductivity and mechanical properties. performance.

Benefits of technology

It achieves the formation of high ion conductivity and stable transmission channels, inhibits the growth of lithium dendrites, improves the mechanical properties and interface compatibility of the gel electrolyte, and the obtained film has high ion conductivity, good softness and stability sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725401A_ABST
    Figure CN118725401A_ABST
Patent Text Reader

Abstract

The invention discloses a three-dimensional array in-situ polymerization MPEGA / ATP composite gel electrolyte and a preparation method thereof, and belongs to the technical field of functional high-molecular polymer films and preparation thereof. The problems that an existing gel electrolyte is low in ionic conductivity, low in mechanical performance, uneven in lithium metal accumulation and the like are solved. The preparation method comprises the following steps: dispersing PEO and ATP in deionized water, uniformly mixing, freezing and drying in a film forming container, dispersing MPEGA, PEGDA and HPCK in LB-008, mixing and infiltrating an ATP / PEO composite array, and polymerizing to prepare the composite gel electrolyte. The composite gel electrolyte is prepared by adopting an in-situ polymerization method, so that the synthesized electrolyte has a smooth and flat surface and relatively high ionic conductivity, has the ionic conductivity of 4.6 * 10 <-4 > S cm <-1 > at room temperature, and still has the ionic conductivity of 9.2 * 10 <-5 > S cm <-1 > at-15 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a three-dimensional array in-situ polymerized MPEGA / ATP composite gel electrolyte and a preparation method thereof, belonging to the technical field of functional high molecular polymer films and preparation thereof. Background Art

[0002] Traditional diaphragm batteries use liquid electrolytes as the medium for lithium ion transmission, which have high ionic conductivity and lithium ion migration number. However, the liquid electrolytes in traditional diaphragm batteries are volatile, flammable, and explosive. The potential safety hazards brought by this unstable nature have caused certain limitations on its application in batteries, especially in high energy density batteries. Solid electrolytes are based on polymers, and their stability is greatly improved compared to liquid electrolytes, but their low ionic conductivity at room temperature also limits their application in batteries.

[0003] The state of gel electrolyte is between liquid electrolyte and solid electrolyte. It uses polymer as the matrix and adds electrolyte into it. It has the toughness and stability of polymer and higher ionic conductivity and lithium ion migration number than solid electrolyte, and has certain application prospects. However, due to the loose chain segments of gel electrolyte polymer, its mechanical properties are lower than those of solid electrolyte. At the same time, the freezing of some polymer segments will also limit the ionic conductivity of gel electrolyte at room temperature. The introduction of inorganic fillers can not only improve the mechanical strength of gel electrolyte while maintaining the toughness of polymer, but also provide higher ionic conductivity. Adding inorganic fillers is an ideal solution to improve the performance of gel electrolyte, but the uneven dispersion of inorganic fillers in polymer electrolytes will lead to uneven migration of lithium ions, inducing the growth of lithium dendrites, which will pierce the film and cause short circuits.

[0004] The inorganic array is designed to form a regular structure of inorganic fillers and a uniform ion migration path, which can significantly improve the ion conductivity and ion migration number of the polymer electrolyte. However, the inorganic array is relatively fragile. After the array is formed, the casting method is easy to disperse the array and destroy the array structure. Therefore, it is very necessary to provide a method for preparing gel electrolyte by in-situ polymerization. Summary of the invention

[0005] In order to solve the problems of low ion conductivity, low mechanical properties, uneven lithium metal accumulation and the like of existing gel electrolytes, the present invention provides a three-dimensional array in-situ polymerized MPEGA / ATP composite gel electrolyte and a preparation method thereof.

[0006] The technical solution of the present invention:

[0007] One of the purposes of the present invention is to provide a method for preparing a three-dimensional array in-situ polymerized MPEGA / ATP composite gel electrolyte, which is characterized by comprising:

[0008] S1, dispersing polyethylene oxide PEO and attapulgite ATP in deionized water, stirring magnetically until uniform, pouring into a mold, freezing with liquid nitrogen and then freeze-drying to obtain a three-dimensional array ATP / PEO porous membrane;

[0009] S2, dispersing polyethylene glycol diacrylate PEGDA, poly(ethylene glycol) diacrylate MPEGA and 1-hydroxycyclohexyl phenyl ketone HPCK in a secondary electrolyte, and subjecting the mixture to magnetic stirring to obtain a MPEGA composite gel electrolyte precursor solution;

[0010] S3, laying the three-dimensional array ATP / PEO porous membrane obtained in S1 on the mold, pouring the MPEGA composite gel electrolyte precursor solution obtained in S2, and initiating polymerization by ultraviolet irradiation to obtain a composite gel electrolyte.

