Photocatalytic coating as well as preparation method and application thereof

By coating the inner surface of the lamp lens with photocatalytic coating and using carbon quantum dot-modified nano-titanium dioxide for photocatalytic reaction, the problem of lamp lens pollution is solved, the light transmittance is improved and the service life is extended, achieving efficient and safe Cleaning effect.

CN118725663AActive Publication Date: 2024-10-01SOUTH CHINA UNIV OF TECH +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410981142.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-01
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Lamp lenses are prone to adhere to oil, dust and other contaminants during long-term use, resulting in a decrease in light transmittance. Traditional cleaning methods are cumbersome and may damage the lens surface, affecting the life of the lamp.

Method used

A photocatalytic coating is used, which consists of a translucent resin and carbon quantum dot-modified nano-titanium dioxide. The carbon quantum dot-modified nano-titanium dioxide is prepared through a hydrothermal reaction, and is mixed with the translucent resin to form a coating. Coated on the inner surface of the lamp lens, it uses photocatalytic reaction to degrade pollutants.

Benefits of technology

It effectively improves the light transmittance of the lamp lens, extends the service life of the lamp, is simple to operate, safe and environmentally friendly, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725663A_ABST
    Figure CN118725663A_ABST
Patent Text Reader

Abstract

The invention discloses a photocatalytic coating as well as a preparation method and application thereof. The photocatalytic coating provided by the invention comprises the following components in percentage by weight: 0.5-2% of light-transmitting resin; 0.5%-2% of carbon quantum dot modified nano titanium dioxide; and 96%-99% of water. The preparation method of the photocatalytic coating comprises the following steps: dissolving the light-transmitting resin in water, adding the carbon quantum dot modified nano titanium dioxide, and uniformly mixing to obtain the photocatalytic coating. The inner surface of a lamp lens is coated with the photocatalytic coating, a coating with a photocatalytic degradation effect can be formed, the coating can degrade oil stains attached to the inner surface of the lamp lens through photocatalytic reaction, the lamp lens can keep high light transmission, and finally the service life of a lamp can be effectively prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photocatalysis, and in particular to a photocatalytic coating and a preparation method and application thereof. Background Art

[0002] Lamp lens is an important part of lamps, and its light transmittance directly affects the lighting effect of lamps. During long-term use of lamps, the inner surface of lamp lenses is prone to oil, dust and other pollutants, which leads to a decrease in light transmittance, which will eventually directly affect the lighting effect of lamps. Traditional lamp lens cleaning methods include manual wiping and chemical cleaning, which are not only cumbersome to operate, but may also damage the lens surface and shorten the service life of the lamp.

[0003] Therefore, it is of great significance to develop a method that is more effective and easier to operate to solve the problem of contamination on the inner surface of the lamp lens. Summary of the invention

[0004] The purpose of the present invention is to provide a photocatalytic coating and a preparation method and application thereof.

[0005] The technical solution adopted by the present invention is:

[0006] A photocatalytic coating comprising the following components in weight percentage:

[0007] Translucent resin: 0.5% to 2%;

[0008] Carbon quantum dot-modified nano-titanium dioxide: 0.5% to 2%;

[0009] Water: 96%~99%.

[0010] Preferably, the light-transmitting resin is at least one of polyvinyl alcohol (PVA), polymethyl methacrylate (PMMA), polycarbonate (PC), polyethylene (PE), polypropylene (PP), polystyrene (PS), and polyurethane (PU).

[0011] Preferably, the number average molecular weight of the polyvinyl alcohol is 10,000 to 100,000.

[0012] Preferably, the number average molecular weight of the polymethyl methacrylate is 50,000 to 500,000.

[0013] Preferably, the number average molecular weight of the polycarbonate is 20,000-200,000.

[0014] Preferably, the number average molecular weight of the polyethylene is 20,000-200,000.

[0015] Preferably, the number average molecular weight of the polypropylene is 30,000 to 300,000.

[0016] Preferably, the number average molecular weight of the polystyrene is 30,000 to 300,000.

[0017] Preferably, the number average molecular weight of the polyurethane is 50,000-500,000.

[0018] Preferably, the weight ratio of nano-titanium dioxide to carbon quantum dots in the carbon quantum dot-modified nano-titanium dioxide is 1:0.05-0.5.

[0019] Preferably, the particle size of the nano-titanium dioxide in the carbon quantum dot-modified nano-titanium dioxide is 20 nm to 100 nm.

