Modified polypropylene resin, intercalated melt-blown sound-absorbing cotton and preparation method and application of modified polypropylene resin and intercalated melt-blown sound-absorbing cotton
By introducing a specific antioxidant system into polypropylene resin, the modified polypropylene resin is used to prepare intercalated melt-blown sound-absorbing cotton, which solves the thermal aging problem of sound-absorbing cotton under high temperature conditions and achieves stable performance in high temperature environments. and long-term use.
Patent Information
- Application Number
- CN202310322237.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Existing PP/PET two-component sound-absorbing cotton is prone to thermal aging under high temperature conditions, resulting in reduced mechanical properties and sound-absorbing performance, making it difficult to meet the long-term application needs of automotive interiors.
Using modified polypropylene resin, a special antioxidant system is introduced, including a three-claw sterically hindered hindered phenolic antioxidant, 2,6-di-tert-butyl-p-methylphenol, and a phosphite antioxidant. and metal ion passivators, through the synergistic effect of these antioxidants, the heat aging resistance of the material is improved.
It can be maintained at 120℃ for more than 3000h without breaking or yellowing. It maintains good compression recovery performance and its performance is not affected. It is suitable for automotive interior functional materials in high temperature environments.
Smart Images

Figure BDA0004152209430000071 
Figure BDA0004152209430000081 
Figure BDA0004152209430000082
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a modified polypropylene resin, an intercalated melt-blown sound-absorbing cotton, and a preparation method and application thereof. Background Art
[0002] Noise pollution is one of the three major pollutions along with water pollution and air pollution. Noise control requires, on the one hand, controlling the source, adopting lubrication, silencing technology or formulating corresponding control rules, and on the other hand, eliminating or reducing noise pollution through reflection, isolation, absorption and other means. In the prior art, high-density metal materials are often used to block noise. When sound waves encounter these materials, they will be reflected or resonate with the materials, thereby weakening the energy of the sound waves. For noise absorption, loose and porous materials with many internal interfaces are often used. When sound passes through these materials, it will be reflected back and forth and attenuated by internal friction. In practical applications, people often combine the principles of sound insulation and sound absorption to control noise.
[0003] The intercalation composite meltblown technology is a technology that blows the opened short fibers into the ultra-fine meltblown fibers during the meltblowing process, and forms a special meltblown nonwoven fabric with an intercalation composite structure through mixing into a web and self-bonding reinforcement. This technology inserts high-curl hollow fibers into soft meltblown fibers to obtain a meltblown material with a highly fluffy pore structure and good elastic recovery performance. This material has very good sound insulation and sound absorption effects. When sound waves propagate into the interior of this material, they will reflect back and forth at the fiber interface, causing the air vibration in the pores and the vibration of the fiber itself to synergistically consume the sound wave energy. For example, in the PP melt-blowing process, hollow PET fibers are blown into the melt-blown fiber network in a certain proportion, and then compounded with non-woven fabrics to prepare the PP / PET two-component melt-blown sound-absorbing material, which is often used in automobile door panels, dashboards, fenders, trunks and other parts for sound absorption. Compared with traditional felt, rubber sheets and foam materials, this material has lower density, good compressibility, a wide range of raw material sources, low cost, easy large-scale production and parameter adjustment, and has good market potential.
