High-wear-resistance conveyor belt cover rubber and preparation method thereof
By using natural rubber, styrene-butadiene rubber, isoprene rubber and other materials in the conveyor belt covering rubber, and adding fillers such as carbon fiber and carbon black, the problem of insufficient wear resistance of the traditional conveyor belt covering rubber is solved, and the transportation efficiency is significantly improved. Belt wear resistance and service life.
Patent Information
- Application Number
- CN202410934169.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
AI Technical Summary
The wear resistance of traditional conveyor belt covering rubber is low, resulting in insufficient service life of the conveyor belt and its inability to effectively cope with the impact and friction in different usage environments.
Using materials such as natural rubber, styrene-butadiene rubber, isoprene rubber, liquid silicone rubber, carbon fiber, carbon black, lignin, starch, alumina and talc, through the rubber matrix processing and vulcanization process, a highly wear-resistant conveyor is prepared With covering glue to improve its wear resistance and crack resistance.
It significantly improves the wear resistance and mechanical properties of the conveyor belt covering glue, extends the service life of the conveyor belt, and brings economic benefits.
Smart Images

Figure CN118725423A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of conveyor belts, and in particular to a highly wear-resistant conveyor belt covering rubber and a preparation method thereof. Background Art
[0002] Conveyor belts, also known as conveyor belts, are composite products of rubber, fiber, metal, or plastic and fabric used in conveyor belts to carry and transport materials. Conveyor belts are widely used in cement, coking, metallurgy, chemical, steel and other industries where the conveying distance is short and the conveying volume is small. The conveyor belt cover rubber is covered on the surface of the conveyor belt and is in direct contact with the material, that is, the conveyor belt cover rubber is the working surface of the conveyor belt.
[0003] During the operation of the conveyor belt, it will directly bear the impact and friction of the material, and will face different usage conditions due to different usage environments. In order to avoid various factors affecting the service life of the conveyor belt during the operation, it is necessary to improve the wear resistance of the conveyor belt surface covering rubber and increase the service life of the conveyor belt. However, for traditional conveyor belt covering rubber, its composition is simple and its wear resistance is relatively low. Therefore, the present invention proposes a high wear-resistant conveyor belt covering rubber and a preparation method to solve the problems existing in the prior art. Summary of the invention
[0004] In view of the above problems, the purpose of the present invention is to propose a highly wear-resistant conveyor belt covering rubber and a preparation method thereof, which have the advantages of improving the wear resistance of the conveyor belt covering rubber and can solve the problems existing in the prior art.
[0005] To achieve the purpose of the present invention, the present invention is achieved through the following technical scheme: a highly wear-resistant conveyor belt covering rubber and a preparation method, comprising the following raw materials in parts by weight: 40 to 55 parts of natural rubber, 40 to 55 parts of styrene-butadiene rubber, 10 to 20 parts of isoprene rubber, 5 to 10 parts of recycled rubber powder, 5 to 18 parts of liquid silicone rubber, 2 to 3 parts of carbon fiber, 30 to 40 parts of carbon black, 8 to 12 parts of wear resistance agent, 3 to 5 parts of silane coupling agent, 3 to 5 parts of plasticizer, 6 to 8 parts of lignin, 6 to 8 parts of starch, 1 to 2 parts of accelerator, 4 to 6 parts of aluminum oxide, 2 to 4 parts of stearic acid, 2 to 4 parts of antioxidant, 2 to 3 parts of vulcanizer, 1 to 2 parts of anti-scorch agent, 6 to 10 parts of talc, 1 to 2 parts of tackifier, and 3 to 5 parts of zinc oxide.
[0006] The further improvement is that it includes the following raw materials in parts by weight: 55 parts of natural rubber, 40 parts of styrene-butadiene rubber, 20 parts of isoprene rubber, 5 parts of recycled rubber powder, 5 parts of liquid silicone rubber, 2 parts of carbon fiber, 30 parts of carbon black, 8 parts of wear resistance agent, 3 parts of silane coupling agent, 3 parts of plasticizer, 6 parts of lignin, 8 parts of starch, 1 part of accelerator, 4 parts of aluminum oxide, 2 parts of stearic acid, 2 parts of antioxidant, 2 parts of vulcanizer, 1 part of anti-scorch agent, 6 parts of talcum powder, 1 part of tackifier, and 3 parts of zinc oxide.
