Water-resistant heat-resistant thermosensitive anti-forgery ink and preparation method thereof

By polymerizing and fixing inorganic fillers in polyimide, it solves the problem of insufficient water resistance and heat resistance of thermal anti-counterfeiting ink in high humidity and high temperature environments, achieves uniform dispersion and improved compatibility of the ink, and significantly improves its performance and printability.

CN118725637AInactive Publication Date: 2024-10-01JIANGSU TANGCAI PRINTING INK SCI TECH CO LTD

Patent Information

Application Number
CN202410886351.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When used in high-humidity and high-temperature environments, existing thermal anti-counterfeiting inks have insufficient water resistance and heat resistance, resulting in blurred, falling off or failure of writing, and the agglomeration of inorganic fillers affects their performance.

Method used

By polymerizing and fixing inorganic fillers in polyimide to avoid agglomeration and improve its compatibility with the resin substrate, water-resistant and heat-resistant thermal anti-counterfeiting inks are prepared, including polyimide resin, epoxy resin, Modified inorganic fillers, thermochromic colorants, dispersants, antioxidants, waterproofing agents and UV absorbers.

Benefits of technology

Significantly improves the water resistance and heat resistance of the ink, ensures even dispersion of inorganic fillers, good compatibility, and good printability, extending the service life of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725637A_ABST
    Figure CN118725637A_ABST
Patent Text Reader

Abstract

The invention provides water-resistant and heat-resistant thermosensitive anti-forgery ink. The water-resistant and heat-resistant thermosensitive anti-forgery ink is prepared from the following components in parts by weight: 20-30 parts of polyimide resin, 10-20 parts of epoxy resin, 3-8 parts of modified inorganic filler, 5-15 parts of a thermochromic material, 0.3-0.8 part of a dispersing agent, 0.1-0.3 part of an antioxidant, 1-2 parts of a waterproof agent, 0.2-0.5 part of an ultraviolet light absorber and 30-45 parts of a solvent, wherein the modified inorganic filler is a product obtained by modifying an inorganic filler with polyimide, and the inorganic filler is polymerized and fixed in the polyimide, so that the agglomeration of the inorganic filler is avoided, the compatibility of the inorganic filler and the resin base material is improved, and the dispersity of the inorganic filler is improved. The ink disclosed by the invention is uniform in system component dispersion, good in compatibility, resistant to high temperature and water, excellent in ink performance and good in printability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of anti-counterfeiting inks, and in particular to a water-resistant and heat-resistant thermosensitive anti-counterfeiting ink and a preparation method thereof. Background Art

[0002] Thermal-sensitive anti-counterfeiting ink uses a colorant whose color changes with temperature. It can display or hide colors or patterns through temperature changes, thereby verifying the authenticity of items. Therefore, thermal-sensitive anti-counterfeiting ink is widely used in a variety of printed materials.

[0003] In addition to being used in a normal dry room temperature environment, some printed materials also need to be used in a high humidity environment or come into direct contact with water, such as some food packaging, beverage bottle labels, toiletries packaging, etc. In this case, if the ink has poor water resistance, the writing and patterns will be blurred, or even faded or peeled off.

[0004] Some printed materials also need to be used at high temperatures. For example, food and drug packaging materials need to be sterilized at high temperatures. If the ink has poor high temperature resistance, the ink will not change color or will become ineffective, thus failing to achieve the anti-counterfeiting purpose. At the same time, poor high temperature resistance will also cause the ink to fall off and age, affecting the appearance and service life of the product.

[0005] The heat resistance and water resistance of ink can be improved by adding inorganic fillers. However, due to their high specific surface area and high surface energy, inorganic fillers are prone to agglomeration and cannot play an effective role, resulting in a decrease in the heat resistance and water resistance of ink, and may also affect the printability of ink. Summary of the invention

[0006] The purpose of the present invention is to provide a water-resistant and heat-resistant thermosensitive anti-counterfeiting ink and a preparation method thereof in view of the deficiencies in the prior art. By polymerizing and fixing inorganic fillers in polyimide, agglomeration of the inorganic fillers is avoided and the compatibility with the resin substrate is improved, thereby improving the dispersibility of the inorganic fillers, enabling the inorganic fillers to play an effective role, and improving the water resistance and heat resistance of the thermosensitive anti-counterfeiting ink.

