A kind of wear-resistant matting TPE foot pad and preparation method thereof

By using modified vermiculite, modified molybdenum disulfide and modified microcrystalline kaolinite in car floor mat materials, the mechanical and matting properties of the material are improved, the poor wear resistance and environmental protection problems of existing materials are solved, and the High performance and environmentally friendly car floor mats.

CN118185327BActive Publication Date: 2024-10-01ZHEJIANG EXPO NEW MATERIALS CO LTD +2
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410459115.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-17
Publication Date
2024-10-01
Estimated Expiration
2044-04-17

Smart Images

  • Figure CN118185327B_ABST
    Figure CN118185327B_ABST
Patent Text Reader

Abstract

The invention is applicable to the technical field of automobile interior materials, and provides a wear-resistant matte TPE foot pad and a preparation method thereof. The foot pad comprises the following raw materials: SEBS, PP, naphthenic white oil, modified vermiculite, modified molybdenum disulfide, nano titanium dioxide, nano calcium carbonate, modified microcrystalline kaolinite, an antioxidant, and a plasticizer. The wear-resistant matte TPE foot pad provided by the invention is prepared by adding modified vermiculite. During the preparation of the foot pad, the modified vermiculite microparticles expand when heated. On the one hand, the internal modified vermiculite can fill the material gap, so that the density and mechanical properties of the foot pad are improved. On the other hand, the external modified vermiculite gradually emerges on the surface, so that the matte effect of the foot pad is improved. By adding the modified microcrystalline kaolinite, the surface has a stable porous structure, the bonding ability with the system is improved, and the modified vermiculite can be evenly dispersed at the nanometer level, so that the matte effect is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of automobile interior decoration materials, and in particular relates to a wear-resistant matting TPE foot pad and a preparation method thereof. Background Art

[0002] Car floor mats are an environmentally friendly car interior component. Car floor mats are interior decorations that protect the cleanliness of the inside and outside of the car and play a role in aesthetics and comfort.

[0003] Existing car floor mat materials generally use polyvinyl chloride, which has excellent properties such as good rigidity, high strength, flame retardancy, corrosion resistance, good electrical insulation, and abundant sources and low cost. However, PVC has poor wear resistance and is very environmentally unfriendly, and easily releases toxic gases. Summary of the invention

[0004] The present invention provides a wear-resistant matting TPE foot pad, aiming to solve the above-mentioned problem.

[0005] The present invention is implemented as follows: a wear-resistant matting TPE foot pad comprises the following raw materials in parts by weight: 80-100 parts of SEBS, 60-80 parts of PP, 90-120 parts of naphthenic white oil, 10-20 parts of modified vermiculite, 20-30 parts of modified molybdenum disulfide, 30-60 parts of nano titanium dioxide, 30-50 parts of nano calcium carbonate, 50-100 parts of modified microcrystalline kaolinite, 1-5 parts of antioxidant, and 2-6 parts of plasticizer;

[0006] The preparation method of the modified vermiculite is as follows:

[0007] The vermiculite is fully soaked in distilled water and then ultrasonicated in an ultrasonic cleaner for 20-30 minutes. After the ultrasonication, it is filtered and dried at 80-90°C. After the drying, it is ground and passed through a 500-mesh sieve to obtain a powder.

[0008] Add 10-20% hypochlorous acid by mass to the powder, heat in a water bath at 30-40°C and stir thoroughly for 30-50 minutes, and adjust the pH to 7;

[0009] Then add a sodium carbonate solution with a concentration of 1-2 mol / L, stir at 80-90°C for 1-2 hours, let stand for 30-50 minutes and then centrifuge;

[0010] Finally, add 0.3-0.5mmol / L octadecyltrimethylammonium chloride solution, heat to 70-90℃ and react for 1-2h, cool to room temperature and centrifuge to remove the solvent, wash with distilled water for 3 times, and dry at 80-100℃ to obtain modified vermiculite;

[0011] Impurities on the vermiculite surface are cleaned by ultrasonic cleaning, hypochlorous acid is added, heated and stirred, hypochlorous acid is decomposed, oxygen and hydrochloric acid are generated, and the vermiculite wafers are broken by soaking in hydrochloric acid, showing porous characteristics, impurities in the particle channels are dissolved, and the channels are unblocked, which is conducive to combining with other components to form a stable structure and improve mechanical properties. Sodium carbonate solution is used as a sodium source, which is conducive to the intercalation of octadecyltrimethylammonium chloride, and the intercalation modification effect is improved, so that its surface energy is increased and the dispersion is better. Furthermore, by adding modified vermiculite, during the preparation of the foot pad, the modified vermiculite microparticles are heated and expanded. On the one hand, the internal modified vermiculite can fill the material gaps, so that the density and mechanical properties of the foot pad are improved. On the other hand, the external modified vermiculite gradually emerges on the surface to improve the matting effect of the foot pad.