[0004] However, ordinary PP / PET two-component sound-absorbing cotton is prone to thermal aging under high temperature conditions, resulting in reduced mechanical properties and sound absorption performance. Generally speaking, after 500 hours of high-temperature thermal oxidation aging test, the sound-absorbing cotton will have problems such as yellowing of the surface and powdering of the material, which makes it difficult to meet the long-term application requirements as a functional material for automotive interiors. Summary of the invention
[0005] Based on the defects of the prior art, the purpose of the present invention is to provide a modified polypropylene resin and an intercalated melt-blown sound-absorbing cotton. A special antioxidant system is introduced into the components of the modified polypropylene resin product to implement modification. The heat aging effect of the obtained intercalated melt-blown sound-absorbing cotton product is significantly improved during production, processing, storage and use. It can be maintained for more than 3000 hours without breaking or yellowing in an environment of 120°C, and at the same time has a good compression recovery performance retention rate, and the use performance is not affected.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A modified polypropylene resin comprises the following components in parts by weight:
[0008] Polypropylene 94-99 parts, primary antioxidant 0.2-0.9 parts, secondary antioxidant 0.2-0.8 parts, metal ion passivator 0.1-0.3 parts, acid absorbent 0.5-3 parts and processing aid 0.05-0.3 parts;
[0009] The modified polypropylene resin comprises a modified polypropylene resin 1 and a modified polypropylene resin 2, wherein the polypropylene in the modified polypropylene resin 1 component is polypropylene 1, and the melt flow rate of the polypropylene 1 under a load of 2.16 kg at 230° C. is 500 to 2000 g / 10 min according to GB / T 3682.1-2018, and the polypropylene in the modified polypropylene resin 2 component is polypropylene 2, and the melt flow rate of the polypropylene 2 under a load of 2.16 kg at 230° C. is 5 to 60 g / 10 min according to GB / T 3682.1-2018;
[0010] The main antioxidant is a mixture of a hindered phenol antioxidant containing a three-claw steric hindered structure and 2,6-di-tert-butyl-p-methylphenol;
[0011] The auxiliary antioxidant is at least one of a phosphite antioxidant and an organic sulfur antioxidant.
[0012] Preferably, the phosphite antioxidant is bis(2,4-dicumylphenyl)pentaerythritol diphosphite, and the organic sulfur antioxidant is pentaerythritol tetrakis(3-laurylthiopropionate).
[0013] Preferably, the hindered phenol antioxidant containing a three-clawed steric hindered structure is at least one of 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid and 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene.
[0014] The inventors found that the existing sound-absorbing cotton made of polypropylene has poor heat aging resistance, mainly because there is a tertiary carbon atom every other carbon atom on the main chain of the polypropylene molecule, which is easily attacked by external oxygen free radicals and peroxy free radicals to produce free radicals, thereby inducing free radical degradation reactions. In addition, the diameter of melt-blown polypropylene fiber is less than 10μm, but the specific surface area is thousands or even tens of thousands times that of ordinary polypropylene products, so the probability of being attacked by active oxygen atoms and free radicals in the external environment is higher. Therefore, the present invention provides a modified polypropylene resin with heat-resistant aging performance, and the modified resin replaces the traditional polypropylene resin matrix component for preparing intercalated melt-blown sound-absorbing cotton. Among the main antioxidant components contained in the modified polypropylene resin, the hindered phenol antioxidant containing a three-claw steric hindrance structure has a three-claw structure that is not in the same plane. The structure uses a benzene ring as a connection center, has high stability, can be well anchored with polypropylene and other organic components, is not easy to migrate, and effectively resists the attack of external oxygen free radicals and peroxyl free radicals; at the same time, for the groups that penetrate into the interior of the product, 2,6-di-tert-butyl-p-methylphenol can well implement directional and rapid capture, inhibit the aging and degradation reaction of the product during the thermal processing process and the use in a hot environment, and improve the heat-resistant aging performance of the product through the synergistic effect of the two key antioxidants.
[0015] On the other hand, phosphite antioxidants (preferably bis(2,4-dicumylphenyl)pentaerythritol diphosphite) and organic sulfur antioxidants (preferably pentaerythritol tetra(3-laurylthiopropionate)) have high high temperature stability and hydrolysis stability, and when used as auxiliary antioxidants, they have a significant alleviating effect on the yellowing phenomenon of the product during thermal processing and use in a hot environment; metal ion passivators are often used in materials that are in close contact with metals, such as wires and cables, and the introduction of the metal ion passivator contained in the product of the present invention is mainly to eliminate the influence of metal ion components introduced or contacted by the product during thermal processing and use in a hot environment (most active metal ions will act as degradation catalysts for polymers in a high-temperature environment, causing the performance of the polymer to be weakened); when polypropylene inevitably undergoes partial degradation reactions during thermal aging, the peroxy acid produced will further decompose into peroxy radicals and hydroxyl radicals, resulting in a trend of continuous degradation. In combination with the main antioxidant, the introduction of a certain amount of acid absorber can effectively neutralize the peroxy acid and inhibit the generation of internal peroxy radicals and free radicals.