[0007] According to a first aspect of the present invention, there is provided a water-resistant and heat-resistant thermosensitive anti-counterfeiting ink, comprising the following components in parts by weight: 20-30 parts of a polyimide resin, 10-20 parts of an epoxy resin, 3-8 parts of a modified inorganic filler, 5-15 parts of a thermochromic material, 0.3-0.8 parts of a dispersant, 0.1-0.3 parts of an antioxidant, 1-2 parts of a waterproofing agent, 0.2-0.5 parts of an ultraviolet absorber, and 30-45 parts of a solvent;

[0008] The modified inorganic filler is a product obtained by modifying an inorganic filler with polyimide. The inorganic filler is polymerized and fixed in the polyimide, thereby avoiding agglomeration of the inorganic filler, improving the compatibility of the inorganic filler with the resin substrate, and improving the dispersibility of the inorganic filler.

[0009] Furthermore, the modified inorganic filler is obtained by the following preparation method:

[0010] A1: Dissolve the dianhydride and diamine monomers in DMF respectively, and then mix them evenly under stirring to obtain a first mixed solution;

[0011] A2: Adding an inorganic filler to the first mixed solution and continuing to stir evenly to obtain a second mixed solution;

[0012] A3: The second mixed solution is subjected to a condensation reaction under heating and stirring conditions. After the reaction is completed, the reaction solution is cooled to room temperature, a precipitate is separated, and the precipitate is washed;

[0013] A4: The washed precipitate is placed in a nitrogen atmosphere and heated to the required temperature to carry out a cyclization reaction to obtain a modified inorganic filler.

[0014] Furthermore, the dianhydride is pyromellitic dianhydride, and the diamine monomer is p-phenylenediamine.

[0015] Furthermore, the molar ratio of the pyromellitic anhydride to p-phenylenediamine is (1-1.03):1

[0016] Furthermore, the total mass of the dianhydride and diamine monomers accounts for 20-30% of the mass of the inorganic filler.

[0017] Furthermore, the temperature of the condensation reaction is 80-120°C; the temperature of the cyclization reaction is increased to 200-250°C at a rate of 5-10°C / min.

[0018] Furthermore, the inorganic filler in the modified inorganic filler includes nano-alumina and nano-silicon dioxide.

[0019] Furthermore, the mass ratio of the nano-alumina to the nano-silicon dioxide is (2-5):(1-3).

[0020] Furthermore, the temperature-changing color material is an inorganic and / or organic temperature-changing color material.

[0021] According to a second aspect of the present invention, there is provided a method for preparing the aforementioned water-resistant and heat-resistant thermosensitive anti-counterfeiting ink, comprising the following steps:

[0022] S1: weighing raw materials according to weight proportions and modifying the inorganic filler;

[0023] S2: uniformly mixing the polyimide resin, epoxy resin and solvent, adding the modified inorganic filler, and continuing to stir uniformly to obtain a first mixed solution;

[0024] S3: adding the thermochromic dye to the first mixed solution, mixing evenly, and ball-milling to a fineness of ≤15 μm to obtain a second mixed solution;

[0025] S4: adding a dispersant, an antioxidant, a water-proofing agent and an ultraviolet absorber to the second mixed solution in sequence, stirring the mixture evenly, and obtaining a water-resistant and heat-resistant thermosensitive anti-counterfeiting ink.

[0026] Compared with the prior art, the present invention has the following significant beneficial effects:

[0027] The water-resistant and heat-resistant thermosensitive anti-counterfeiting ink of the present invention modifies the inorganic filler. In the process of polyimide polymerization, the inorganic filler is introduced so that the inorganic filler is polymerized and fixed in the cavities formed by the polyimide, thereby avoiding the agglomeration of the inorganic filler. In addition, the polyimide polymerized on the surface of the inorganic filler has better compatibility with the resin substrate, thereby improving the compatibility of the inorganic material with the resin substrate and the dispersibility of the inorganic filler. The inorganic filler is evenly dispersed in the system without agglomeration, thereby effectively playing a role and improving the water resistance and heat resistance of the ink.

[0028] The water-resistant and heat-resistant thermosensitive anti-counterfeiting ink of the present invention has uniformly dispersed system components, good compatibility, excellent ink performance and good printability. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The present invention is a process flow chart of the water-resistant and heat-resistant thermosensitive anti-counterfeiting ink. DETAILED DESCRIPTION

[0030] In order to better understand the technical content of the present invention, specific embodiments are given and described as follows in conjunction with the accompanying drawings.