[0012] Preferably, the following raw materials are included in parts by weight: 85-95 parts of SEBS, 65-75 parts of PP, 100-110 parts of cyclohexane white oil, 12-18 parts of modified vermiculite, 23-27 parts of modified molybdenum disulfide, 40-50 parts of nano titanium dioxide, 35-45 parts of nano calcium carbonate, 65-85 parts of modified microcrystalline kaolinite, 2-4 parts of antioxidant, and 3-5 parts of plasticizer.

[0013] Preferably, the following raw materials are included in parts by weight: 90 parts of SEBS, 70 parts of PP, 105 parts of cyclohexane white oil, 15 parts of modified vermiculite, 25 parts of modified molybdenum disulfide, 45 parts of nano titanium dioxide, 40 parts of nano calcium carbonate, 75 parts of modified microcrystalline kaolinite, 3 parts of antioxidant, and 4 parts of plasticizer.

[0014] Preferably, the mass ratio of the powder to hypochlorous acid, sodium carbonate solution and octadecyltrimethylammonium chloride solution is 1:5-10:4-8:3-10.

[0015] Preferably, the preparation method of the modified molybdenum disulfide is as follows: placing molybdenum disulfide in ethanol, stirring at 70-80°C for 40-60 minutes, adding sodium alginate after dispersion, continuing stirring for 30-50 minutes, and then adding sodium dodecyl sulfate, stirring for 30-50 minutes, filtering after standing, washing with deionized water, and drying to obtain modified molybdenum disulfide. By modifying molybdenum disulfide, the dispersibility and interface compatibility of molybdenum disulfide are improved, and the wear resistance of the foot pad is improved.

[0016] Preferably, the mass ratio of molybdenum disulfide, ethanol, sodium alginate and sodium dodecyl sulfate is 1:5-8:1-2:0.5-0.8.

[0017] Preferably, the preparation method of the modified microcrystalline kaolinite is as follows: put the microcrystalline kaolinite into a hydrochloric acid solution with a mass concentration of 15-25%, wherein the solid-liquid ratio is 1:30 in g / mL, and stir at 600 rad / min for 1-2h in a constant temperature water bath of 50-70°C, filter the acid-washed microcrystalline kaolinite, wash it, dry it at 60°C for 30-50min, grind it to pass through a 200-mesh sieve to obtain a powder, and then add 8-10 times the weight of the powder and a concentration of 30-40% The magnesium sulfate solution is ultrasonically treated at 70-80°C for 40-60 minutes with an ultrasonic power of 1000-1200W, filtered and dried to obtain modified microcrystalline kaolinite, and the surface of the microcrystalline kaolinite is modified by hydrochloric acid corrosion to form a stable porous structure on the surface of the microcrystalline kaolinite particles, thereby improving the bonding ability of the microcrystalline kaolinite with the system. By adding the magnesium sulfate solution, the microcrystalline kaolinite can be peeled and dispersed into thinner single crystals, which can be evenly dispersed at the nanometer level and improve the matting effect.

[0018] Preferably, the antioxidant is trioctyl ester or tridecyl ester.

[0019] Preferably, the plasticizer is at least one of dioctyl phthalate, ethylene glycol, and methyl methacrylate.

[0020] The present invention also provides a method for preparing the above-mentioned wear-resistant matting TPE foot pad, comprising the following steps:

[0021] Weigh each raw material according to the ratio;

[0022] Put SEBS and PP into a high-speed mixer and stir for 8-12 minutes, then add naphthenic white oil, modified vermiculite, modified molybdenum disulfide, nano titanium dioxide, nano calcium carbonate, modified microcrystalline kaolinite, antioxidant and plasticizer and stir until the material temperature reaches 80-90℃, then release the mixture into a barrel;

[0023] The mixed material is granulated by a twin-screw extruder and then extruded into a sheet by a single-screw extruder;

[0024] The plate is placed in a blister mold and heated to 180-220° C., and the blister mold is used to obtain a foot pad.

[0025] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0026] The wear-resistant matting TPE foot pad provided by the present invention adopts TPE material, has high elasticity, high strength and high resilience of rubber, can be processed by injection molding, is environmentally friendly, non-toxic and safe, has a wide hardness range, has excellent colorability, soft touch, weather resistance, fatigue resistance and temperature resistance, and has excellent processing performance; by adding modified molybdenum disulfide, the dispersibility and interface compatibility of molybdenum disulfide are improved, and the wear resistance of the foot pad is improved; by adding modified vermiculite, during the preparation process of the foot pad, the modified vermiculite microparticles expand when heated, on the one hand, the internal modified vermiculite can fill the material gap, so that the density and mechanical properties of the foot pad are improved, and on the other hand, the external modified vermiculite gradually emerges on the surface, so that the matting effect of the foot pad is improved; by adding modified microcrystalline kaolinite, the surface has a stable porous structure, the bonding ability with the system is improved, and it can be evenly dispersed at the nanometer level, so as to improve the matting effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The present invention provides a flow chart of a method for preparing a wear-resistant matting TPE foot pad.