[0020] Preferably, the particle size of the carbon quantum dots in the carbon quantum dot-modified nano-titanium dioxide is ≤10 nm.

[0021] Preferably, the carbon quantum dot-modified nano titanium dioxide is prepared by a preparation method comprising the following steps:

[0022] 1) immersing the secondary collagen fibers in an alkaline solution to obtain a secondary collagen fiber extract;

[0023] 2) heating the secondary collagen fiber extract to perform a hydrothermal reaction, and then separating the product to obtain carbon quantum dots;

[0024] 3) Add nano-titanium dioxide and carbon quantum dots into a solvent, mix them thoroughly, and then dry them to obtain nano-titanium dioxide modified with carbon quantum dots.

[0025] Preferably, the secondary collagen fibers in step 1) are recycled collagen fibers made from waste leather by mechanical or chemical methods. The principle of the mechanical method: the fibers are extracted by physical methods, the waste leather is first placed in an opening device for an opening process, a certain amount of auxiliary agent is added, the waste leather is torn to a certain extent, the penetration of the auxiliary agent and the swelling of the waste leather are accelerated, the fiber opening rate is increased, and then the waste leather is placed in a fiber extraction device to obtain secondary collagen fibers; the principle of the chemical method: the hydrolysis reaction equilibrium of the chromium complex will move in the dissociation direction under acidic conditions, and the acid radical will react with the chromium ion to form a complex, which can separate the carboxyl group in the collagen fiber from the chromium complex, thereby obtaining secondary collagen fibers.

[0026] Preferably, the solute in the alkaline solution in step 1) is at least one of sodium hydroxide, potassium hydroxide and calcium hydroxide.

[0027] Preferably, the concentration of the solute in the alkaline solution in step 1) is 0.01 mol / L to 0.05 mol / L.

[0028] Preferably, the immersion treatment in step 1) is carried out at a temperature of 70°C to 100°C and a stirring speed of 400r / min to 600r / min, and the immersion treatment time is 4h to 6h.

[0029] Preferably, the hydrothermal reaction in step 2) is carried out at a temperature of 150° C. to 180° C., and the reaction time is 6 h to 8 h.

[0030] Preferably, the product separation method in step 2) is dialysis, and freeze-drying is performed after dialysis.

[0031] Preferably, the freeze-drying time is 36 h to 48 h.

[0032] Preferably, the mixing method in step 3) is stirring, the stirring speed is 400r / min to 600r / min, and the stirring time is 0.5h to 4h.

[0033] Preferably, the drying in step 3) is carried out at a temperature of 100° C. to 120° C., and the drying time is 4 h to 12 h.

[0034] A method for preparing the photocatalytic coating as described above comprises the following steps:

[0035] The light-transmitting resin is dissolved in water, and then the carbon quantum dot-modified nano-titanium dioxide is added and mixed to obtain the photocatalytic coating.

[0036] A lamp comprises a lens; the inner surface of the lens is covered with a coating made of the above-mentioned photocatalytic paint.

[0037] Preferably, the coating is made by the following method: coating the photocatalytic coating on the inner surface of the lens, followed by drying and UV curing.

[0038] Preferably, the coating method is one of spray coating, dip coating, spin coating, blade coating, and electrophoretic deposition.

[0039] Preferably, the drying is carried out at a temperature of 50° C. to 70° C., and the drying time is 4 h to 12 h.

[0040] Preferably, the UV curing time is 30 min to 60 min.

[0041] The beneficial effect of the present invention is that the photocatalytic coating of the present invention is coated on the inner surface of the lamp lens to form a coating with a photocatalytic degradation effect. The coating can degrade oil stains attached to the inner surface of the lamp lens through a photocatalytic reaction, so that the lamp lens maintains high light transmittance, and ultimately can effectively extend the service life of the lamp.

[0042] Specifically:

[0043] 1) The photocatalytic coating of the present invention is added with nano titanium dioxide modified with carbon quantum dots, and the carbon quantum dots are firmly attached to the surface of nano titanium dioxide particles through chemical modification, which not only improves the light absorption capacity of nano titanium dioxide (for example, expands the light absorption range of nano titanium dioxide; enhances the absorption capacity of nano titanium dioxide in the visible light region), but also improves the separation efficiency of photogenerated carriers (carbon quantum dots can effectively capture and transfer photogenerated electrons, reduce the recombination of electron-hole pairs, and improve the utilization efficiency of photogenerated carriers), enhances the photocatalytic performance of the formed coating, and can more efficiently degrade organic pollutants;

[0044] 2) The photocatalytic coating of the present invention can be used in lamps to give lamp lenses an efficient and lasting oil degradation effect, thereby improving the light transmittance of the lamp lenses and effectively extending the service life of the lamps;

[0045] 3) The photocatalytic coating of the present invention has a simple formula, is safe and environmentally friendly, and does not damage the surface of the lamp lens, and is suitable for large-scale industrial production and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 This is the SEM image of the nano-titanium dioxide in Example 1.