[0007] The further improvement is that it includes the following raw materials in parts by weight: 40 parts of natural rubber, 55 parts of styrene-butadiene rubber, 10 parts of isoprene rubber, 10 parts of recycled rubber powder, 18 parts of liquid silicone rubber, 3 parts of carbon fiber, 40 parts of carbon black, 12 parts of wear resistance agent, 5 parts of silane coupling agent, 5 parts of plasticizer, 8 parts of lignin, 6 parts of starch, 2 parts of accelerator, 6 parts of aluminum oxide, 4 parts of stearic acid, 4 parts of antioxidant, 3 parts of vulcanizer, 2 parts of anti-scorch agent, 10 parts of talcum powder, 2 parts of tackifier and 5 parts of zinc oxide.
[0008] A further improvement is that the plasticizer is one of softened heavy oil and pine tar.
[0009] A further improvement is that the carbon black is a composition of carbon black N220 and carbon black N330, and the weight ratio of the carbon black N220 to the carbon black N330 is 2:1.
[0010] A further improvement is that the anti-wear agent is silicone oil.
[0011] A further improvement is that the antioxidant is one of antioxidant 4010NA, antioxidant RD and antioxidant BLE.
[0012] A further improvement is that the vulcanizing agent is sulfur, the tackifier is polyisobutylene, the anti-scorch agent is anti-scorch agent CTP, and the silane coupling agent is coupling agent KH560.
[0013] A method for preparing a highly wear-resistant conveyor belt covering rubber comprises the following steps:
[0014] Step 1: Material preparation
[0015] Accurately weigh all raw materials, including natural rubber, styrene-butadiene rubber, isoprene rubber, recycled rubber powder, liquid silicone rubber, carbon fiber, carbon black, wear-resistant agent, silane coupling agent, plasticizer, lignin, starch, accelerator, aluminum oxide, stearic acid, antioxidant, vulcanizer, anti-scorch agent, talcum powder, tackifier, zinc oxide;
[0016] Step 2: Primary rubber matrix processing
[0017] Add natural rubber, styrene-butadiene rubber, isoprene rubber, recycled rubber powder and liquid silicone rubber into an internal mixer, mix for 5 to 10 minutes, the temperature of the internal mixer is 65 to 80° C., and a rubber matrix is obtained after internal mixing, wherein the speed of the internal mixer is 40 r / min;
[0018] Step 3: Secondary rubber matrix processing
[0019] The carbon fiber, carbon black, lignin, starch, talcum powder and silane coupling agent are sequentially added into an internal mixer and internally mixed with the rubber matrix. The internal mixing time is 8 to 10 minutes and the internal mixing temperature is 75 to 90° C. After internal mixing, a mixed colloid is obtained, wherein the speed of the internal mixer remains unchanged;
[0020] Step 4: Vulcanization of mixed colloid
[0021] The remaining raw materials are then added to the internal mixer, the temperature is kept constant, the internal mixing time is 10 to 12 minutes, the internal mixer speed is 30 r / min, a mixed rubber mixture is obtained, and then the rubber mixture is placed in a vulcanizer for vulcanization;
[0022] Step 5: Conveyor belt cover rubber molding
[0023] After step 4 vulcanization, the material is taken out and cooled, and after cooling, it is added into a calender to form the covering rubber.
[0024] A further improvement is that in step three, the interval between each addition of material is 30 seconds.
[0025] The beneficial effects of the present invention are as follows: the high wear-resistant conveyor belt covering rubber provided by the present invention, on the basis of natural rubber and styrene-butadiene rubber, adds isoprene rubber and liquid silicone rubber as the main material part of the rubber, improves the basic formula of the conveyor belt covering rubber, improves the density and resilience of the material, thereby enhancing the wear resistance and crack resistance, and on this basis, introduces carbon fiber, carbon black, lignin, starch, alumina and talcum powder as fillers to improve the comprehensive performance of the conveyor belt covering rubber, thereby improving the wear resistance of the conveyor belt covering rubber through the change of the rubber matrix formula and the addition of fillers, so that the service life of the conveyor belt can be improved, bringing good economic benefits to the enterprise. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of the steps of the preparation method of the present invention. DETAILED DESCRIPTION
[0027] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.