[0028] Figure 2 The present invention provides a flow chart of a method for preparing modified vermiculite in a wear-resistant matting TPE foot pad. DETAILED DESCRIPTION

[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by technicians in the technical field of this application; the terms used in the specification of the application herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned drawings are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, not to describe a specific order.

[0030] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0031] Example 1

[0032] The embodiment of the present invention provides a wear-resistant matte TPE foot pad, such as Figure 1 As shown, the preparation method comprises the following steps:

[0033] Weigh the following raw materials in parts by weight according to the proportion: 80 parts of SEBS, 60 parts of PP, 90 parts of naphthenic white oil, 10 parts of modified vermiculite, 20 parts of modified molybdenum disulfide, 30 parts of nano titanium dioxide, 30 parts of nano calcium carbonate, 50 parts of modified microcrystalline kaolinite, 1 part of antioxidant, and 2 parts of plasticizer;

[0034] Put SEBS and PP into a high-speed mixer and stir for 8 minutes, then add naphthenic white oil, modified vermiculite, modified molybdenum disulfide, nano titanium dioxide, nano calcium carbonate, modified microcrystalline kaolinite, antioxidant and plasticizer and stir until the material temperature reaches 80°C, then release the mixture into a barrel;

[0035] The mixed material is granulated by a twin-screw extruder and then extruded into a sheet by a single-screw extruder;

[0036] The plate is placed in a blister mold and heated to 180° C., and the blister molded plate is used to obtain a foot pad.

[0037] Wherein, the antioxidant is trioctyl phthalate, and the plasticizer is a mixture of dioctyl phthalate, ethylene glycol, and methyl methacrylate in equal proportions;

[0038] In this embodiment, Figure 2 As shown, the preparation method of the modified vermiculite is as follows:

[0039] The vermiculite was fully soaked in distilled water and then ultrasonicated in an ultrasonic cleaner for 20 minutes. After the ultrasonication, it was filtered and dried at 80°C. After the drying, it was ground and passed through a 500-mesh sieve to obtain a powder.

[0040] Add 10% hypochlorous acid to the powder, heat in a water bath at 30°C and stir thoroughly for 30 min, and adjust the pH to 7;

[0041] Then, a 1 mol / L sodium carbonate solution was added, stirred at 80°C for 1 h, allowed to stand for 30 min, and then centrifuged;

[0042] Finally, a 0.3 mmol / L octadecyltrimethylammonium chloride solution was added, the temperature was raised to 70°C for reaction for 1 hour, the solvent was removed by centrifugation after cooling to room temperature, the mixture was washed 3 times with distilled water, and dried at 80°C to obtain modified vermiculite; wherein the mass ratio of the powder to hypochlorous acid, sodium carbonate solution and octadecyltrimethylammonium chloride solution was 1:5:4:3.

[0043] Preferably, the preparation method of the modified molybdenum disulfide is as follows: placing molybdenum disulfide in ethanol, stirring at 70°C for 40 minutes, adding sodium alginate after dispersion, continuing stirring for 30 minutes, then adding sodium dodecyl sulfate, stirring for 30 minutes, filtering after standing, washing with deionized water, and drying to obtain modified molybdenum disulfide, wherein the mass ratio of the molybdenum disulfide, ethanol, sodium alginate and sodium dodecyl sulfate is 1:5:1:0.5.

[0044] In a specific implementation, the preparation method of the modified microcrystalline kaolinite is as follows: take microcrystalline kaolinite and put it into a hydrochloric acid solution with a mass concentration of 15%, wherein the solid-liquid ratio is 1:30 in g / mL, and stir it at 600 rad / min in a constant temperature water bath at 50°C for 1 hour, filter the acid-washed microcrystalline kaolinite, wash it, dry it at 60°C for 30 minutes, and grind it to pass through a 200-mesh sieve to obtain a powder, then add a magnesium sulfate solution with a concentration of 30% and a weight of 8 times the weight of the powder, ultrasonically treat it at 70°C for 40 minutes, and the ultrasonic power is 1000W. After filtering, dry it to obtain the modified microcrystalline kaolinite.