[0011] It is further defined that the mass volume ratio of ATP, PEO and deionized water in S1 is (28-68) g: (17-46) g: 1.5 L.

[0012] It is further defined that the rotation speed of the magnetic stirring in S1 is 600-800 rpm and the time is more than 10 minutes.

[0013] It is further defined that the liquid nitrogen freezing time in S1 is more than 10 minutes.

[0014] It is further defined that the freeze-drying time in S1 is more than 12 hours.

[0015] It is further defined that the mass volume ratio of PEGDA, MPEGA, HPCK and secondary electrolyte in S2 is 5 g:100 g:1 g:600 mL.

[0016] It is further defined that the magnetic stirring speed in S2 is 600-800 rpm and the time is more than 10 min.

[0017] It is further defined that the mass volume ratio of the three-dimensional array ATP / PEO porous membrane and the MPEGA composite gel electrolyte precursor solution in S3 is 80g:1.5L; the ultraviolet irradiation initiation polymerization time is more than 10min, and the power is 360W.

[0018] The second object of the present invention is to provide a three-dimensional array in-situ polymerized MPEGA / ATP composite gel electrolyte prepared by the above method.

[0019] The third object of the present invention is to provide an application of the above-mentioned three-dimensional array in-situ polymerized MPEGA / ATP composite gel electrolyte, specifically for the preparation of lithium-ion batteries.

[0020] Beneficial effects:

[0021] The present invention adopts an in-situ polymerization method to prepare a composite gel electrolyte, so that the surface of the synthesized electrolyte is smooth and flat, and the interface compatibility between the electrolyte and the electrode is increased, which is suitable for high ion conductivity and stable transmission. Compared with the prior art, it has at least the following advantages:

[0022] (1) The present invention uses MPEGA as a polymer matrix, the ether oxygen bonds contained in it are conducive to the transmission of lithium ions, and further uses a three-dimensional array ATP / PEO porous membrane as an inorganic filler, and effectively enhances the ionic conductivity of the polymer electrolyte by the introduction of ATP. In addition, the secondary electrolyte is directly added during polymerization by an in-situ polymerization method, so that the electrolyte is evenly integrated into the polymer network structure, so that the obtained composite gel electrolyte has a relatively regular three-dimensional array inside, which can form a stable and uniform example transmission channel and effectively inhibit the growth of lithium dendrites. At the same time, the introduction of ATP also improves the mechanical properties of the gel electrolyte, making the prepared film soft and not easily broken.

[0023] (2) The present invention uses ultraviolet light to initiate in-situ polymerization. The polymerization process is simple and the conditions are mild. The soft composite gel electrolyte prepared has high ionic conductivity. The test results show that it has a conductivity of 4.6×10 -4 S cm -1 The ionic conductivity is still 9.2×10 at -15℃. -5 S cm -1 ionic conductivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a SEM photo of the three-dimensional array ATP / PEO porous membrane prepared in Example 1;

[0025] Figure 2 This is a SEM photo of the three-dimensional array ATP / PEO porous membrane prepared in Example 2;

[0026] Figure 3 This is an EDS photograph of the MPEGA / ATP composite film prepared in Example 1;

[0027] Figure 4 This is the impedance curve of the MPEGA / ATP composite film prepared in Example 1 at room temperature;

[0028] Figure 5The impedance curve of the MPEGA / ATP composite film prepared in Example 1 at -15°C;

[0029] Figure 6 is the LSV curve of the MPEGA / ATP composite film prepared in Example 1;

[0030] Figure 7 The cycle curve of the lithium iron phosphate battery prepared in Example 1;

[0031] Figure 8 This is an optical photograph of the MPEGA composite film prepared in Comparative Example 1;

[0032] Fig. 9 The infrared absorption comparison spectra of the MPEGA / ATP composite film prepared in Example 1 and the MPEGA composite film prepared in Comparative Example 1 are shown;

[0033] Fig.10 The X-ray diffraction comparison spectra of the MPEGA / ATP composite film prepared in Example 1 and the MPEGA composite film prepared in Comparative Example 1;

[0034] Fig.11 It is a comparison diagram of the tensile curves of the MPEGA / ATP composite films prepared in Example 1 and Example 2. DETAILED DESCRIPTION

[0035] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0036] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0037] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0038] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art, and the purity of the solid and liquid reagents used is analytically pure.

[0039] Example 1

[0040] The operation process of preparing the three-dimensional array in-situ polymerized MPEGA / ATP composite gel electrolyte in this embodiment is as follows:

[0041] Step 1: Disperse 32 g PEO and 47 g ATP in 1.5 mL deionized water, stir at high speed for 1 h at room temperature, mix well, and obtain a mixed solution.

