Preparation method and application of ground calcium carbonate based on multiple surface components
By grafting functional group molecules on the surface of calcium carbonate and self-assembling with degradable resin molecules, a multi-component modified calcium carbonate is formed, which solves the problem of poor dispersion and compatibility in biodegradable plastics and improves the mechanics of composite materials. performance and reduced production costs.
Patent Information
- Application Number
- CN202410665008.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-27
- Publication Date
- 2024-10-01
AI Technical Summary
Heavy calcium carbonate has poor dispersion and compatibility in biodegradable plastics, resulting in a limited application range in composite materials. Moreover, existing modification methods have physical mixing disadvantages, making it difficult to effectively improve its incorporation into polymer matrices. Miscellaneous amount.
Through molecular self-assembly technology, different functional functional group molecules are grafted on the surface of calcium carbonate, and multi-functional surface modification is performed using acrylic maleic acid copolymer, polyethylene glycol and glycidyl methacrylate to form multi-functional modified calcium carbonate (PMPG-C). ), self-assembles with degradable resin PBAT or PLA molecules to form a highly uniform organic-inorganic composite material.
It significantly improves the dispersion and compatibility of calcium carbonate in biodegradable plastics, breaks through the drawbacks of physical mixing, improves the mechanical properties of composite materials, and reduces production costs.
Smart Images

Figure CN118725610A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biodegradable plastic polymer materials, and in particular to a preparation method and application of heavy calcium carbonate based on surface multi-components. Background Art
[0002] Calcium carbonate (CaCO3) is one of the most commonly used inorganic fillers in plastics, rubber, coatings, adhesives, papermaking industry, thermosetting resins, etc., and has received extensive attention in plastic applications due to its low cost, high yield and significant improvement in the properties of polymers, such as Young's modulus, tensile strength and heat deflection temperature, etc. However, due to its large specific surface area and high surface energy, it is easy to agglomerate, resulting in poor dispersibility in hydrophobic polymer matrices. In addition, the weak interfacial interaction between CaCO3 particles and the polymer body may also lead to significant phase separation, thereby significantly affecting the performance of the composite material, and then resulting in the fact that the actual application range of CaCO3 is not large. At present, the surface modification and in-situ polymerization of CaCO3 particles are considered to be two methods that are more practical commercially. For surface modification, hydrophobic low molecular weight modifiers such as stearic acid, oleic acid, palmitic acid, silane coupling agents, titanate coupling agents, etc. and surfactants are the most convenient and widely used modifiers. In the process of surface modification, hydrophobic organic molecules are attached to the mineral surface, thereby significantly reducing the surface energy of calcium carbonate particles. In the case of in-situ polymerization, hydrophilic inorganic particles are usually dispersed into the grafted monomers, and then the small molecule monomers are directly polymerized to form macromolecules, thereby improving the dispersibility of CaCO3. However, the modified CaCO3 particles still have weak interfacial adhesion with the polymer matrix, that is, the force between the polymer chains and the small molecules attached to the surface of CaCO3 is not enough to obtain a thermodynamically stable and uniform composite material system.
[0003] After searching, several patent documents related to modified calcium carbonate were found. Among them, the Chinese patent with patent application number CN202310410755.8 provides a method for modifying calcium carbonate for biodegradable plastics by using 1000-2500 mesh calcium carbonate and sequentially adding coupling agents, chain extenders, plasticizers and other additives during high temperature and high-speed stirring. The Chinese patent with patent application number CN202211034207.1 provides a method of using an in-situ encapsulation technology to use an aqueous sodium methyl silicate solution or an aqueous potassium methyl silicate solution and a carbonate compound as a film-forming aid to achieve organic modification of the surface of calcium carbonate. At present, there are many methods for modifying CaCO3, but there are not many reports on grafting functional group molecules with different functions on the surface of heavy calcium carbonate materials through molecular self-assembly nano-modification technology.