[0028] The raw materials used in the following examples were all obtained through conventional commercial routes.
[0029] Embodiment 1
[0030] according to Figure 1 As shown, this embodiment proposes a highly wear-resistant conveyor belt covering rubber, 55 parts of natural rubber, 40 parts of styrene-butadiene rubber, 20 parts of isoprene rubber, 5 parts of recycled rubber powder, 5 parts of liquid silicone rubber, 2 parts of carbon fiber, 30 parts of carbon black, 8 parts of wear-resistant agent, 3 parts of silane coupling agent, 3 parts of plasticizer, 6 parts of lignin, 8 parts of starch, 1 part of accelerator, 4 parts of aluminum oxide, 2 parts of stearic acid, 2 parts of antioxidant, 2 parts of vulcanizer, 2 parts of anti-scorch The invention discloses a novel polyol comprising: a plasticizer of 1 part, talcum powder of 6 parts, a tackifier of 1 part, and zinc oxide of 3 parts, wherein the plasticizer is softened heavy oil, the carbon black is a combination of carbon black N220 and carbon black N330, the weight ratio of carbon black N220 to carbon black N330 is 2:1, the anti-wear agent is silicone oil, the antioxidant is antioxidant 4010NA, the vulcanizing agent is sulfur, the tackifier is polyisobutylene, the anti-scorch agent is anti-scorch agent CTP, and the silane coupling agent is coupling agent KH560.
[0031] A method for preparing a highly wear-resistant conveyor belt covering rubber comprises the following steps:
[0032] Step 1: Material preparation
[0033] Accurately weigh all raw materials, including natural rubber, styrene-butadiene rubber, isoprene rubber, recycled rubber powder, liquid silicone rubber, carbon fiber, carbon black, wear-resistant agent, silane coupling agent, plasticizer, lignin, starch, accelerator, aluminum oxide, stearic acid, antioxidant, vulcanizer, anti-scorch agent, talcum powder, tackifier, zinc oxide;
[0034] Step 2: Primary rubber matrix processing
[0035] Add natural rubber, styrene-butadiene rubber, isoprene rubber, recycled rubber powder and liquid silicone rubber into an internal mixer and mix for 5 minutes. The temperature of the internal mixer is 65°C. After mixing, a rubber matrix is obtained. The speed of the internal mixer is 40 r / min.
[0036] Step 3: Secondary rubber matrix processing
[0037] Carbon fiber, carbon black, lignin, starch, talcum powder and silane coupling agent are sequentially added into an internal mixer and internally mixed with the rubber matrix. The internal mixing time is 8 minutes and the internal mixing temperature is 75°C. After internal mixing, a mixed colloid is obtained. The speed of the internal mixer remains unchanged and the interval between each addition of materials is 30 seconds.
[0038] Step 4: Vulcanization of mixed colloid
[0039] The remaining raw materials are then added to an internal mixer, the temperature is kept constant, the internal mixer time is 10 minutes, the internal mixer speed is 30r / min, a mixed rubber mixture is obtained, and then the rubber mixture is placed in a vulcanizer for vulcanization;
[0040] Step 5: Conveyor belt cover rubber molding
[0041] After step 4 vulcanization, the material is taken out and cooled, and after cooling, it is added into a calender to form the covering rubber.
[0042] Embodiment 2
[0043] according to Figure 1 As shown, this embodiment proposes a highly wear-resistant conveyor belt covering rubber, including the following raw materials by weight: 40 parts of natural rubber, 55 parts of styrene-butadiene rubber, 10 parts of isoprene rubber, 10 parts of recycled rubber powder, 18 parts of liquid silicone rubber, 3 parts of carbon fiber, 40 parts of carbon black, 12 parts of wear-resistant agent, 5 parts of silane coupling agent, 5 parts of plasticizer, 8 parts of lignin, 6 parts of starch, 2 parts of accelerator, 6 parts of aluminum oxide, 4 parts of stearic acid, and 4 parts of antioxidant. The invention discloses a novel polyol comprising the following components: a polyol, ...