[0042] Step 2: Pour the mixed solution into a film-forming container and freeze it with liquid nitrogen for more than 10 minutes until it is frozen solid. Then transfer it to a freeze dryer and freeze-dry it at -60°C for 12 hours to obtain a three-dimensional array ATP / PEO porous membrane.

[0043] Step 3: Disperse 100 g MPEGA, 5 g PEGDA and 1 g HPCK in 600 ml secondary electrolyte (LB-008), and stir magnetically at 600 rpm for 1 h to obtain a MPEGA composite gel electrolyte precursor solution.

[0044] Step 4: Spread 80g of the three-dimensional array ATP / PEO porous membrane obtained in step 2 flatly in a film-forming container, pour 1.5L of the MPEGA composite gel electrolyte precursor solution obtained in step 3 into the film-forming container, evenly infiltrate the three-dimensional array ATP / PEO porous membrane, and polymerize it under ultraviolet irradiation at a power of 360W for 10 minutes to obtain an in-situ polymerized array MPEGA / ATP composite gel electrolyte film, named MPEGA / ATP composite film.

[0045] Example 2

[0046] The differences between this embodiment and embodiment 1 are as follows: in step 1, PEO is 45 g and ATP is 66 g; in step 3, the mass volume ratio of the three-dimensional array ATP / PEO porous membrane and the MPEGA composite gel electrolyte precursor solution is 100 g:1.5 L; the remaining process steps and parameter settings are the same as those in embodiment 1.

[0047] Comparative Example 1

[0048] The operation process of preparing MPEGA / ATP composite gel electrolyte in this comparative example is as follows:

[0049] Step 1: Disperse 100 g MPEGA, 5 g PEGDA and 1 g HPCK in 600 ml secondary electrolyte (LB-008), and stir magnetically at 600 rpm for 1 h to obtain a MPEGA composite gel electrolyte precursor solution.

[0050] Step 2: Pour the MPEGA composite gel electrolyte precursor solution into a film-forming container and irradiate it with ultraviolet light at a power of 360W for 10 minutes to obtain an in-situ polymerized MPEGA composite gel electrolyte film, which is named MPEGA composite film.

[0051] Effect example

[0052] (1) The microstructure of the three-dimensional array ATP / PEO porous membrane prepared in Example 1 was characterized. The SEM images are shown in FIG. Figure 1 As shown, the SEM image shows that the three-dimensional array MPEGA / ATP composite film has a three-dimensional array structure.

[0053] (2) The microstructure of the ATP / PEO porous membrane prepared in Example 2 was characterized. The SEM images are shown in FIG. Figure 2 As shown, the SEM image shows that the MPEGA / ATP composite film has a porous structure.

[0054] (3) EDS element analysis was performed on the MPEGA / ATP composite film prepared in Example 1. The results are as follows Figure 3 As shown by Figure 3 It can be seen that the film is polymerized uniformly and various elements are evenly distributed in the film.

[0055] (4) The impedance curve of the MPEGA / ATP composite film prepared in Example 1 at room temperature is tested. Figure 4 As shown by Figure 4 It can be seen that the ionic conductivity of the three-dimensional array in-situ polymerized MPEGA / ATP composite film at room temperature is calculated to be about 4.6×10 -4 S cm -1 , proving that the polymer gel electrolyte has high ionic conductivity.

[0056] (5) The impedance curve of the MPEGA / ATP composite film prepared in Example 1 at -15°C was tested. Figure 5 As shown by Figure 5 It can be seen that the ionic conductivity of the three-dimensional array in-situ polymerized MPEGA / ATP composite film at -15°C is calculated to be about 1.50×10 -3 S cm -1 , proving that the polymer gel electrolyte has the ability to operate at low temperatures.

[0057] (6) The LSV curve of the MPEGA / ATP composite film prepared in Example 1 is as follows Figure 6 As shown by Figure 6It can be seen that the electrochemical window of the three-dimensional array in situ polymerized MPEGA / ATP composite gel electrolyte is about 4.5V, which has a wide electrochemical window, proving the stability of the gel electrolyte.

[0058] (7) The MPEGA / ATP composite film prepared in Example 1 was used to assemble a lithium iron phosphate button battery, and a battery cycle test was performed on it. The test results are as follows: Figure 7 As shown in the figure, the specific assembly method of lithium iron phosphate button battery is: assemble the positive battery shell, lithium iron phosphate positive electrode sheet, MPEGA / ATP composite film, lithium sheet and battery negative electrode shell in sequence, and compact them with a hydraulic press. Figure 7 It can be seen that the lithium iron phosphate button cell assembled using the MPEGA / ATP composite film prepared in Example 1 has a discharge capacity of 168.63 mAh / g in the first cycle, and retains a capacity of more than 150 mAh / g after 350 cycles, proving its cycle stability.