[0031] Various aspects of the present invention are described in this disclosure with reference to the accompanying drawings, in which many illustrative embodiments are shown. The embodiments of the present disclosure are not necessarily intended to include all aspects of the present invention. It should be understood that the various concepts and embodiments introduced above, as well as those described in more detail below, can be implemented in any of many ways.

[0032] In an exemplary embodiment of the present invention, a water-resistant and heat-resistant thermosensitive anti-counterfeiting ink is provided, comprising the following components in parts by weight: 20-30 parts of a polyimide resin, 10-20 parts of an epoxy resin, 3-8 parts of a modified inorganic filler, 5-15 parts of a thermochromic material, 0.3-0.8 parts of a dispersant, 0.1-0.3 parts of an antioxidant, 1-2 parts of a waterproofing agent, 0.2-0.5 parts of an ultraviolet absorber, and 30-45 parts of a solvent;

[0033] The modified inorganic filler is a product obtained by modifying the inorganic filler with polyimide. The inorganic filler is polymerized and fixed in the polyimide, thereby avoiding agglomeration of the inorganic filler, improving the compatibility of the inorganic filler with the resin substrate, and improving the dispersibility of the inorganic filler.

[0034] As a preferred embodiment, the modified inorganic filler is obtained by the following preparation method:

[0035] A1: Dissolve the dianhydride and diamine monomers in DMF respectively, and then mix them evenly under stirring to obtain a first mixed solution;

[0036] A2: Adding an inorganic filler to the first mixed solution and continuing to stir evenly to obtain a second mixed solution;

[0037] A3: The second mixed solution is subjected to a condensation reaction under heating and stirring conditions. After the reaction is completed, the reaction solution is cooled to room temperature, a precipitate is separated, and the precipitate is washed;

[0038] A4: The washed precipitate is placed in a nitrogen atmosphere and heated to the required temperature to carry out a cyclization reaction to obtain a modified inorganic filler.

[0039] As a preferred embodiment, the dianhydride is pyromellitic dianhydride (PMDA), and the diamine monomer is p-phenylenediamine (PPD).

[0040] As a preferred embodiment, the molar ratio of pyromellitic dianhydride to p-phenylenediamine is (1-1.03): 1

[0041] As a preferred embodiment, the total mass of the dianhydride and diamine monomers accounts for 20-30% of the mass of the inorganic filler.

[0042] As a preferred embodiment, the temperature of the condensation reaction is 80-120°C; the temperature of the cyclization reaction is increased to 200-250°C at a rate of 5-10°C / min.

[0043] As a preferred embodiment, the inorganic filler in the modified inorganic filler includes nano-alumina and nano-silicon dioxide.

[0044] In a more preferred embodiment, the average particle size of nano-alumina is 50-100 nm, and the average particle size of nano-silicon dioxide is 50-100 nm.

[0045] As a preferred embodiment, the mass ratio of nano-alumina to nano-silicon dioxide is (2-5):(1-3).

[0046] As a preferred embodiment, the temperature-changing colorant is an inorganic and / or organic temperature-changing colorant, and the required colorant can be purchased directly from the market as needed, and no further limitation is made here.

[0047] As a preferred embodiment, the solvent includes ethanol, which is used to adjust the viscosity and dryness of the ink. Other solvents, such as isopropanol, n-butanol, ethyl acetate, etc., may also be added as needed.

[0048] As a preferred embodiment, the waterproofing agent is a silicon-based waterproofing agent, for example, SF-932, HY-903, etc.

[0049] As a preferred embodiment, the dispersant is Disponer 983, the antioxidant is a hindered phenol antioxidant, and the ultraviolet absorber is UV-531.

[0050] It can be understood that the dispersant, antioxidant, water-repellent and ultraviolet absorber in the present invention include but are not limited to the above-mentioned types, and can be selected according to actual needs.