[0045] Example 2

[0046] The embodiment of the present invention provides a wear-resistant matte TPE foot pad, such as Figure 1 As shown, the preparation method thereof comprises the following steps:

[0047] Weigh the following raw materials in parts by weight according to the proportion: 85 parts of SEBS, 65 parts of PP, 100 parts of naphthenic white oil, 12 parts of modified vermiculite, 23 parts of modified molybdenum disulfide, 40 parts of nano titanium dioxide, 35 parts of nano calcium carbonate, 65 parts of modified microcrystalline kaolinite, 2 parts of antioxidant, and 3 parts of plasticizer;

[0048] Put SEBS and PP into a high-speed mixer and stir for 8 minutes, then add naphthenic white oil, modified vermiculite, modified molybdenum disulfide, nano titanium dioxide, nano calcium carbonate, modified microcrystalline kaolinite, antioxidant and plasticizer and stir until the material temperature reaches 80°C, then release the mixture into a barrel;

[0049] The mixed material is granulated by a twin-screw extruder and then extruded into a sheet by a single-screw extruder;

[0050] The plate is placed in a blister mold and heated to 180° C., and the blister molded plate is used to obtain a foot pad.

[0051] Wherein, the antioxidant is tridecyl ester, and the plasticizer is a mixture of dioctyl phthalate, ethylene glycol, and methyl methacrylate in equal proportions;

[0052] In this embodiment, Figure 2 As shown, the preparation method of the modified vermiculite is as follows:

[0053] The vermiculite was fully soaked in distilled water and then ultrasonicated in an ultrasonic cleaner for 20 minutes. After the ultrasonication, it was filtered and dried at 80°C. After the drying, it was ground and passed through a 500-mesh sieve to obtain a powder.

[0054] Add 10% hypochlorous acid to the powder, heat in a water bath at 30°C and stir thoroughly for 30 min, and adjust the pH to 7;

[0055] Then, a 1 mol / L sodium carbonate solution was added, stirred at 80°C for 1 h, allowed to stand for 30 min, and then centrifuged;

[0056] Finally, a 0.3 mmol / L octadecyltrimethylammonium chloride solution was added, the temperature was raised to 70°C for reaction for 1 hour, the solvent was removed by centrifugation after cooling to room temperature, the mixture was washed 3 times with distilled water, and dried at 80°C to obtain modified vermiculite; wherein the mass ratio of the powder to hypochlorous acid, sodium carbonate solution and octadecyltrimethylammonium chloride solution was 1:5:4:3.

[0057] Preferably, the preparation method of the modified molybdenum disulfide is as follows: placing molybdenum disulfide in ethanol, stirring at 70°C for 40 minutes, adding sodium alginate after dispersion, continuing stirring for 30 minutes, then adding sodium dodecyl sulfate, stirring for 30 minutes, filtering after standing, washing with deionized water, and drying to obtain modified molybdenum disulfide, wherein the mass ratio of the molybdenum disulfide, ethanol, sodium alginate and sodium dodecyl sulfate is 1:5:1:0.5.

[0058] In a specific implementation, the preparation method of the modified microcrystalline kaolinite is as follows: take microcrystalline kaolinite and put it into a hydrochloric acid solution with a mass concentration of 15%, wherein the solid-liquid ratio is 1:30 in g / mL, and stir it at 600 rad / min in a constant temperature water bath at 50°C for 1 hour, filter the acid-washed microcrystalline kaolinite, wash it, dry it at 60°C for 30 minutes, and grind it to pass through a 200-mesh sieve to obtain a powder, then add a magnesium sulfate solution with a concentration of 30% and a weight of 8 times the weight of the powder, ultrasonically treat it at 70°C for 40 minutes, and the ultrasonic power is 1000W. After filtering, dry it to obtain the modified microcrystalline kaolinite.

[0059] Example 3

[0060] The embodiment of the present invention provides a wear-resistant matte TPE foot pad, such as Figure 1 As shown, the preparation method comprises the following steps:

[0061] Weigh the following raw materials in parts by weight according to the proportion: 90 parts of SEBS, 70 parts of PP, 105 parts of naphthenic white oil, 15 parts of modified vermiculite, 25 parts of modified molybdenum disulfide, 45 parts of nano titanium dioxide, 40 parts of nano calcium carbonate, 75 parts of modified microcrystalline kaolinite, 3 parts of antioxidant, and 4 parts of plasticizer;

[0062] Put SEBS and PP into a high-speed mixer and stir for 10 minutes, then add naphthenic white oil, modified vermiculite, modified molybdenum disulfide, nano titanium dioxide, nano calcium carbonate, modified microcrystalline kaolinite, antioxidant and plasticizer and stir until the material temperature reaches 85°C, then release the mixture into a barrel;

[0063] The mixed material is granulated by a twin-screw extruder and then extruded into a sheet by a single-screw extruder;

[0064] The plate is placed in a blister mold and heated to 200° C., and blister molded to obtain a foot pad.