[0016] Preferably, the weight proportion of the primary antioxidant is 0.2 to 0.8 parts; the weight proportion of the hindered phenol antioxidant containing a three-claw steric structure and 2,6-di-tert-butyl-p-methylphenol is (6:4) to (8.5:1.5).
[0017] Since the two key substances in the main antioxidant have different mechanisms of action, changes in their ratio and total amount will lead to changes in the activity of external or internal oxygen free radicals and peroxyl free radicals, and the degree of inhibition of the free radical degradation reaction of the product will also change. After optimization, the main antioxidant under the above ratio can exert the best activity effect.
[0018] Preferably, the metal ion passivator is at least one of N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate][oxalylbis(azanediyl)]bis(ethane-2,1-diyl)ester, benzotriazole and melamine.
[0019] More preferably, the metal ion passivator is a mixture of benzotriazole and melamine, and the mass ratio of the two is (1-4):1.
[0020] For metal ions that appear during processing or use, in order to further inhibit their catalytic activity, a mixture of benzotriazole and melamine is used together as a metal ion passivator for better results.
[0021] Preferably, the acid absorber is at least one of magnesium hydroxystearate, zinc hydroxystearate, calcium hydroxystearate and calcium aluminum hydrotalcite.
[0022] Preferably, the processing aid is a lubricant;
[0023] More preferably, the lubricant is a fluorine-containing polymer lubricant.
[0024] More preferably, the fluorine-containing polymer lubricant is selected from at least one of Dynamar FX5912, Dynamar FX5920, Dynamar FX5922 and Dynamar FX5924 produced by 3M Company.
[0025] Another object of the present invention is to provide a method for preparing the modified polypropylene resin, comprising the following steps: mixing the remaining components of the modified polypropylene resin 1 except polypropylene 1, and placing them in a twin-screw extruder according to the component ratio with polypropylene 1 to melt-mix until uniform, then cooling and pelletizing to prepare modified polypropylene resin 1; mixing the remaining components of the modified polypropylene resin 2 except polypropylene 2, and placing them in a twin-screw extruder according to the component ratio with polypropylene 2 to melt-mix until uniform, then cooling and pelletizing to prepare modified polypropylene resin 2.
[0026] Preferably, the temperature during the melt mixing is 190-230°C.
[0027] Another object of the present invention is to provide an intercalated melt-blown sound-absorbing cotton, comprising the modified polypropylene resin of the present invention and PET hollow fibers. Preferably, the PET hollow fibers have a fineness of 1 to 7 dtex and a length of 30 to 60 mm.
[0028] Another object of the present invention is to provide a method for preparing the intercalated melt-blown sound-absorbing cotton, comprising the following steps:
[0029] (1) transferring part of the modified polypropylene resin 1 to a single screw extruder for melting and plasticization and conveying it to a melt-blowing die head for spraying to obtain a polypropylene melt-blown fiber; then blowing the pretreated PET hollow fiber into the polypropylene melt-blown fiber to obtain a two-component fiber layer;
[0030] (2) adding the remaining modified polypropylene resin 1 and modified polypropylene resin 2 into a single screw extruder, respectively, to melt and plasticize, and conveying them to a melt-blown and spun-bonded die to form a web, and then laminating them online to obtain an SMS (spun-bonded-melt-blown-spun-bonded, S layer-M layer-S layer) non-woven fabric;
[0031] (3) The intercalated melt-blown sound-absorbing cotton is obtained by compounding the bicomponent fiber layer and the SMS non-woven fabric, hot-rolling cutting, and ultrasonic edge sealing.
[0032] Based on the differences in configuration and composition of the two structures of the two-component fiber layer and the SMS non-woven fabric in the product, the heat-aging-resistant intercalated melt-blown sound-absorbing cotton of the present invention needs to use two polypropylenes with large fluidity differences as component raw materials, and construct the product with different processes. The preparation method has simple operating steps and can be implemented using industrially mature melting and spunbond melt-blown equipment, and can realize large-scale industrial production.