[0004] Therefore, how to improve the dispersibility of heavy calcium carbonate particles in the polymer matrix and the affinity between the particles and the matrix through molecular self-assembly technology so that the doping amount of calcium carbonate in the biodegradable plastic is higher and the cost is reduced is a problem that needs to be solved at present. Summary of the invention
[0005] The present invention provides a preparation method of heavy calcium carbonate based on surface multi-components and its application. Functional group molecules with different functions are grafted onto the surface of calcium carbonate materials so that calcium carbonate can react with biodegradable resin (PBAT, PLA) molecules through self-assembly and bond to form highly uniform organic-inorganic composite materials, thus overcoming the disadvantages caused by physical mixing, thereby increasing the effective addition amount of calcium carbonate and achieving the purpose of reducing the production cost of biodegradable plastic products.
[0006] A preparation method of heavy calcium carbonate based on surface multi-components, the steps are as follows:
[0007] (1) Calcium carbonate powder is dried for standby use;
[0008] (2) Add the dried calcium carbonate powder to a mixed solution of ethanol and water, the mass ratio of the calcium carbonate powder to the mixed solution of ethanol and water is 1:5-6, and mechanically stir at high temperature for 30 minutes:
[0009] (3) preparing aqueous solutions of acrylic acid-maleic acid copolymers with different contents and adding them to the above solution, and stirring for 1 hour;
[0010] (4) Add polyethylene glycol aqueous solutions with different contents into the above solution and continue stirring for 1 h;
[0011] (5) preparing a mixed solution of glycidyl methacrylate with different contents, adding it to the above reaction solution, and maintaining the same temperature and stirring for 1 hour;
[0012] (6) The mixed solution after the reaction is filtered, dried, and ground to obtain multi-modified calcium carbonate (PMPG-C).
[0013] Furthermore, in step (1), the calcium carbonate powder used is heavy calcium carbonate powder that has not been subjected to any treatment.
[0014] Furthermore, in step (2), the mass ratio of the mixed solution of ethanol and water is 6:4 or 7:3, the reaction temperature is 80-100° C., and the rotation speed is 300-450 r / min.
[0015] Furthermore, in step (3), the mass fraction of the acrylic acid-maleic acid copolymer aqueous solution is 0.5%-2%:
[0016] Furthermore, in step (4), the polyethylene glycol is polyethylene glycol 400 and the mass fraction of its aqueous solution is 0.5%-1.5%.
[0017] Furthermore, in step (5), the solvent in the glycidyl methacrylate mixed solution is anhydrous ethanol, and the solute mass fraction thereof is 0.5%-2%, and the above mass fraction is calculated relative to the total mixed solution.
[0018] Furthermore, in step (6), the suction filtration is repeatedly washed with deionized water and anhydrous ethanol.
[0019] Furthermore, in step (6), the drying temperature is 60° C. vacuum drying, and the drying time is 12 hours to obtain modified calcium carbonate.
[0020] The present invention also provides an application of heavy calcium carbonate based on surface multi-components obtained by the above preparation method, and the modified calcium carbonate and a degradable resin are used to prepare a film, and the steps are:
[0021] The film prepared by modified calcium carbonate and biodegradable resin was dried in a vacuum drying oven for 2 hours;
[0022] The modified calcium carbonate (10-30wt%) and the biodegradable resin (PBAT:PLA=6:4), 1 part of a chain extender, and 1 part of a mixed antioxidant of antioxidant 1076 and antioxidant 626 were uniformly mixed, melt-extruded, drawn, air-cooled, granulated, and dried by a twin-screw extruder to obtain a modified heavy calcium carbonate-filled MPG-C / PBAT / PLA composite film.
[0023] Furthermore, the degradable resin is PBAT or PLA.
[0024] Compared with the prior art, the present invention has the following advantages:
[0025] (1) The present invention utilizes molecular self-assembly technology to graft different functional groups onto calcium carbonate to achieve the purpose of modification. The calcium carbonate is subjected to multi-element surface modification by using acrylic acid maleic acid copolymer, polyethylene glycol, and glycidyl methacrylate. Compared with directly mixing unmodified calcium carbonate with a polymer, the present invention solves the problem of poor compatibility and dispersibility of heavy calcium carbonate in biodegradable plastics, thereby better integrating the two, further overcoming the disadvantages caused by physical mixing, and further improving the mechanical properties of the composite material.