[0065] Wherein, the antioxidant is trioctyl phthalate, and the plasticizer is a mixture of dioctyl phthalate, ethylene glycol, and methyl methacrylate in equal proportions;

[0066] In this embodiment, Figure 2 As shown, the preparation method of the modified vermiculite is as follows:

[0067] The vermiculite was fully soaked in distilled water and then ultrasonicated in an ultrasonic cleaner for 25 minutes. After the ultrasonication, it was filtered and dried at 85°C. After the drying, it was ground and passed through a 500-mesh sieve to obtain a powder.

[0068] Add 15% hypochlorous acid to the powder, heat in a water bath at 35°C and stir thoroughly for 40 min, and adjust the pH to 7;

[0069] Then, a sodium carbonate solution with a concentration of 1.5 mol / L was added, stirred at 85°C for 1.5 h, allowed to stand for 40 min, and then centrifuged;

[0070] Finally, a 0.4 mmol / L octadecyltrimethylammonium chloride solution was added, the temperature was raised to 80°C, the reaction was performed for 1.5 hours, the solvent was removed by centrifugation after cooling to room temperature, the mixture was washed 3 times with distilled water, and the mixture was dried at 90°C to obtain modified vermiculite; wherein the mass ratio of the powder to the hypochlorous acid, the sodium carbonate solution and the octadecyltrimethylammonium chloride solution was 1:7.5:6:6.5.

[0071] Preferably, the preparation method of the modified molybdenum disulfide is as follows: placing molybdenum disulfide in ethanol, stirring at 75°C for 50 minutes, adding sodium alginate after dispersion, continuing stirring for 40 minutes, then adding sodium dodecyl sulfate, stirring for 40 minutes, filtering after standing, washing with deionized water, and drying to obtain modified molybdenum disulfide, wherein the mass ratio of the molybdenum disulfide, ethanol, sodium alginate and sodium dodecyl sulfate is 1:6.5:1.5:0.65.

[0072] In a specific implementation, the preparation method of the modified microcrystalline kaolinite is as follows: take microcrystalline kaolinite and put it into a 20% hydrochloric acid solution with a solid-liquid ratio of 1:30 in g / mL, stir it at 600 rad / min in a 60°C constant temperature water bath for 1.5 hours, filter the acid-washed microcrystalline kaolinite, wash it, dry it at 60°C for 40 minutes, and grind it to pass through a 200-mesh sieve to obtain a powder, then add a magnesium sulfate solution with a concentration of 35% and a weight of 9 times the weight of the powder, ultrasonically treat it at 75°C for 50 minutes, and the ultrasonic power is 1100 W. After filtering, dry it to obtain the modified microcrystalline kaolinite.

[0073] Example 4

[0074] The embodiment of the present invention provides a wear-resistant matte TPE foot pad, such as Figure 1 As shown, the preparation method thereof comprises the following steps:

[0075] Weigh the following raw materials in parts by weight according to the proportion: 95 parts of SEBS, 75 parts of PP, 110 parts of naphthenic white oil, 18 parts of modified vermiculite, 27 parts of modified molybdenum disulfide, 50 parts of nano titanium dioxide, 45 parts of nano calcium carbonate, 85 parts of modified microcrystalline kaolinite, 4 parts of antioxidant, and 5 parts of plasticizer;

[0076] Put SEBS and PP into a high-speed mixer and stir for 12 minutes, then add naphthenic white oil, modified vermiculite, modified molybdenum disulfide, nano titanium dioxide, nano calcium carbonate, modified microcrystalline kaolinite, antioxidant and plasticizer and stir until the material temperature reaches 90°C, then release the mixture into a barrel;

[0077] The mixed material is granulated by a twin-screw extruder and then extruded into a sheet by a single-screw extruder;

[0078] The plate is placed in a blister mold and heated to 220° C., and the blister mold is used to obtain a foot pad.

[0079] Wherein, the antioxidant is tridecyl ester, and the plasticizer is a mixture of dioctyl phthalate, ethylene glycol, and methyl methacrylate in equal proportions;

[0080] In this embodiment, Figure 2 As shown, the preparation method of the modified vermiculite is as follows:

[0081] The vermiculite was fully soaked in distilled water and then ultrasonicated in an ultrasonic cleaner for 30 minutes. After the ultrasonication, it was filtered and dried at 90°C. After the drying, it was ground and passed through a 500-mesh sieve to obtain a powder.