[0059] (8) Figure 8 This is an optical picture of the MPEGA composite film prepared in Comparative Example 1. Figure 8 It can be seen that the in-situ polymerized MPEGA composite film has good transparency, that is, the prepared composite film material is evenly distributed.

[0060] (9) Fig. 9 The infrared absorption comparison spectra of the MPEGA / ATP composite film prepared in Example 1 and the MPEGA composite film prepared in Comparative Example 1 are shown in FIG. 2, wherein 2877 cm -1 With 1801cm -1 The peak at 1045cm is the vibration peak of carbonyl group. -1 The peak at 500 cm is the vibration peak of the ether bond. -1 The peak at 4° demonstrated the incorporation of ATP.

[0061] (10) Fig.10 The X-ray diffraction comparison images of the MPEGA / ATP composite film prepared in Example 1 and the MPEGA composite film prepared in Comparative Example 1 are shown in FIG. Fig.10 It can be seen that both have no obvious crystallization peaks, proving that the polymer is basically non-crystalline, ensuring good flexibility of the polymer chain segments, which is beneficial to the transmission of lithium ions.

[0062] (11) Fig.11 : is a comparison diagram of the tensile curves of the MPEGA / ATP composite film prepared in Example 1 and the MPEGA / ATP composite film prepared in Example 2. Fig.11 It can be seen that the elastic yield stress of the film with increased ATP / PEO composite array ratio changes from the original 0.022MPa to 0.1MPa.

[0063] Although the present invention has been disclosed as above in the preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A method for preparing a three-dimensional array in-situ polymerized MPEGA / ATP composite gel electrolyte, characterized in that: include: S1, PEO and ATP are dispersed in deionized water, magnetically stirred until uniform, poured into a mold, frozen in liquid nitrogen and then freeze-dried to obtain a three-dimensional array ATP / PEO porous membrane; S2, dispersing PEGDA, MPEGA and HPCK in a secondary electrolyte, and subjecting the mixture to magnetic stirring to obtain a MPEGA composite gel electrolyte precursor solution; S3, laying the three-dimensional array ATP / PEO porous membrane obtained in S1 on the mold, pouring the MPEGA composite gel electrolyte precursor solution obtained in S2, and initiating polymerization by ultraviolet irradiation to obtain a composite gel electrolyte.

2. The preparation method according to claim 1, characterized in that: The mass volume ratio of ATP, PEO and deionized water in S1 is (28~68)g:(17~46)g:1.5L.

3. The preparation method according to claim 1, characterized in that: The speed of magnetic stirring in S1 is 600-800 rpm, and the time is more than 10 minutes.

4. The preparation method according to claim 1, characterized in that: The liquid nitrogen freezing time in S1 is more than 10 minutes.

5. The preparation method according to claim 1, characterized in that: The freeze-drying time in S1 is more than 12 h.

6. The preparation method according to claim 1, characterized in that: The mass volume ratio of PEGDA, MPEGA, HPCK and secondary electrolyte in S2 is 5g:100g:1g:600mL.

7. The preparation method according to claim 1, characterized in that: The magnetic stirring speed in S2 is 600-800 rpm, and the time is more than 10 minutes.

8. The preparation method according to claim 1, characterized in that: The mass volume ratio of the three-dimensional array ATP / PEO porous membrane and the MPEGA composite gel electrolyte precursor solution in S3 is 80g:1.5L; the ultraviolet irradiation initiation polymerization time is more than 10min, and the power is 360W.

9. A three-dimensional array in-situ polymerized MPEGA / ATP composite gel electrolyte prepared by the method according to any one of claims 1 to 8.

10. An application of the three-dimensional array in-situ polymerized MPEGA / ATP composite gel electrolyte according to claim 9, characterized in that: Used in the preparation of lithium-ion batteries.

Citation Information

Patent Citations

  • Application of multifunctional organogel to lithium ion battery

    CN110071324A

  • Preparation method of all-solid-state polymer electrolyte containing vertical array skeleton

    CN110212248A

  • Preparation method and application of inorganic clay array

    CN113471530A

  • In-situ polymerization gel polymer electrolyte with improved stability and preparation method and application thereof

    CN117613374A

  • Gel electrolyte and nonaqueous electrolytic solution battery using this

    JP2004063385A