[0026] (2) The synthesis method of the present invention is simple to operate, the raw materials are cheap and readily available, the reaction time is short, the speed is fast, and no complicated and expensive instruments and cumbersome operation steps are required to obtain the required multi-modified calcium carbonate - MPG-C, which can be used as a polymer biodegradable material and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1The XRD pattern of the modified calcium carbonate provided in Example 1 of the present invention;
[0028] Figure 2 The infrared spectrum of the modified calcium carbonate provided in Example 1 of the present invention;
[0029] Figure 3 This is the SEM spectrum of the biodegradable film doped with modified calcium carbonate prepared in Comparative Example 1;
[0030] Figure 4 This is the SEM image of the modified calcium carbonate provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0031] The present invention is further described in detail below through specific embodiments in combination with drawings, but the embodiments of the present invention are not limited thereto.
[0032] It should be noted that, unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods:
[0033] Embodiment 1:
[0034] A method for preparing heavy calcium carbonate based on surface multi-components comprises the following steps:
[0035] (1) Add 50 g of heavy calcium carbonate powder to 300 ml of ethanol aqueous solution, stir at high temperature in a glass reactor capable of condensation and reflux, wherein the mass ratio of ethanol to water is 7:3, and after ultrasonic dispersion, heat to 100° C. and heat and stir for 30 min;
[0036] (2) dissolving 0.5 wt % of acrylic acid-maleic acid copolymer in 10 ml of deionized water, performing ultrasonic dispersion, and dropping the mixture into the above solution, stirring and reacting for 1 h;
[0037] (3) 0.5 wt % polyethylene glycol 400 was dissolved in 10 ml of deionized water, and after ultrasonic dispersion, it was added to the above solution and the reaction was continued with stirring for 1 h;
[0038] (4) Dissolve 0.5 wt % of glycidyl methacrylate in 10 ml of anhydrous ethanol, dissolve under ultrasonication, and then add to the above solution, stirring and reacting for 1 h;
[0039] (5) The mixed solution after the reaction was filtered and repeatedly washed with anhydrous ethanol and deionized water, dried in a vacuum drying oven at 60° C. for 12 h, and then ground to obtain 0.5% modified calcium carbonate:
[0040] Embodiment 2:
[0041] (1) 50 g of heavy calcium carbonate powder was added to 300 ml of ethanol-water solution, and stirred at high temperature in a glass reactor capable of condensation and reflux, wherein the mass ratio of ethanol to water was 7:3. After ultrasonic dispersion, the temperature was raised to 100° C. and heated and stirred for 30 min.
[0042] (2) dissolving 1 wt % of acrylic acid-maleic acid copolymer in 10 ml of deionized water, performing ultrasonic dispersion, and dropping the mixture into the above solution, stirring and reacting for 1 h;
[0043] (3) 0.5 wt % polyethylene glycol 400 was dissolved in 10 ml of deionized water, and after ultrasonic dispersion, it was added to the above solution and the reaction was continued with stirring for 1 h;
[0044] (4) Dissolve 0.5 wt % of glycidyl methacrylate in 10 ml of anhydrous ethanol, dissolve under ultrasonication, and then add to the above solution, stirring and reacting for 1 h;
[0045] (5) The mixed solution after the reaction was filtered and repeatedly washed with anhydrous ethanol and deionized water, and then dried in a vacuum drying oven at 60° C. for 12 h and ground to obtain 1% modified calcium carbonate.
[0046] Comparative Example 1:
[0047] (1) Dry the unmodified calcium carbonate and biodegradable resin (PBAT, PLA) in a vacuum drying oven for 2 h.
[0048] (2) unmodified calcium carbonate, PBAT, 1 part of chain extender, 1 part of antioxidant 1076 and antioxidant 626 were mixed uniformly, melt-extruded, stretched, air-cooled, granulated and dried by a twin-screw extruder to obtain an unmodified heavy calcium carbonate-filled CaCO3 / PBAT / PLA composite film;
[0049] Comparative Example 2:
[0050] (1) Drying the modified calcium carbonate and biodegradable resin (PBAT, PLA) prepared in the above example in a vacuum drying oven for 2 h;
[0051] (2) After the modified calcium carbonate (MPG-C), PLA, 1 part of chain extender, 1 part of antioxidant 1076 and antioxidant 626 are uniformly mixed, melt-extruded, stretched, air-cooled, granulated, and dried by a twin-screw extruder to obtain a modified heavy calcium carbonate filled MPG-C / PBAT / PLA composite film;
[0052] Depend on Figure 3 It can be seen that the multi-component modified calcium carbonate prepared by the method of the present invention can significantly improve the dispersibility of calcium carbonate in the polymer after being added to the biodegradable plastic film, and the obtained composite film has good mechanical properties. Figure 4It can be seen that the particle size of the modified calcium carbonate becomes significantly finer, and the small particles on the surface indicate that the surface functional groups have been successfully grafted.