[0082] Add 20% hypochlorous acid to the powder, heat in a water bath at 40°C and stir thoroughly for 50 min, and adjust the pH to 7;

[0083] Then, a 2 mol / L sodium carbonate solution was added, stirred at 90°C for 2 h, allowed to stand for 50 min, and then centrifuged;

[0084] Finally, a 0.5 mmol / L octadecyltrimethylammonium chloride solution was added, the temperature was raised to 90°C for reaction for 2 hours, the solvent was removed by centrifugation after cooling to room temperature, the mixture was washed 3 times with distilled water, and the mixture was dried at 100°C to obtain modified vermiculite; wherein the mass ratio of the powder to the hypochlorous acid, the sodium carbonate solution and the octadecyltrimethylammonium chloride solution was 1:10:8:10.

[0085] Preferably, the preparation method of the modified molybdenum disulfide is as follows: placing molybdenum disulfide in ethanol, stirring at 80°C for 60 minutes, adding sodium alginate after dispersion, continuing stirring for 50 minutes, then adding sodium dodecyl sulfate, stirring for 50 minutes, filtering after standing, washing with deionized water, and drying to obtain modified molybdenum disulfide, wherein the mass ratio of the molybdenum disulfide, ethanol, sodium alginate and sodium dodecyl sulfate is 1:8:2:0.8.

[0086] In a specific implementation, the preparation method of the modified microcrystalline kaolinite is as follows: take microcrystalline kaolinite and put it into a 25% mass concentration hydrochloric acid solution, wherein the solid-liquid ratio is 1:30 in g / mL, and stir it at 600 rad / min for 2 hours in a 70°C constant temperature water bath, filter the acid-washed microcrystalline kaolinite, wash it, dry it at 60°C for 50 minutes, and grind it to pass through a 200-mesh sieve to obtain a powder, then add a magnesium sulfate solution with a concentration of 40% and a weight that is 10 times the weight of the powder, ultrasonically treat it at 80°C for 60 minutes, and the ultrasonic power is 1200W. After filtering, dry it to obtain the modified microcrystalline kaolinite.

[0087] Example 5

[0088] The embodiment of the present invention provides a wear-resistant matte TPE foot pad, such as Figure 1 As shown, the preparation method thereof comprises the following steps:

[0089] Weigh the following raw materials in parts by weight according to the proportion: 100 parts of SEBS, 80 parts of PP, 120 parts of naphthenic white oil, 20 parts of modified vermiculite, 30 parts of modified molybdenum disulfide, 60 parts of nano titanium dioxide, 50 parts of nano calcium carbonate, 100 parts of modified microcrystalline kaolinite, 5 parts of antioxidant, and 6 parts of plasticizer;

[0090] Put SEBS and PP into a high-speed mixer and stir for 12 minutes, then add naphthenic white oil, modified vermiculite, modified molybdenum disulfide, nano titanium dioxide, nano calcium carbonate, modified microcrystalline kaolinite, antioxidant and plasticizer and stir until the material temperature reaches 90°C, then release the mixture into a barrel;

[0091] The mixed material is granulated by a twin-screw extruder and then extruded into a sheet by a single-screw extruder;

[0092] The plate is placed in a blister mold and heated to 220° C., and the blister mold is used to obtain a foot pad.

[0093] Wherein, the antioxidant is tridecyl ester, and the plasticizer is a mixture of dioctyl phthalate, ethylene glycol, and methyl methacrylate in equal proportions;

[0094] In this embodiment, Figure 2 As shown, the preparation method of the modified vermiculite is as follows:

[0095] The vermiculite was fully soaked in distilled water and then ultrasonicated in an ultrasonic cleaner for 30 minutes. After the ultrasonication, it was filtered and dried at 90°C. After the drying, it was ground and passed through a 500-mesh sieve to obtain a powder.

[0096] Add 20% hypochlorous acid to the powder, heat in a water bath at 40°C and stir thoroughly for 50 min, and adjust the pH to 7;

[0097] Then, a 2 mol / L sodium carbonate solution was added, stirred at 90°C for 2 h, allowed to stand for 50 min, and then centrifuged;

[0098] Finally, a 0.5 mmol / L octadecyltrimethylammonium chloride solution was added, the temperature was raised to 90°C for reaction for 2 hours, the solvent was removed by centrifugation after cooling to room temperature, the mixture was washed 3 times with distilled water, and the mixture was dried at 100°C to obtain modified vermiculite; wherein the mass ratio of the powder to the hypochlorous acid, the sodium carbonate solution and the octadecyltrimethylammonium chloride solution was 1:10:8:10.