[0051] Combination Figure 1 As shown, in another exemplary embodiment of the present invention, a method for preparing the aforementioned water-resistant and heat-resistant thermosensitive anti-counterfeiting ink is also provided, comprising the following steps:

[0052] S1: weighing raw materials according to weight proportions and modifying the inorganic filler;

[0053] S2: uniformly mixing the polyimide resin, epoxy resin and solvent, adding the modified inorganic filler, and continuing to stir uniformly to obtain a first mixed solution;

[0054] S3: adding the thermochromic dye to the first mixed solution, mixing evenly, and ball-milling to a fineness of ≤15 μm to obtain a second mixed solution;

[0055] S4: adding a dispersant, an antioxidant, a water-proofing agent and an ultraviolet absorber to the second mixed solution in sequence, stirring the mixture evenly, and obtaining a water-resistant and heat-resistant thermosensitive anti-counterfeiting ink.

[0056] For better understanding, the present invention is further described below in conjunction with several specific examples, but the preparation process is not limited thereto, and the content of the present invention is not limited thereto.

[0057] Unless otherwise specified, the materials in the examples were prepared according to existing methods or directly purchased from the market.

[0058] The inorganic fillers used in the following examples and comparative examples are nano-alumina (average particle size of 50-100 nm) and nano-silicon dioxide (average particle size of 50-100 nm) in a mass ratio of 2:1;

[0059] The thermochromic material is an inorganic thermochromic material, the dispersant is Disponer 983, the antioxidant is antioxidant 1010, the waterproofing agent is SF-932, the ultraviolet absorber is UV-531, and the solvent is ethanol.

[0060] The modified inorganic filler is obtained by the following preparation method:

[0061] A1: Dissolve pyromellitic anhydride and p-phenylenediamine (molar ratio of 1.02:1) in DMF respectively, and then stir at 300 rpm for 30 min to mix evenly to obtain a first mixed solution.

[0062] A2: Add inorganic filler (the total mass of pyromellitic dianhydride and p-phenylenediamine accounts for 30% of the mass of the inorganic filler) to the first mixed solution, and continue stirring at a rotation speed of 300 rpm for 30 minutes to obtain a second mixed solution.

[0063] A3: The second mixed solution was stirred at 90° C. and 300 rpm for 6 h. After the reaction, the reaction solution was cooled to room temperature, the precipitate was separated, and the precipitate was washed.

[0064] A4: The washed precipitate was placed in a nitrogen atmosphere, heated to 200° C. at a rate of 5° C. / min and reacted for 1 h to obtain a modified inorganic filler.

[0065] Example 1

[0066] 20 parts of polyimide resin, 10 parts of epoxy resin, 3 parts of modified inorganic filler, 5 parts of thermochromic material, 0.3 parts of dispersant, 0.1 parts of antioxidant, 1 part of waterproofing agent, 0.2 parts of ultraviolet absorber and 30 parts of solvent.

[0067] S1: Weigh the raw materials according to their weight proportions, mix the polyimide resin, epoxy resin and solvent, and stir at a rotation speed of 300 rpm for 30 min, then add the modified inorganic filler, and continue to stir at a rotation speed of 300 rpm for 30 min to obtain a first mixed solution.

[0068] S2: adding the thermochromic dye to the first mixed solution, stirring at a rotation speed of 300 rpm for 30 min, and ball-milling to a fineness of ≤15 μm to obtain a second mixed solution.

[0069] S3: adding a dispersant, an antioxidant, a water-proofing agent and an ultraviolet absorber to the second mixed solution in sequence, stirring at a rotation speed of 300 rpm for 60 minutes, and obtaining a water-resistant and heat-resistant thermosensitive anti-counterfeiting ink.

[0070] Example 2

[0071] 30 parts of polyimide resin, 20 parts of epoxy resin, 8 parts of modified inorganic filler, 15 parts of thermochromic material, 0.8 parts of dispersant, 0.3 parts of antioxidant, 2 parts of waterproofing agent, 0.5 parts of ultraviolet absorber and 45 parts of solvent.

[0072] S1: Weigh the raw materials according to their weight proportions, mix the polyimide resin, epoxy resin and solvent, and stir at a rotation speed of 300 rpm for 30 min, then add the modified inorganic filler, and continue to stir at a rotation speed of 300 rpm for 30 min to obtain a first mixed solution.

[0073] S2: adding the thermochromic dye to the first mixed solution, stirring at a rotation speed of 300 rpm for 30 min, and ball-milling to a fineness of ≤15 μm to obtain a second mixed solution.

[0074] S3: adding a dispersant, an antioxidant, a water-proofing agent and an ultraviolet absorber to the second mixed solution in sequence, stirring at a rotation speed of 300 rpm for 60 minutes, and obtaining a water-resistant and heat-resistant thermosensitive anti-counterfeiting ink.