[0053] Finally, it should be noted that the above embodiments do not limit the present invention in any form. For those skilled in the art, some modifications and improvements can be made to the present invention. Therefore, any modification or improvement made without departing from the spirit of the present invention belongs to the scope of protection claimed in the present invention.
Claims
1. A method for preparing heavy calcium carbonate based on surface multi-components, characterized in that: Here are the steps: (1) Calcium carbonate powder is dried for standby use; (2) adding the dried calcium carbonate powder to a mixed solution of ethanol and water, wherein the mass ratio of the calcium carbonate powder to the mixed solution of ethanol and water is 1:5-6, and mechanically stirring at high temperature for 30 minutes; (3) preparing aqueous solutions of acrylic acid-maleic acid copolymers with different contents and adding them to the above solution, and stirring for 1 hour; (4) Add polyethylene glycol aqueous solutions with different contents into the above solution and continue stirring for 1 h; (5) preparing a mixed solution of glycidyl methacrylate with different contents, adding it to the above reaction solution, and maintaining the same temperature and stirring for 1 hour; (6) The mixed solution after the reaction is filtered, dried, and ground to obtain multi-modified calcium carbonate (PMPG-C).
2. The method for preparing heavy calcium carbonate based on surface multi-components according to claim 1, characterized in that: In step (1), the calcium carbonate powder used is heavy calcium carbonate powder that has not been subjected to any treatment.
3. The method for preparing heavy calcium carbonate based on surface multi-components according to claim 1, characterized in that: In step (2), the mass ratio of the mixed solution of ethanol and water is 6:4 or 7:3, the reaction temperature is 80-100° C., and the rotation speed is 300-450 r / min.
4. The method for preparing heavy calcium carbonate based on surface multi-components according to claim 1, characterized in that: In step (3), the mass fraction of the acrylic acid-maleic acid copolymer aqueous solution is 0.5%-2%.
5. The method for preparing heavy calcium carbonate based on surface multi-components according to claim 1, characterized in that: In step (4), the polyethylene glycol is polyethylene glycol 400 and the mass fraction of its aqueous solution is 0.5%-1.5%.
6. The method for preparing heavy calcium carbonate based on surface multi-components according to claim 1, characterized in that: In step (5), the solvent in the glycidyl methacrylate mixed solution is anhydrous ethanol, and the solute mass fraction thereof is 0.5%-2%, and the above mass fraction is calculated relative to the total mixed solution.
7. The method for preparing heavy calcium carbonate based on surface multi-components according to claim 1, characterized in that: In step (6), the suction filtration is repeatedly washed with deionized water and anhydrous ethanol.
8. The method for preparing heavy calcium carbonate based on surface multi-components according to claim 1, characterized in that: In step (6), the drying temperature is 60° C. in vacuum drying, and the drying time is 12 h to obtain modified calcium carbonate.
9. An application of heavy calcium carbonate based on surface multi-components, characterized in that: The heavy calcium carbonate is obtained by the preparation method of heavy calcium carbonate based on surface multi-components according to any one of claims 1 to 8, and the modified calcium carbonate and the degradable resin are prepared into a film, the steps of which are: The film prepared by modified calcium carbonate and biodegradable resin was dried in a vacuum drying oven for 2 hours; The modified calcium carbonate and the biodegradable resin, 1 part of chain extender, 1 part of antioxidant 1076 and a mixed antioxidant of antioxidant 626 were uniformly mixed, melt-extruded, stretched, air-cooled, granulated and dried by a twin-screw extruder to obtain a modified heavy calcium carbonate filled MPG-C / PBAT / PLA composite film.
10. The use of heavy calcium carbonate based on surface multi-components according to claim 9, characterized in that: The degradable resin is PBAT or PLA.
Citation Information
Patent Citations
In-situ surface coated modified calcium carbonate filler as well as preparation method and application thereof
CN115386247A
Modified calcium carbonate for biodegradable plastic and preparation method thereof
CN116376113A