[0099] Preferably, the preparation method of the modified molybdenum disulfide is as follows: placing molybdenum disulfide in ethanol, stirring at 80°C for 60 minutes, adding sodium alginate after dispersion, continuing stirring for 50 minutes, then adding sodium dodecyl sulfate, stirring for 50 minutes, filtering after standing, washing with deionized water, and drying to obtain modified molybdenum disulfide, wherein the mass ratio of the molybdenum disulfide, ethanol, sodium alginate and sodium dodecyl sulfate is 1:8:2:0.8.

[0100] In a specific implementation, the preparation method of the modified microcrystalline kaolinite is as follows: take microcrystalline kaolinite and put it into a 25% mass concentration hydrochloric acid solution, wherein the solid-liquid ratio is 1:30 in g / mL, and stir it at 600 rad / min for 2 hours in a 70°C constant temperature water bath, filter the acid-washed microcrystalline kaolinite, wash it, dry it at 60°C for 50 minutes, and grind it to pass through a 200-mesh sieve to obtain a powder, then add a magnesium sulfate solution with a concentration of 40% and a weight that is 10 times the weight of the powder, ultrasonically treat it at 80°C for 60 minutes, and the ultrasonic power is 1200W. After filtering, dry it to obtain the modified microcrystalline kaolinite.

[0101] Comparative Example 1: Compared with Example 3, the modified molybdenum disulfide is replaced by ordinary molybdenum disulfide.

[0102] Comparative Example 2: Compared with Example 3, the modified molybdenum disulfide is not contained.

[0103] Comparative Example 3: Compared with Example 3, the modified vermiculite was replaced by ordinary vermiculite.

[0104] Comparative Example 4: Compared with Example 3, the modified vermiculite is not contained.

[0105] Comparative Example 5: Compared with Example 3, the modified microcrystalline kaolinite is replaced by ordinary microcrystalline kaolinite.

[0106] Comparative Example 6: Compared with Example 3, the modified microcrystalline kaolinite is not contained.

[0107] Comparative Example 7: Compared with Example 3, the vermiculite was not treated with hypochlorous acid.

[0108] Comparative Example 8: Compared with Example 3, the vermiculite was not treated with sodium carbonate solution.

[0109] Comparative Example 9: Compared with Example 3, the modified vermiculite was replaced by ordinary vermiculite and the modified microcrystalline kaolinite was replaced by ordinary microcrystalline kaolinite.

[0110] test

[0111] 1. Wear resistance: The foot pads prepared in Examples 1-5 and Comparative Examples 1-2 were fixed on a wear tester under the same conditions for scraping and rubbing. After rubbing 200 times, the wear rate was tested. The results are shown in Table 1 below:

[0112] Group Wear rate (%) Example 1 4.8 Example 2 4.6 Example 3 4.3 Example 4 4.7 Example 5 4.8 Comparative Example 1 15.6 Comparative Example 2 24.8

[0113] It can be seen from the above results that the foot pad prepared by the present invention has good wear resistance, and the wear resistance can be greatly improved by adding modified molybdenum disulfide.

[0114] 2. Glossiness: The glossiness test was performed on the foot pads prepared in Examples 1-5 and Comparative Examples 3-9.

[0115] Gloss standard: Gloss industry standards include GB / T8807, ASTM D523, ASTM D2457, etc. According to the standard requirements, for samples with unknown gloss, we generally start measuring at 60°. If the result is between 10-70GU, the coating can be called semi-gloss, and it is best to use a 60° angle to measure. If the result is less than 10GU, the product is called low gloss and should be measured at 85°. If the result is higher than 70GU, the product is high gloss and is best measured at 20°.

[0116] The gloss test results are shown in Table 2:

[0117] Group Glossiness (GU) Example 1 4.2 Example 2 3.9 Example 3 3.8 Example 4 3.9 Example 5 4.1 Comparative Example 3 30.8 Comparative Example 4 38.5 Comparative Example 5 25.2 Comparative Example 6 32.8 Comparative Example 7 8.4 Comparative Example 8 9.6 Comparative Example 9 45.5

[0118] It can be seen from the above results that the doormat prepared by the present invention has low gloss and excellent matting performance. By adding modified vermiculite and modified microcrystalline kaolinite, the two have a synergistic effect and can greatly improve the matting performance.

[0119] It should be noted that, for the above embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the described order of actions, because according to the present invention, some steps may be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and modules involved are not necessarily required by the present invention.

[0120] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the scope of protection of the invention. Obviously, the described embodiments are only some embodiments of the present invention, rather than all embodiments. Based on these embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in this field can still combine, add, delete or make other adjustments to the features in the various embodiments of the present invention according to the circumstances without conflict, without making creative work, so as to obtain different other technical solutions that do not deviate from the concept of the present invention in essence, and these technical solutions also belong to the scope of protection of the present invention.