[0075] Example 3

[0076] 25 parts of polyimide resin, 15 parts of epoxy resin, 5 parts of modified inorganic filler, 10 parts of thermochromic material, 0.5 parts of dispersant, 0.2 parts of antioxidant, 2 parts of waterproofing agent, 0.3 parts of ultraviolet absorber, and 40 parts of solvent.

[0077] S1: Weigh the raw materials according to their weight proportions, mix the polyimide resin, epoxy resin and solvent, and stir at a rotation speed of 300 rpm for 30 min, then add the modified inorganic filler, and continue to stir at a rotation speed of 300 rpm for 30 min to obtain a first mixed solution.

[0078] S2: adding the thermochromic dye to the first mixed solution, stirring at a rotation speed of 300 rpm for 30 min, and ball-milling to a fineness of ≤15 μm to obtain a second mixed solution.

[0079] S3: adding a dispersant, an antioxidant, a water-proofing agent and an ultraviolet absorber to the second mixed solution in sequence, stirring at a rotation speed of 300 rpm for 60 minutes, and obtaining a water-resistant and heat-resistant thermosensitive anti-counterfeiting ink.

[0080] Comparative Example 1

[0081] The inorganic filler used in this comparative example is nano-alumina (average particle size of 50-100 nm) and nano-silicon dioxide (average particle size of 50-100 nm) in a mass ratio of 2:1.

[0082] 25 parts of polyimide resin, 15 parts of epoxy resin, 5 parts of modified inorganic filler, 10 parts of thermochromic material, 0.5 parts of dispersant, 0.2 parts of antioxidant, 2 parts of waterproofing agent, 0.3 parts of ultraviolet absorber, and 40 parts of solvent.

[0083] S1: Weigh the raw materials according to their weight proportions, mix the polyimide resin, epoxy resin and solvent, and stir at a rotation speed of 300 rpm for 30 min, then add the inorganic filler, and continue to stir at a rotation speed of 300 rpm for 30 min to obtain a first mixed solution.

[0084] S2: adding the thermochromic dye to the first mixed solution, stirring at a rotation speed of 300 rpm for 30 min, and ball-milling to a fineness of ≤15 μm to obtain a second mixed solution.

[0085] S3: adding a dispersant, an antioxidant, a water-proofing agent and an ultraviolet absorber to the second mixed solution in sequence, stirring at a rotation speed of 300 rpm for 60 minutes, and obtaining a water-resistant and heat-resistant thermosensitive anti-counterfeiting ink.

[0086] Performance Testing

[0087] The performance tests of the thermosensitive anti-counterfeiting inks prepared in Examples 1-3 and Comparative Example 1 were conducted, wherein: High temperature stability test: the inks prepared in the Examples and Comparative Examples were applied to a standard test plate, and the color, glossiness, adhesion and temperature change of the inks on the test plate were observed after baking at 160°C for 48 hours; Immersion test: the inks prepared in the Examples and Comparative Examples were printed on a 5cm×5cm paperboard surface to prepare a sample, and the sample was immersed in water for 48 hours and then the surface condition was observed. The scoring criteria are shown in Table 1;

[0088] Table 1

[0089] 1 point Large area fading and shedding, more than half of the area 2 points Fading and shedding, about half of the area 3 points Obvious fading and shedding, less than half the area 4 points Slight fading and shedding 5 points Basically no fading, basically no shedding

[0090] The test results are shown in Table 2:

[0091] Table 2

[0092]

[0093]

[0094] It can be seen from the above results that the thermosensitive anti-counterfeiting ink prepared by the present invention has excellent water resistance and heat resistance. This is because the present invention adopts a resin substrate with heat and water resistance, and polymerizes and fixes the inorganic filler in the polyimide, thereby avoiding the agglomeration of the inorganic filler and improving the compatibility with the resin substrate, thereby improving the dispersibility of the inorganic filler, allowing the inorganic filler to play an effective role, thereby obtaining excellent water and heat resistance.

[0095] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. A person with ordinary knowledge in the technical field to which the present invention belongs may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be determined by the definition of the claims.