[0033] Preferably, the pretreatment of the PET hollow fiber in step (1) includes unpacking, loosening and combing. Preferably, the temperature during melt plasticization in step (1) is 220-250°C, and the temperature during melt blowing die spraying is 250-280°C.
[0034] Preferably, the temperature during melt plasticization in step (2) is 220-250°C, and the temperature during web formation by the spunbond die is 230-260°C.
[0035] Another object of the present invention is to provide an application of the intercalated melt-blown sound-absorbing cotton in the preparation of functional materials for automotive interior decoration.
[0036] The intercalated melt-blown sound-absorbing cotton of the present invention has high structural stability, can effectively resist the invasion of external oxygen free radicals or peroxy free radicals in a high temperature environment, inhibit its own degradation reaction, will not turn yellow or differentiate during thermal processing and use in a hot environment, has a high performance retention rate, can give full play to the sound absorption performance of the sound-absorbing cotton product, and is particularly suitable for automotive interior functional materials that have high requirements for mechanics, appearance, sound absorption and heat aging resistance.
[0037] The beneficial effect of the present invention is that the present invention provides a modified polypropylene resin and an intercalated melt-blown sound-absorbing cotton. The modified polypropylene resin product is modified by introducing a special antioxidant system into a polypropylene matrix component. The obtained intercalated melt-blown sound-absorbing cotton product has significantly improved thermal aging effects during production, processing, storage and use. It can be kept for more than 3000 hours at 120°C without breaking or yellowing, and has a good compression recovery performance retention rate, and the use performance is not affected. DETAILED DESCRIPTION
[0038] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by those of ordinary skill in the art without making creative work premise belong to the protection scope of the present invention. The experimental reagents and instruments involved in the implementation of the present invention, unless otherwise specified, are all commonly used common reagents and instruments.
[0039] Examples 1 to 15
[0040] The modified polypropylene resin, intercalated melt-blown sound-absorbing cotton and the preparation method and application thereof of the present invention are shown in Table 1. The modified polypropylene resin is used to prepare heat-resistant and aging-resistant intercalated melt-blown sound-absorbing cotton.
[0041] The preparation method of the intercalated melt-blown sound-absorbing cotton comprises the following steps:
[0042] (1) selecting polypropylene as a preparation raw material, wherein the polypropylene includes polypropylene 1 and polypropylene 2;
[0043] (2) mixing the remaining components of the modified resin except polypropylene, and placing them into a twin-screw extruder with polypropylene 1 and polypropylene 2 according to the component ratio, melt-mixing them at 200° C. until they are uniform, and then cooling and pelletizing to prepare modified resin 1 and modified resin 2;
[0044] (3) The modified resin 1 is transferred to a single screw extruder, melted and plasticized at 250° C., and transported to a melt-blown die head to be sprayed at 280° C. to obtain a polypropylene melt-blown fiber; then the PET hollow fiber after unpacking, opening and combing is evenly blown into the polypropylene melt-blown fiber at a mass ratio of 3:1 to obtain a bicomponent fiber layer, the bicomponent fiber layer density of which is 300 g / m 2 ;
[0045] (4) The modified resin 1 and the modified resin 2 were transferred to a single screw extruder, melted and plasticized at 230° C., and respectively conveyed to a melt-blown die and a spunbond die to form a web at 260° C., and then online compounded to obtain an SMS nonwoven fabric having a surface density of 30 g / m 2 , where the density ratio of S layer: M layer: S layer is about 3:4:3;
[0046] (5) The bicomponent fiber layer and the SMS nonwoven fabric are compounded and subjected to hot rolling, cutting, and ultrasonic edge sealing treatment to obtain the intercalated melt-blown sound-absorbing cotton.
[0047] Comparative Examples 1 to 5
[0048] The difference between the comparative examples and the embodiments is only in the types and proportions of components, as shown in Table 2.
