High-infiltration road modified asphalt and application thereof

By adding mineral fillers and modifiers to asphalt to form a composite layer structure, the problem of insufficient waterproof performance of asphalt pavement is solved, achieving higher water resistance and extending service life.

CN118725593APending Publication Date: 2024-10-01JIANGSU ZHONGYITONG ROAD NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410983344.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing asphalt pavements are prone to cracking and peeling due to moisture ingress after long-term use, resulting in insufficient waterproof performance.

Method used

High-wetting road modified asphalt is used. Mineral fillers, resin modifiers and fiber modifiers are added to the asphalt to form a composite layer structure to improve the water resistance and waterproof performance of the asphalt.

Benefits of technology

Effectively prevent moisture from entering the pavement interior, extend the service life of the asphalt pavement, and improve its waterproof performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses high-infiltration road modified asphalt, which is prepared from the following raw materials in percentage by mass: 60 to 70 percent of matrix asphalt, 20 to 30 percent of mineral filler, 7 to 12 percent of modifier and 0.5 to 1 percent of additive. The modifier comprises a resin modifier and a fiber modifier in a mass ratio of 1: 1. The modified asphalt is prepared from different resin modifier contents and mineral filler contents, during laying, at least 2-3 asphalt layers are laid and stacked to form a road pavement, and the content of the resin modifier is reduced and the content of the mineral filler is increased from bottom to top in the asphalt layers. The water resistance of the asphalt material is improved by using the mixed modifier containing the resin modifier and the mineral filler, and asphalt is paved in a composite layer form when a pavement is paved, so that the surface of the pavement can be kept to absorb water to a certain extent, and the water can be prevented from being immersed into the pavement for transition, thereby improving the wettability of the asphalt pavement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a road asphalt technology, in particular to a highly wettable road modified asphalt and application thereof. Background Art

[0002] Asphalt is the main material for road construction and maintenance. Since it is used in public and open environments, after long-term use, moisture enters the road surface and causes problems such as cracking and peeling.

[0003] Asphalt wettability refers to the depth to which asphalt is absorbed by a fixed mass of material under specific conditions and within a certain period of time. This indicator is an important indicator for measuring asphalt quality, and its accuracy and stability play a key role in ensuring project quality and service life. Wetting asphalt has excellent wettability and adhesion, and can form a watertight grease film layer on the pavement surface, thereby preventing moisture from penetrating into the pavement. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a highly wettable road modified asphalt to improve the waterproof performance of asphalt on the road surface.

[0005] Technical solution: A highly wettable road modified asphalt, the raw materials for preparation include 60-70% base asphalt, 20-30% mineral filler, 7-12% modifier, and 0.5-1% additive, and the above percentages are mass percentages; the modifier includes resin modifier and fiber modifier, which are mixed in a mass ratio of 1:1.

[0006] Furthermore, the resin modifier is polyurethane and PE, which are mixed in a mass ratio of 1:1; the fiber modifier is methyl cellulose and glass fiber.

[0007] Most preferably, the polyurethane is a polyolefin-based thermoplastic elastomer.

[0008] Furthermore, the mineral filler is clay.

[0009] A highly wettable road modified asphalt is prepared from raw materials including 64% of base asphalt, 24% of mineral filler, 11.5% of modifier and 0.5% of additive, wherein the above percentages are by mass.

[0010] A highly wettable road modified asphalt is prepared from raw materials including 64% of base asphalt, 26% of mineral filler, 9.5% of modifier and 0.5% of additive, wherein the above percentages are by mass.

[0011] An application of the above-mentioned highly wettable road modified asphalt is to prepare modified asphalt with different resin modifier contents and mineral filler contents respectively. When paving, at least 2 to 3 layers of asphalt are laid and stacked to form a road surface. From the bottom to the top of the asphalt layer, the resin modifier content decreases and the mineral filler content increases.

[0012] Furthermore, between two adjacent asphalt layers, the thickness of the lower layer is 1.2 times the thickness of the upper layer.

[0013] Beneficial effects: The advantages of the present invention are: using a mixed modifier containing a resin modifier and a mineral filler to improve the water resistance of the asphalt material. When paving the road surface, paving the asphalt in the form of a composite layer can not only maintain a certain absorption of moisture on the road surface, but also prevent moisture from infiltrating into the interior of the road surface, thereby improving the wettability of the asphalt pavement. DETAILED DESCRIPTION

[0014] The present invention will be further illustrated below in conjunction with specific embodiments.

[0015] A highly wettable road modified asphalt, the preparation raw materials of which include 60-70% of base asphalt, 20-30% of mineral filler, 7-12% of modifier and 0.5-1% of additive, the above percentages being mass percentages.

[0016] The mineral filler is clay.

[0017] The modifier includes a resin modifier and a fiber modifier, which are mixed in a mass ratio of 1:1. The resin modifier is polyurethane and PE, which are mixed in a mass ratio of 1:1, and the polyurethane adopts a polyolefin thermoplastic elastomer; the fiber modifier is methyl cellulose and glass fiber, which are mixed in any mass ratio.

[0018] Additives include stabilizers such as antioxidants and anti-aging agents, and rheology modifiers such as surfactants and dispersants.

[0019] The following examples are based on the above raw material selection.

[0020] Example 1

[0021] A highly wettable road modified asphalt (referred to as modified asphalt A), the raw materials for preparation, based on the total mass of 100%, include 64% base asphalt, 24% clay, 4% each of polyolefin thermoplastic elastomer and PE, 3% methyl cellulose, 0.5% glass fiber, and 0.5% additives.