[0044] A method for preparing a highly wear-resistant conveyor belt covering rubber comprises the following steps:
[0045] Step 1: Material preparation
[0046] Accurately weigh all raw materials, including natural rubber, styrene-butadiene rubber, isoprene rubber, recycled rubber powder, liquid silicone rubber, carbon fiber, carbon black, wear-resistant agent, silane coupling agent, plasticizer, lignin, starch, accelerator, aluminum oxide, stearic acid, antioxidant, vulcanizer, anti-scorch agent, talcum powder, tackifier, zinc oxide;
[0047] Step 2: Primary rubber matrix processing
[0048] Add natural rubber, styrene-butadiene rubber, isoprene rubber, recycled rubber powder and liquid silicone rubber into an internal mixer and mix for 10 minutes at a temperature of 80°C to obtain a rubber matrix at a speed of 40 r / min.
[0049] Step 3: Secondary rubber matrix processing
[0050] Carbon fiber, carbon black, lignin, starch, talcum powder and silane coupling agent are sequentially added into an internal mixer and internally mixed with the rubber matrix. The internal mixing time is 10 minutes and the internal mixing temperature is 90°C. After internal mixing, a mixed colloid is obtained. The speed of the internal mixer remains unchanged and the interval between each addition of materials is 30 seconds.
[0051] Step 4: Vulcanization of mixed colloid
[0052] The remaining raw materials are then added to an internal mixer, the temperature is kept constant, the internal mixer time is 12 minutes, the internal mixer speed is 30 r / min, a mixed rubber mixture is obtained, and then the rubber mixture is placed in a vulcanizer for vulcanization;
[0053] Step 5: Conveyor belt cover rubber molding
[0054] After step 4 vulcanization, the material is taken out and cooled, and after cooling, it is added into a calender to form the covering rubber.
[0055] Embodiment 3
[0056] according to Figure 1 As shown, this embodiment proposes a highly wear-resistant conveyor belt covering rubber, including the following raw materials by weight: 50 parts of natural rubber, 50 parts of styrene-butadiene rubber, 15 parts of isoprene rubber, 7 parts of recycled rubber powder, 12 parts of liquid silicone rubber, 2.5 parts of carbon fiber, 35 parts of carbon black, 10 parts of wear-resistant agent, 4 parts of silane coupling agent, 4 parts of plasticizer, 7 parts of lignin, 7 parts of starch, 1.5 parts of accelerator, 5 parts of aluminum oxide, 3 parts of stearic acid, 3 parts of antioxidant, and 10 parts of sulfur. The composition comprises: 2.5 parts of a scorching agent, 1.5 parts of a scorching retarder, 8 parts of talc, 1.5 parts of a tackifier, 4 parts of zinc oxide, the plasticizer is softened heavy oil, the carbon black is a composition of carbon black N220 and carbon black N330, the weight ratio of carbon black N220 to carbon black N330 is 2:1, the anti-wear agent is silicone oil, the antioxidant is antioxidant BLE, the vulcanizing agent is sulfur, the tackifier is polyisobutylene, the scorching retarder is scorching retarder CTP, and the silane coupling agent is coupling agent KH560.
[0057] A method for preparing a highly wear-resistant conveyor belt covering rubber comprises the following steps:
[0058] Step 1: Material preparation
[0059] Accurately weigh all raw materials, including natural rubber, styrene-butadiene rubber, isoprene rubber, recycled rubber powder, liquid silicone rubber, carbon fiber, carbon black, wear-resistant agent, silane coupling agent, plasticizer, lignin, starch, accelerator, aluminum oxide, stearic acid, antioxidant, vulcanizer, anti-scorch agent, talcum powder, tackifier, zinc oxide;
[0060] Step 2: Primary rubber matrix processing
[0061] Add natural rubber, styrene-butadiene rubber, isoprene rubber, recycled rubber powder and liquid silicone rubber into an internal mixer and mix for 8 minutes. The temperature of the internal mixer is 75°C. After mixing, a rubber matrix is obtained. The speed of the internal mixer is 40 r / min.