[0047] Figure 2 This is the AFM image of the carbon quantum dots in Example 1.

[0048] Figure 3 This is a graph showing the test results of the grease degradation effect of the coating formed by the photocatalytic coating of Examples 1 to 5 and the comparative example. DETAILED DESCRIPTION

[0049] The present invention will be further explained and illustrated below in conjunction with specific embodiments.

[0050] Embodiment 1:

[0051] A photocatalytic coating, the composition of which is shown in the following table:

[0052] Table 1 Composition of a photocatalytic coating

[0053]

[0054]

[0055] Note:

[0056] The carbon quantum dot-modified nano-titanium dioxide was prepared by the following steps:

[0057] 1) adding 20 g of secondary collagen fibers into 480 mL of a 0.02 mol / L sodium hydroxide solution, and then immersing for 5 h at a temperature of 70° C. and a stirring speed of 400 r / min to obtain a secondary collagen fiber extract;

[0058] 2) The secondary collagen fiber extract was heated to 180°C and reacted for 8 hours, and the product was dialyzed with deionized water for 48 hours, and then freeze-dried at -40°C for 48 hours to obtain carbon quantum dots (CQDs; particle size ≤ 10 nm);

[0059] 3) Add 1 g of nano-titanium dioxide (20 nm to 100 nm) and 0.1 g of carbon quantum dots into 100 mL of deionized water, stir for 30 min at a stirring speed of 400 r / min, and then dry at 100 °C for 6 h to obtain nano-titanium dioxide modified with carbon quantum dots.

[0060] The scanning electron microscope (SEM) image of the nano-titanium dioxide in this embodiment is as follows: Figure 1 As shown in the AFM image of carbon quantum dots Figure 2 shown.

[0061] Depend on Figure 1 It can be seen that the particle size of nano titanium dioxide is 20nm~100nm.

[0062] Depend on Figure 2 It can be seen that the carbon quantum dots are oblate spherical and the particle size is less than 10nm.

[0063] The preparation method of the above-mentioned photocatalytic coating is as follows:

[0064] Polyvinyl alcohol was added into water, and then stirred at a temperature of 70° C. and a stirring speed of 500 r / min until the polyvinyl alcohol was completely dissolved. Then, nano-titanium dioxide modified with carbon quantum dots was added and stirring was continued for 30 minutes to obtain a photocatalytic coating.

[0065] Embodiment 2:

[0066] A photocatalytic coating, the composition of which is shown in the following table:

[0067] Table 2 Composition of a photocatalytic coating

[0068]

[0069] Note:

[0070] The carbon quantum dot-modified nano-titanium dioxide was prepared by the following steps:

[0071] 1 g of nano titanium dioxide (particle size of 20 nm to 100 nm) and 0.05 g of carbon quantum dots (same as in Example 1) were added to 100 mL of deionized water, stirred for 30 min at a stirring speed of 400 r / min, and dried at 100° C. for 6 h to obtain nano titanium dioxide modified with carbon quantum dots.

[0072] The preparation method of the above-mentioned photocatalytic coating is as follows:

[0073] Polyvinyl alcohol was added into water, and then stirred at 80°C and 500 r / min until the polyvinyl alcohol was completely dissolved. Then, nano-titanium dioxide modified with carbon quantum dots was added and stirred for 30 minutes to obtain a photocatalytic coating.

[0074] Embodiment 3:

[0075] A photocatalytic coating, the composition of which is shown in the following table:

[0076] Table 3 Composition of a photocatalytic coating

[0077]

[0078] Note:

[0079] The carbon quantum dot-modified nano-titanium dioxide was prepared by the following steps:

[0080] 1 g of nano titanium dioxide (particle size of 20 nm to 100 nm) and 0.2 g of carbon quantum dots (same as in Example 1) were added to 100 mL of deionized water, stirred for 30 min at a stirring speed of 400 r / min, and dried at 100° C. for 6 h to obtain nano titanium dioxide modified with carbon quantum dots.