[0022] A highly wettable road modified asphalt (referred to as modified asphalt B), the raw materials for preparation of which, based on the total mass of 100%, include 64% base asphalt, 26% clay, 6% each of polyolefin thermoplastic elastomer and PE, 3% methyl cellulose, 0.5% glass fiber, and 0.5% additives.

[0023] The preparation process of the above two modified asphalts is the same. The base asphalt is heated to a molten state, and the mineral filler and the modifier are gradually added during the stirring process, and mixed evenly, and then the additive is added, and the stirring is continued until it is uniform to obtain the modified asphalt.

[0024] When paving the road, first lay the lower asphalt layer with modified asphalt A, and then lay the upper asphalt layer on the lower asphalt layer with modified asphalt B. The standard thickness of conventional asphalt pavement is 12 to 18 cm, and the thickness of the lower asphalt layer is 1.2 times the thickness of the upper asphalt layer.

[0025] Example 2

[0026] A highly wettable road modified asphalt (referred to as modified asphalt C), the raw materials for preparation of which, based on the total mass of 100%, include 66% base asphalt, 24% clay, 3% each of polyolefin thermoplastic elastomer and PE, 3% methyl cellulose, 0.5% glass fiber and 0.5% additives.

[0027] A highly wettable road modified asphalt (referred to as modified asphalt D), the raw materials for preparation of which, based on the total mass of 100%, include 66% base asphalt, 26% clay, 2% each of polyolefin thermoplastic elastomer and PE, 3% methyl cellulose, 0.5% glass fiber, and 0.5% additives.

[0028] The preparation process of the above two modified asphalts is the same. The base asphalt is heated to a molten state, and the mineral filler and the modifier are gradually added during the stirring process, and mixed evenly, and then the additive is added, and the stirring is continued until it is uniform to obtain the modified asphalt.

[0029] When paving the road, first lay the lower asphalt layer with modified asphalt C, and then lay the upper asphalt layer on the lower asphalt layer with modified asphalt D. The standard thickness of conventional asphalt pavement is 12 to 18 cm, and the thickness of the lower asphalt layer is 1.2 times the thickness of the upper asphalt layer.

[0030] Example 3

[0031] A highly wettable road modified asphalt (referred to as modified asphalt E), the raw materials for preparation of which, based on the total mass of 100%, include 68% base asphalt, 22% clay, 3% each of polyolefin thermoplastic elastomer and PE, 3% methyl cellulose, 0.5% glass fiber and 0.5% additives.

[0032] A highly wettable road modified asphalt (referred to as modified asphalt F), the raw materials for preparation of which, based on the total mass of 100%, include 68% base asphalt, 24% clay, 2% each of polyolefin thermoplastic elastomer and PE, 3% methyl cellulose, 0.5% glass fiber and 0.5% additives.

[0033] The preparation process of the above two modified asphalts is the same. The base asphalt is heated to a molten state, and the mineral filler and the modifier are gradually added during the stirring process, and mixed evenly, and then the additive is added, and the stirring is continued until it is uniform to obtain the modified asphalt.

[0034] When paving the road surface, first lay the lower asphalt layer with modified asphalt E, and then lay the upper asphalt layer on the lower asphalt layer with modified asphalt F. The standard thickness of conventional asphalt pavement is 12 to 18 cm, and the thickness of the lower asphalt layer is 1.2 times the thickness of the upper asphalt layer.

[0035] Clay has good air permeability and alkali corrosion resistance, and polyolefin thermoplastic elastomer has excellent water resistance. When preparing modified asphalt, the raw materials are mixed. Under different proportions, the waterproof performance of the prepared modified asphalt can be comprehensively improved. When paving roads, modified asphalt with different proportions is used to pave the upper and lower asphalt layers. The principle is that the lower asphalt layer has a higher content of polyolefin thermoplastic elastomer and a lower content of clay than the upper asphalt layer. This can not only maintain a certain absorption of moisture on the surface of the road surface, but also prevent moisture from infiltrating into the interior of the road surface, thereby improving the wettability of the asphalt pavement.

Claims

1. A highly wettable road modified asphalt, Features: The preparation raw materials include 60-70% of base asphalt, 20-30% of mineral filler, 7-12% of modifier, and 0.5-1% of additive, and the above percentages are mass percentages; the modifier includes resin modifier and fiber modifier, which are mixed in a mass ratio of 1:

1.

2. The highly wettable road modified asphalt according to claim 1, Features: The resin modifiers are polyurethane and PE, which are mixed in a mass ratio of 1:1; the fiber modifiers are methyl cellulose and glass fiber.

3. The highly wettable road modified asphalt according to claim 1, Features: Polyurethane is a polyolefin thermoplastic elastomer.

4. The highly wettable road modified asphalt according to claim 1, Features: The mineral filler is clay.

5. The highly wettable road modified asphalt according to claim 1, Features: The raw materials for preparation include 64% of base asphalt, 24% of mineral filler, 11.5% of modifier and 0.5% of additive, and the above percentages are by mass.

6. The highly wettable road modified asphalt according to claim 1, Features: The raw materials for preparation include 64% of base asphalt, 26% of mineral filler, 9.5% of modifier and 0.5% of additive, and the above percentages are by mass.

7. An application of the highly wettable road modified asphalt according to any one of claims 1 to 4, Features: Modified asphalt is prepared with different contents of resin modifier and mineral filler. When paving, at least 2 to 3 asphalt layers are laid and stacked to form a road surface. From bottom to top, the content of resin modifier decreases and the content of mineral filler increases.

8. Application of the highly wettable road modified asphalt according to claim 7, Features: The thickness of the lower layer of two adjacent asphalt layers is 1.2 times that of the upper layer.