[0062] Step 3: Secondary rubber matrix processing
[0063] Carbon fiber, carbon black, lignin, starch, talcum powder and silane coupling agent are sequentially added into an internal mixer and internally mixed with the rubber matrix. The internal mixing time is 9 minutes and the internal mixing temperature is 85°C. After internal mixing, a mixed colloid is obtained. The speed of the internal mixer remains unchanged and the interval between each addition of materials is 30 seconds.
[0064] Step 4: Vulcanization of mixed colloid
[0065] The remaining raw materials are then added to an internal mixer, the temperature is kept constant, the internal mixer time is 11 minutes, the internal mixer speed is 30 r / min, a mixed rubber mixture is obtained, and then the rubber mixture is placed in a vulcanizer for vulcanization;
[0066] Step 5: Conveyor belt cover rubber molding
[0067] After step 4 vulcanization, the material is taken out and cooled, and after cooling, it is added into a calender to form the covering rubber.
[0068] In combination with Example 1, Example 2 and Example 3, Comparative Example 1 is set. Comparative Example 1 is a conveyor belt covering rubber conventionally purchased in the market, and its main components are natural rubber, styrene-butadiene rubber, carbon black, and calcium carbonate. Other components are not described. Compared with Comparative Example 1, mechanical properties, wear resistance and Akron abrasion tests are performed, and the comparison results are shown in the following table:
[0069]
[0070] As shown in the above table, the mechanical properties and wear resistance of the conveyor belt covering rubber prepared in Example 1, Example 2, and Example 3 are significantly improved. Specifically, in this application, on the basis of natural rubber and styrene-butadiene rubber, isoprene rubber and liquid silicone rubber are added as the main material part of the rubber to improve the basic formula of the conveyor belt covering rubber, as described below:
[0071] Isoprene rubber has excellent elasticity, which can improve the resilience and fatigue resistance of the conveyor belt cover rubber. At the same time, it has good wear resistance.
[0072] Liquid silicone rubber is added as a filler in the present invention, and the density and hardness of the material are increased through physical filling, thereby improving the wear resistance.
[0073] Furthermore, by introducing recycled rubber powder, the present invention has the effects of reducing environmental pollution and lowering costs.
[0074] Then on this basis, carbon fiber, carbon black, lignin, starch, alumina and talcum powder are introduced as fillers. The addition of carbon fiber, carbon black and alumina can improve the strength and wear resistance of the conveyor belt covering rubber, while lignin, starch and talcum powder have a reinforcing effect, further improving the strength and wear resistance of the conveyor belt covering rubber. Then, a certain wear-resistant agent is added. Through the above method, the wear resistance and mechanical properties of the conveyor belt covering rubber can be effectively improved, thereby increasing the service life of the conveyor belt in the subsequent use process, bringing economic benefits to the enterprise.
[0075] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the framework and scope of application of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A highly wear-resistant conveyor belt covering rubber, characterized in that: The invention comprises the following raw materials in parts by weight: 40-55 parts of natural rubber, 40-55 parts of styrene-butadiene rubber, 10-20 parts of isoprene rubber, 5-10 parts of recycled rubber powder, 5-18 parts of liquid silicone rubber, 2-3 parts of carbon fiber, 30-40 parts of carbon black, 8-12 parts of wear resistance agent, 3-5 parts of silane coupling agent, 3-5 parts of plasticizer, 6-8 parts of lignin, 6-8 parts of starch, 1-2 parts of accelerator, 4-6 parts of aluminum oxide, 2-4 parts of stearic acid, 2-4 parts of antioxidant, 2-3 parts of vulcanizer, 1-2 parts of anti-scorch agent, 6-10 parts of talc powder, 1-2 parts of tackifier and 3-5 parts of zinc oxide.
2. The highly wear-resistant conveyor belt covering rubber according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 55 parts of natural rubber, 40 parts of styrene-butadiene rubber, 20 parts of isoprene rubber, 5 parts of recycled rubber powder, 5 parts of liquid silicone rubber, 2 parts of carbon fiber, 30 parts of carbon black, 8 parts of wear resistance agent, 3 parts of silane coupling agent, 3 parts of plasticizer, 6 parts of lignin, 8 parts of starch, 1 part of accelerator, 4 parts of aluminum oxide, 2 parts of stearic acid, 2 parts of antioxidant, 2 parts of vulcanizer, 1 part of anti-scorch agent, 6 parts of talc, 1 part of tackifier and 3 parts of zinc oxide.