[0049] Among the components described in each embodiment and comparative example,
[0050] Polypropylene 1 is PP-91500 produced by Kingfa Science & Technology, with a melt mass flow rate of 1500 g / 10 min at 230 °C and a load of 2.16 kg;
[0051] Polypropylene 2 is PP S2040 produced by Shanghai Saike, with a melt mass flow rate of 38 g / 10 min at 230°C and a load of 2.16 kg;
[0052] The hindered phenol antioxidant 1 containing a three-claw steric hindered structure is 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione (Cyanox 1790) produced by Solvay;
[0053] The hindered phenol antioxidant 2 containing a three-claw steric hindered structure is 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid (Irganox 3114) produced by BASF;
[0054] The hindered phenol antioxidant 3 containing a three-claw steric hindered structure is 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene (Irganox 1330) produced by BASF;
[0055] 2,6-di-tert-butyl-p-methylphenol is used by BASF to produce antioxidant 264;
[0056] The main antioxidant 1 for comparison is the commercially available antioxidant 1010;
[0057] The comparative main antioxidant 2 is commercially available 6-tert-butyl-2,4-dimethylphenol;
[0058] The phosphite antioxidant is bis(2,4-dicumylphenyl)pentaerythritol diphosphite produced by Dover Chemical Company of the United States;
[0059] The organic sulfur antioxidant is pentaerythritol tetrakis(3-laurylthiopropionate) produced by Tianjin Lianlong Company;
[0060] The comparative auxiliary antioxidant 1 is antioxidant 168 produced by BASF;
[0061] Metal ion passivator 1 is commercially available melamine;
[0062] Metal ion passivator 2 is commercially available benzotriazole;
[0063] The metal ion passivator 3 is a mixture of the metal ion passivator 1 and the metal ion passivator 2 in a mass ratio of 1:1;
[0064] Metal ion passivator 4 is a mixture of metal ion passivator 1 and metal ion passivator 2 in a mass ratio of 4:1;
[0065] The metal ion passivator 5 is a mixture of the metal ion passivator 1 and the metal ion passivator 2 in a mass ratio of 1:2;
[0066] The metal ion passivator 6 is a mixture of the metal ion passivator 1 and the metal ion passivator 2 in a mass ratio of 6:1;
[0067] Metal ion passivator 7 is commercially available zinc stearate;
[0068] Acid absorbent 1 is commercially available magnesium hydroxystearate;
[0069] Acid absorbent 2 is commercially available calcium aluminum hydrotalcite;
[0070] The fluoropolymer lubricant is Dynamar FX5912 produced by 3M Company;
[0071] The PET hollow fiber is ZK652 produced by Yizheng Chemical Fiber, with a fineness of 6.67 dtex and a length of 60 mm.
[0072] Unless otherwise specified, the components used in the embodiments and comparative examples of the present invention are all commercially available, and the components used in each parallel experiment are all of the same type.
[0073] Table 1
[0074]
[0075]
[0076] Table 2
[0077]
[0078]
[0079] Effect Example 1
[0080] In order to verify the performance of the intercalated melt-blown sound-absorbing cotton of the present invention, the following performance tests were performed on the products of each embodiment and comparative example, and the specific steps are as follows:
[0081] (1) Powdering performance test: Cut each product into square samples of 20×20 cm and subject them to thermal aging treatment at 120°C for 2000 h. Observe whether there is powdering on the surface. Then, gently tap and bend the samples with a slight external force to further observe whether powdering occurs. If powdering occurs at any stage, it means that the product is not resistant to heat aging powdering and the compression recovery test is no longer performed.
[0082] (2) Yellowing test: Cut each product into 20×20 cm square samples and subject them to thermal aging treatment at 120°C for 2000 h. Use a colorimeter to measure the Lab values of the product surface before and after treatment (test at 5 points on the plane and take the average value). If the b value (△b) of the product after treatment is greater than 10, it means that the product has yellowed, indicating that the product is not resistant to heat aging yellowing.