[0081] The preparation method of the above-mentioned photocatalytic coating is as follows:

[0082] Polyvinyl alcohol was added into water, and then stirred at a temperature of 90° C. and a stirring speed of 500 r / min until the polyvinyl alcohol was completely dissolved. Then, nano-titanium dioxide modified with carbon quantum dots was added and stirring was continued for 30 minutes to obtain a photocatalytic coating.

[0083] Embodiment 4:

[0084] A photocatalytic coating, the composition of which is shown in the following table:

[0085] Table 4 Composition of a photocatalytic coating

[0086]

[0087] Note:

[0088] The carbon quantum dot-modified nano-titanium dioxide was prepared by the following steps:

[0089] 1 g of nano titanium dioxide (particle size of 20 nm to 100 nm) and 0.15 g of carbon quantum dots (same as in Example 1) were added to 100 mL of deionized water, stirred for 30 min at a stirring speed of 400 r / min, and dried at 100° C. for 6 h to obtain nano titanium dioxide modified with carbon quantum dots.

[0090] The preparation method of the above-mentioned photocatalytic coating is as follows:

[0091] Polyvinyl alcohol was added into water, and then stirred at a temperature of 70° C. and a stirring speed of 500 r / min until the polyvinyl alcohol was completely dissolved. Then, nano-titanium dioxide modified with carbon quantum dots was added and stirring was continued for 30 minutes to obtain a photocatalytic coating.

[0092] Embodiment 5:

[0093] A photocatalytic coating, the composition of which is shown in the following table:

[0094] Table 5 Composition of a photocatalytic coating

[0095]

[0096] Note:

[0097] The carbon quantum dot-modified nano-titanium dioxide was prepared by the following steps:

[0098] 1 g of nano titanium dioxide (particle size of 20 nm to 100 nm) and 0.3 g of carbon quantum dots (same as in Example 1) were added to 100 mL of deionized water, stirred for 30 min at a stirring speed of 400 r / min, and dried at 100° C. for 6 h to obtain nano titanium dioxide modified with carbon quantum dots.

[0099] The preparation method of the above-mentioned photocatalytic coating is as follows:

[0100] Polyvinyl alcohol was added into water, and then stirred at a temperature of 90° C. and a stirring speed of 500 r / min until the polyvinyl alcohol was completely dissolved. Then, nano-titanium dioxide modified with carbon quantum dots was added and stirring was continued for 30 minutes to obtain a photocatalytic coating.

[0101] Comparative Example:

[0102] A photocatalytic coating, the composition of which is shown in the following table:

[0103] Table 6 Composition of a photocatalytic coating

[0104]

[0105]

[0106] The preparation method of the above-mentioned photocatalytic coating is as follows:

[0107] Polyvinyl alcohol was added into water, and then stirred at a temperature of 70° C. and a stirring speed of 500 r / min until the polyvinyl alcohol was completely dissolved. Then, nano titanium dioxide was added and stirring was continued for 30 minutes to obtain a photocatalytic coating.

[0108] Performance Test:

[0109] The photocatalytic coatings of Examples 1 to 5 and the comparative example were uniformly coated (the corresponding coating methods of the photocatalytic coatings of Examples 1 to 5 and the comparative example were spray coating, dip coating, spin coating, scraping coating, electrophoretic deposition and spray coating, respectively) on the clean inner surface of the lamp lens, and then the lens was placed in an oven at 60° C. for 4 hours, and then cured by ultraviolet light for 30 minutes, and then the lens surface covered with the coating was coated with lubricating oil, and then subjected to light treatment under sunlight, and the grease degradation on the lens surface was measured. The test results are shown in the following table (the corresponding grease degradation effect test results are shown in the figure below). Figure 3 shown):

[0110] Table 7 Test results of grease degradation effect of coating formed by photocatalytic coating

[0111]

[0112]

[0113] Note:

[0114] Degradation rate (%) = (initial oil weight - residual oil weight) / initial oil weight × 100%.