3. The highly wear-resistant conveyor belt covering rubber according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 40 parts of natural rubber, 55 parts of styrene-butadiene rubber, 10 parts of isoprene rubber, 10 parts of recycled rubber powder, 18 parts of liquid silicone rubber, 3 parts of carbon fiber, 40 parts of carbon black, 12 parts of wear resistance agent, 5 parts of silane coupling agent, 5 parts of plasticizer, 8 parts of lignin, 6 parts of starch, 2 parts of accelerator, 6 parts of aluminum oxide, 4 parts of stearic acid, 4 parts of antioxidant, 3 parts of vulcanizer, 2 parts of anti-scorch agent, 10 parts of talc, 2 parts of tackifier and 5 parts of zinc oxide.
4. The highly wear-resistant conveyor belt covering rubber according to claim 1, characterized in that: The plasticizer is one of softened heavy oil and pine tar.
5. The highly wear-resistant conveyor belt covering rubber according to claim 1, characterized in that: The carbon black is a composition of carbon black N220 and carbon black N330, and the weight ratio of the carbon black N220 to the carbon black N330 is 2:
1.
6. The highly wear-resistant conveyor belt covering rubber according to claim 1, characterized in that: The anti-wear agent is silicone oil.
7. The highly wear-resistant conveyor belt covering rubber according to claim 1, characterized in that: The antioxidant is one of antioxidant 4010NA, antioxidant RD and antioxidant BLE.
8. The highly wear-resistant conveyor belt covering rubber according to claim 1, characterized in that: The vulcanizing agent is sulfur, the tackifier is polyisobutylene, the anti-scorch agent is anti-scorch agent CTP, and the silane coupling agent is coupling agent KH560.
9. A method for preparing a highly wear-resistant conveyor belt covering rubber as claimed in claim 1, characterized in that: The following steps are involved: Step 1: Material preparation Accurately weigh all raw materials, including natural rubber, styrene-butadiene rubber, isoprene rubber, recycled rubber powder, liquid silicone rubber, carbon fiber, carbon black, wear-resistant agent, silane coupling agent, plasticizer, lignin, starch, accelerator, aluminum oxide, stearic acid, antioxidant, vulcanizer, anti-scorch agent, talcum powder, tackifier, zinc oxide; Step 2: Primary rubber matrix processing Add natural rubber, styrene-butadiene rubber, isoprene rubber, recycled rubber powder and liquid silicone rubber into an internal mixer, mix for 5 to 10 minutes, the temperature of the internal mixer is 65 to 80° C., and a rubber matrix is obtained after internal mixing, wherein the speed of the internal mixer is 40 r / min; Step 3: Secondary rubber matrix processing The carbon fiber, carbon black, lignin, starch, talcum powder and silane coupling agent are sequentially added into an internal mixer and internally mixed with the rubber matrix. The internal mixing time is 8 to 10 minutes and the internal mixing temperature is 75 to 90° C. After internal mixing, a mixed colloid is obtained, wherein the speed of the internal mixer remains unchanged; Step 4: Vulcanization of mixed colloid The remaining raw materials are then added to the internal mixer, the temperature is kept constant, the internal mixing time is 10 to 12 minutes, the internal mixer speed is 30 r / min, a mixed rubber mixture is obtained, and then the rubber mixture is placed in a vulcanizer for vulcanization; Step 5: Conveyor belt cover rubber molding After step 4 vulcanization, the material is taken out and cooled, and after cooling, it is added into a calender to form the covering rubber.
10. The method for preparing a highly wear-resistant conveyor belt covering rubber according to claim 9, characterized in that: In the step 3, the interval between each addition of materials is 30 seconds.
Citation Information
Cited By
Puncture-resistant and wear-resistant rubber surface formula and coating process
CN119463314A
NR wear-resistant molded part material for poultry depilator as well as preparation method and application of NR wear-resistant molded part material
CN121517782A