[0083] (3) Compression recovery test: each sample was allowed to stand at 23±2°C and 50±5% RH for 16 h, and then the thickness L0 of the sample was tested according to the method described in 9.3 of GB / T 24218.2-2009 (20 Pa pressure); a pressure of 5 kPa was applied to the sample, and it was allowed to stand at 23±2°C and 50±5% RH for 16 h, and then the load pressure was removed to allow the sample to recover freely for 30 min; the thickness L1 of the sample was tested according to the method described in 9.3 of GB / T 24218.2-2009 (20 Pa pressure), and the compression recovery performance R = (L1 / L0) × 100%; the compression recovery performance R0 and R1 of the sample before and after thermal oxidative aging (120°C thermal oxidative aging treatment for 2000 h) were tested respectively. a , calculate the compression recovery performance retention rate (%) of the sample, the calculation formula = 100% × Ra / R0, where when the retention rate is ≥90%, the sample can be considered to have qualified heat aging resistance compression recovery performance.
[0084] The test results are shown in Table 3.
[0085] Table 3
[0086]
[0087] Table 4
[0088]
[0089] It can be seen from Tables 3 and 4 that the intercalated melt-blown sound-absorbing cotton prepared in each embodiment of the present invention has excellent heat aging resistance, and no powdering phenomenon occurs after testing. Furthermore, when the weight portion of the main antioxidant in the product is 0.2 to 0.8 parts; and the weight of the hindered phenolic antioxidant containing a three-claw steric hindered structure and 2,6-di-tert-butyl-p-methylphenol accounts for (6:4) to (8.5:1.5), the obtained product has a △b in the yellowing test of <10, and the product does not yellow. At the same time, the compression recovery performance retention rate of the product after thermal oxidative aging treatment can be maintained in the range of 93 to 95%. In contrast, the main antioxidant used in the product of Comparative Example 1 is a single antioxidant 1010, which cannot achieve the expected heat aging resistance, and the product shows powdering and yellowing; although the product of Comparative Example 2 is compounded with antioxidant 1010 and 2,6-di-tert-butyl-p-methylphenol respectively, the synergistic effect of the hindered phenolic antioxidant containing a three-claw steric structure and 2,6-di-tert-butyl-p-methylphenol cannot be achieved; similarly, the hindered phenolic antioxidant containing a three-claw steric structure and 6-tert-butyl-2,4-dimethylphenol in the product of Comparative Example 3 cannot achieve the same effect, and the heat aging resistance of both products is poor. In the product of the present invention, in addition to the main antioxidant, the type of auxiliary antioxidant cannot be selected at will. As shown in Comparative Example 4, if an inappropriate auxiliary antioxidant is used, the heat aging resistance of the product cannot meet expectations.
[0090] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A modified polypropylene resin, characterized in that: The composition comprises the following components in parts by weight: Polypropylene 94-99 parts, primary antioxidant 0.2-0.9 parts, secondary antioxidant 0.2-0.8 parts, metal ion passivator 0.1-0.3 parts, acid absorbent 0.5-3 parts and processing aid 0.05-0.3 parts; The modified polypropylene resin comprises a modified polypropylene resin 1 and a modified polypropylene resin 2, wherein the polypropylene in the modified polypropylene resin 1 component is polypropylene 1, and the melt flow rate of the polypropylene 1 under a load of 2.16 kg at 230° C. is 500 to 2000 g / 10 min according to GB / T 3682.1-2018, and the polypropylene in the modified polypropylene resin 2 component is polypropylene 2, and the melt flow rate of the polypropylene 2 under a load of 2.16 kg at 230° C. is 5 to 60 g / 10 min according to GB / T 3682.1-2018; The main antioxidant is a mixture of a hindered phenol antioxidant containing a three-claw steric hindered structure and 2,6-di-tert-butyl-p-methylphenol; The auxiliary antioxidant is at least one of a phosphite antioxidant and an organic sulfur antioxidant.
2. The modified polypropylene resin according to claim 1, characterized in that: The weight proportion of the main antioxidant is 0.2 to 0.8 parts; the weight proportion of the hindered phenol antioxidant containing a three-claw steric hindrance structure and 2,6-di-tert-butyl-p-methylphenol is (6:4) to (8.5:1.5); preferably, the hindered phenol antioxidant containing a three-claw steric hindrance structure is at least one of 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)-1,3,5-triazine-2,4,6-(1H,3H,5H)-trione, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid and 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene.