[0115] From Table 7 and Figure 3 It can be seen that:

[0116] 1) The coatings formed by the photocatalytic coatings of Examples 1 to 5 all showed high grease degradation efficiency, especially the coating formed by the photocatalytic coating of Example 5, the degradation rate of which reached 90% in 8 hours, while the degradation rate of the coating formed by the photocatalytic coating of the comparative example was only 50% in 8 hours, and the degradation rate was increased by 40%, indicating that the photocatalytic degradation effect of the nano-titanium dioxide modified by carbon quantum dots was significantly better than that of the unmodified nano-titanium dioxide;

[0117] 2) The coatings formed by the photocatalytic coatings of Examples 1 to 5 showed obvious grease degradation effects within the first 4 hours, with degradation rates exceeding 50%, and the grease degradation rates of the coatings formed by the photocatalytic coatings of Examples 1 to 5 in each time period were significantly higher than those of the coatings formed by the photocatalytic coatings of the comparative examples, indicating that the modification effect of carbon quantum dots on nano-titanium dioxide was significant;

[0118] 3) Different coating methods have a significant impact on the degradation effect of the coating, among which the coatings formed by electrophoretic deposition (Example 5) and dip coating (Example 2) show the best degradation performance;

[0119] In summary, the photocatalytic coating of the present invention is coated on the inner surface of the lamp lens to form a coating with a photocatalytic degradation effect. The coating can degrade oil stains attached to the inner surface of the lamp lens through a photocatalytic reaction, thereby enabling the lamp lens to maintain high light transmittance, and ultimately effectively extending the service life of the lamp.

[0120] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A photocatalytic coating, characterized in that: The composition includes the following weight percentages: Translucent resin: 0.5% to 2%; Carbon quantum dot-modified nano-titanium dioxide: 0.5% to 2%; Water: 96%~99%.

2. The photocatalytic coating according to claim 1, characterized in that: The light-transmitting resin is at least one of polyvinyl alcohol, polymethyl methacrylate, polycarbonate, polyethylene, polypropylene, polystyrene, and polyurethane.

3. The photocatalytic coating according to claim 1, characterized in that: The weight ratio of nano-titanium dioxide to carbon quantum dots in the carbon quantum dot-modified nano-titanium dioxide is 1:0.05-0.

5.

4. The photocatalytic coating according to claim 3, characterized in that: The particle size of the nano titanium dioxide in the nano titanium dioxide modified by carbon quantum dots is 20nm-100nm; the particle size of the carbon quantum dots in the nano titanium dioxide modified by carbon quantum dots is ≤10nm.

5. The photocatalytic coating according to any one of claims 1 to 4, characterized in that: The carbon quantum dot-modified nano titanium dioxide is prepared by a preparation method comprising the following steps: 1) immersing the secondary collagen fibers in an alkaline solution to obtain a secondary collagen fiber extract; 2) heating the secondary collagen fiber extract to perform a hydrothermal reaction, and then separating the product to obtain carbon quantum dots; 3) Add nano-titanium dioxide and carbon quantum dots into a solvent, mix them thoroughly, and then dry them to obtain nano-titanium dioxide modified with carbon quantum dots.

6. The photocatalytic coating according to claim 5, characterized in that: The secondary collagen fibers in step 1) are recycled collagen fibers made from waste leather by mechanical or chemical methods; the solute in the alkaline solution in step 1) is at least one of sodium hydroxide, potassium hydroxide, and calcium hydroxide; the concentration of the solute in the alkaline solution in step 1) is 0.01 mol / L to 0.05 mol / L.

7. The photocatalytic coating according to claim 5, characterized in that: Step 1) The immersion treatment is carried out at a temperature of 70°C to 100°C and a stirring speed of 400r / min to 600r / min, and the immersion treatment time is 4h to 6h.

8. The photocatalytic coating according to claim 5, characterized in that: Step 2) The hydrothermal reaction is carried out at a temperature of 150° C. to 180° C., and the reaction time is 6 h to 8 h.

9. A method for preparing a photocatalytic coating as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: The light-transmitting resin is dissolved in water, and then the carbon quantum dot-modified nano-titanium dioxide is added and mixed to obtain the photocatalytic coating.

10. A lamp, characterized in that: The composition comprises a lens; the inner surface of the lens is covered with a coating made of the photocatalytic coating according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Method for improving transparency of LED lamp

    CN101644403A

  • Carbon quantum dot / titanium dioxide composite photocatalytic material and preparation method and application thereof

    CN107876035A

  • Preparation method of CQDs / TiO2 sunlight photocatalyst

    CN107876036A

  • Nano-titanium dioxide sol with visible light activity

    CN109731565A

  • Anti-counterfeiting ink, preparation method thereof, double anti-counterfeiting label and preparation method of double anti-counterfeiting label

    CN117844307A