Claims

1. A water-resistant and heat-resistant thermosensitive anti-counterfeiting ink, characterized in that: The invention comprises the following components in parts by weight: 20-30 parts of polyimide resin, 10-20 parts of epoxy resin, 3-8 parts of modified inorganic filler, 5-15 parts of thermochromic material, 0.3-0.8 parts of dispersant, 0.1-0.3 parts of antioxidant, 1-2 parts of waterproofing agent, 0.2-0.5 parts of ultraviolet absorber and 30-45 parts of solvent; The modified inorganic filler is a product obtained by modifying an inorganic filler with polyimide. The inorganic filler is polymerized and fixed in the polyimide, thereby avoiding agglomeration of the inorganic filler, improving the compatibility of the inorganic filler with the resin substrate, and improving the dispersibility of the inorganic filler.

2. The water-resistant and heat-resistant thermosensitive anti-counterfeiting ink according to claim 1, characterized in that: The modified inorganic filler is obtained by the following preparation method: A1: Dissolve the dianhydride and diamine monomers in DMF respectively, and then mix them evenly under stirring to obtain a first mixed solution; A2: Adding an inorganic filler to the first mixed solution and continuing to stir evenly to obtain a second mixed solution; A3: The second mixed solution is subjected to a condensation reaction under heating and stirring conditions. After the reaction is completed, the reaction solution is cooled to room temperature, a precipitate is separated, and the precipitate is washed; A4: The washed precipitate is placed in a nitrogen atmosphere and heated to the required temperature to carry out a cyclization reaction to obtain a modified inorganic filler.

3. The water-resistant and heat-resistant thermosensitive anti-counterfeiting ink according to claim 2, characterized in that: The dianhydride is pyromellitic dianhydride, and the diamine monomer is p-phenylenediamine.

4. The water-resistant and heat-resistant thermosensitive anti-counterfeiting ink according to claim 3, characterized in that: The molar ratio of the pyromellitic dianhydride to p-phenylenediamine is (1-1.03): 1 5. The water-resistant and heat-resistant thermosensitive anti-counterfeiting ink according to claim 2, characterized in that: The total mass of the dianhydride and diamine monomers accounts for 20-30% of the mass of the inorganic filler.

6. The water-resistant and heat-resistant thermosensitive anti-counterfeiting ink according to claim 2, characterized in that: The temperature of the condensation reaction is 80-120°C; the temperature of the cyclization reaction is raised to 200-250°C at a rate of 5-10°C / min.

7. The water-resistant and heat-resistant thermosensitive anti-counterfeiting ink according to claim 1, characterized in that: The inorganic filler in the modified inorganic filler includes nano-alumina and nano-silicon dioxide.

8. The water-resistant and heat-resistant thermosensitive anti-counterfeiting ink according to claim 6, characterized in that: The mass ratio of the nano-alumina to the nano-silicon dioxide is (2-5):(1-3).

9. The water-resistant and heat-resistant thermosensitive anti-counterfeiting ink according to claim 1, characterized in that: The temperature-changing color material is an inorganic and / or organic temperature-changing color material.

10. A method for preparing the water-resistant and heat-resistant thermosensitive anti-counterfeiting ink as claimed in claim 1, characterized in that: The steps include: S1: weighing raw materials according to weight proportions and modifying the inorganic filler; S2: uniformly mixing the polyimide resin, epoxy resin and solvent, adding the modified inorganic filler, and continuing to stir uniformly to obtain a first mixed solution; S3: adding the thermochromic dye to the first mixed solution, mixing evenly, and ball-milling to a fineness of ≤15 μm to obtain a second mixed solution; S4: adding a dispersant, an antioxidant, a water-proofing agent and an ultraviolet absorber to the second mixed solution in sequence, stirring the mixture evenly, and obtaining a water-resistant and heat-resistant thermosensitive anti-counterfeiting ink.

Citation Information

Patent Citations

  • Modified calcium carbonate and preparation method and application thereof

    CN111040252A

  • Conductive carbon nanotube modified polyimide film material and preparation method thereof

    CN111548626A

  • Polyimide resin composition as well as preparation method and application thereof

    CN114517074A

  • Thermal response self-assembly organic material serving as photon ink and preparation method of thermal response self-assembly organic material

    CN116113670A

  • Heat-resistant block copolyimide composition for screen printing use and composition of ink using the polyimide and method of forming coating film

    JP2003113338A

Cited By

  • Heat-insulating anti-corrosion composite coating for roof of industrial factory building and preparation method of heat-insulating anti-corrosion composite coating

    CN119899561A