Claims

1. A wear-resistant matting TPE foot pad, characterized in that: include: The invention comprises the following raw materials in parts by weight: 80-100 parts of SEBS, 60-80 parts of PP, 90-120 parts of naphthenic white oil, 10-20 parts of modified vermiculite, 20-30 parts of modified molybdenum disulfide, 30-60 parts of nano titanium dioxide, 30-50 parts of nano calcium carbonate, 50-100 parts of modified microcrystalline kaolinite, 1-5 parts of antioxidant, and 2-6 parts of plasticizer; The preparation method of the modified vermiculite is as follows: The vermiculite is fully soaked in distilled water and then ultrasonicated in an ultrasonic cleaner for 20-30 minutes. After the ultrasonication, it is filtered and dried at 80-90°C. After the drying, it is ground and passed through a 500-mesh sieve to obtain a powder. Add 10-20% hypochlorous acid by mass to the powder, heat in a water bath at 30-40°C and stir thoroughly for 30-50 minutes, and adjust the pH to 7; Then add a sodium carbonate solution with a concentration of 1-2 mol / L, stir at 80-90°C for 1-2 hours, let stand for 30-50 minutes and then centrifuge; Finally, add 0.3-0.5mmol / L octadecyltrimethylammonium chloride solution, heat to 70-90°C for reaction for 1-2h, cool to room temperature and centrifuge to remove the solvent, wash with distilled water for 3 times, and dry at 80-100°C to obtain modified vermiculite, wherein the mass ratio of the powder to hypochlorous acid, sodium carbonate solution and octadecyltrimethylammonium chloride solution is 1:5-10:4-8:3-10; The preparation method of the modified molybdenum disulfide is as follows: placing molybdenum disulfide in ethanol, stirring at 70-80° C. for 40-60 minutes, adding sodium alginate after dispersion, continuing stirring for 30-50 minutes, then adding sodium dodecyl sulfate, stirring for 30-50 minutes, filtering after standing, washing with deionized water, and drying to obtain the modified molybdenum disulfide, wherein the mass ratio of the molybdenum disulfide, ethanol, sodium alginate and sodium dodecyl sulfate is 1:5-8:1-2:0.5-0.8; The preparation method of the modified microcrystalline kaolinite is as follows: taking microcrystalline kaolinite and putting it into a hydrochloric acid solution with a mass concentration of 15-25%, wherein the solid-liquid ratio is 1:30 in g / mL, stirring at 600 rad / min for 1-2 hours in a constant temperature water bath of 50-70°C, filtering and washing the acid-washed microcrystalline kaolinite, drying it at 60°C for 30-50 minutes, and grinding it to pass through a 200-mesh sieve to obtain a powder, then adding a magnesium sulfate solution with a concentration of 30-40% and a weight of 8-10 times the weight of the powder, ultrasonically treating it at 70-80°C for 40-60 minutes with an ultrasonic power of 1000-1200W, filtering and drying to obtain the modified microcrystalline kaolinite.

2. The wear-resistant matting TPE foot pad according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 85-95 parts of SEBS, 65-75 parts of PP, 100-110 parts of cycloalkane white oil, 12-18 parts of modified vermiculite, 23-27 parts of modified molybdenum disulfide, 40-50 parts of nano titanium dioxide, 35-45 parts of nano calcium carbonate, 65-85 parts of modified microcrystalline kaolinite, 2-4 parts of antioxidant and 3-5 parts of plasticizer.

3. The wear-resistant matting TPE foot pad according to claim 2, characterized in that: The invention comprises the following raw materials in parts by weight: 90 parts of SEBS, 70 parts of PP, 105 parts of cyclohexane white oil, 15 parts of modified vermiculite, 25 parts of modified molybdenum disulfide, 45 parts of nano titanium dioxide, 40 parts of nano calcium carbonate, 75 parts of modified microcrystalline kaolinite, 3 parts of antioxidant and 4 parts of plasticizer.

4. The method for preparing the wear-resistant matting TPE foot pad according to any one of claims 1 to 3, characterized in that: The steps include: Weigh each raw material according to the ratio; Put SEBS and PP into a high-speed mixer and stir for 8-12 minutes, then add naphthenic white oil, modified vermiculite, modified molybdenum disulfide, nano titanium dioxide, nano calcium carbonate, modified microcrystalline kaolinite, antioxidant and plasticizer and stir until the material temperature reaches 80-90℃, then release the mixture into a barrel; The mixed material is granulated by a twin-screw extruder and then extruded into a sheet by a single-screw extruder; The plate is placed in a blister mold and heated to 180-220° C., and the blister mold is used to obtain a foot pad.

Citation Information

Cited By

  • Colorful TPO interior foot pad skin and preparation method thereof

    CN120039002A

  • A colorful TPO interior floor mat skin and its preparation method

    CN120039002B