3. The modified polypropylene resin according to claim 1, characterized in that: The phosphite antioxidant is bis(2,4-dicumylphenyl)pentaerythritol diphosphite, and the organic sulfur antioxidant is pentaerythritol tetrakis(3-laurylthiopropionate).
4. The modified polypropylene resin according to claim 1, characterized in that: The metal ion passivator is at least one of N,N'-bis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl]hydrazine, bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid], [oxalylbis(azanediyl)]bis(ethane-2,1-diyl)ester, benzotriazole, and melamine; preferably, the metal ion passivator is a mixture of benzotriazole and melamine, and the mass ratio of the two is (1 to 4):
1.
5. The modified polypropylene resin according to claim 1, characterized in that: The acid absorber is at least one of magnesium hydroxystearate, zinc hydroxystearate, calcium hydroxystearate and calcium aluminum hydrotalcite; the processing aid is a lubricant; preferably, the lubricant is a fluorine-containing polymer lubricant.
6. The method for preparing the modified polypropylene resin according to any one of claims 1 to 5, characterized in that: The following steps are involved: The remaining components of the modified polypropylene resin 1 except polypropylene 1 are mixed, and are respectively placed in a twin-screw extruder with polypropylene 1 according to the component ratio for melt mixing until uniform, followed by cooling and pelletizing to prepare modified polypropylene resin 1; the remaining components of the modified polypropylene resin 2 except polypropylene 2 are mixed, and are respectively placed in a twin-screw extruder with polypropylene 2 according to the component ratio for melt mixing until uniform, followed by cooling and pelletizing to prepare modified polypropylene resin 2.
7. An intercalated melt-blown sound-absorbing cotton, characterized in that: The invention comprises the modified polypropylene resin according to any one of claims 1 to 5 and PET hollow fibers.
8. The intercalated melt-blown sound-absorbing cotton according to claim 7, characterized in that: The PET hollow fiber has a fineness of 1 to 7 dtex and a length of 30 to 60 mm.
9. The method for preparing the intercalated melt-blown sound-absorbing cotton according to claim 7 or 8, characterized in that: The following steps are involved: (1) transferring part of the polypropylene modified resin 1 to a single screw extruder for melting and plasticization and conveying the resin to a melt-blowing die head for spraying to obtain a polypropylene melt-blown fiber; The pretreated PET hollow fibers are then blown into polypropylene melt-blown fibers to obtain a bicomponent fiber layer; (2) adding the remaining modified polypropylene resin 1 and modified polypropylene resin 2 into a single screw extruder, melting and plasticizing them, and conveying them to a melt-blowing die and a spunbond die to form a web, and then compounding them online to obtain an SMS non-woven fabric; (3) compounding the bicomponent fiber layer and the SMS nonwoven fabric, hot-rolling cutting, and ultrasonic edge sealing to obtain the intercalated melt-blown sound-absorbing cotton; Preferably, the pretreatment of the PET hollow fibers in step (1) includes unpacking, loosening and combing; the surface density of the SMS nonwoven fabric in step (2) is between 25 and 35 g / m 2 , among which the ratio of S layer:M layer:S layer density is (2.8~3.2):(3.8~4.2):(2.8~3.2).
10. Use of the intercalated melt-blown sound-absorbing cotton as claimed in claim 7 or 8 in the preparation of functional materials for automotive interior decoration.
Citation Information
Patent Citations
Thermo-oxidative-aging-resistant polypropylene composite and preparation method thereof
CN104558809A
Amphipathic compound containing hindered phenol and phosphite, synthetic method and application thereof
CN105732713A
Amphipathic compound containing hindered phenol and pentaerythritol phosphite, synthetic method and application thereof
CN105732714A
Polypropylene material and preparation process thereof
CN107652547A
Sound-absorbing cotton material and preparation method thereof
CN107778655A