Preparation method of hydrogen sulfide-resistant anticorrosive paint and coating

Through the coating technology of phenolic epoxy resin and phenolic amine epoxy curing agent combined with fillers, the problem of corrosion of metal materials by hydrogen sulfide is solved, corrosion resistance and wear resistance in high temperature and high pressure environments are achieved, and the service life of oil and gas field facilities is extended. service life.

CN118725686AInactive Publication Date: 2024-10-01CHINA UNIV OF PETROLEUM (EAST CHINA)

Patent Information

Application Number
CN202410955094.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The presence of hydrogen sulfide in oil and gas fields causes damage to metal materials due to electrochemical corrosion and hydrogen embrittlement, threatening the safety of oil and gas field facilities.

Method used

The coating uses phenolic epoxy resin and phenolic amine epoxy curing agent as the main components, combined with fillers such as chromium oxide green, talc powder, barium sulfate, graphite powder, etc., and improves the hardness and adhesion of the coating through efficient stirring and sandblasting. , forming an anti-hydrogen sulfide anti-corrosion coating.

Benefits of technology

It achieves corrosion resistance and wear resistance of the coating in high temperature, high pressure and hydrogen sulfide environments, extends the service life of downhole oil casing and surface carbon steel pipelines, and meets the relevant standard requirements of SY/T6717-2016.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004948517440000011
    Figure HDA0004948517440000011
  • Figure HDA0004948517440000012
    Figure HDA0004948517440000012
  • Figure HDA0004948517440000021
    Figure HDA0004948517440000021
Patent Text Reader

Abstract

The invention relates to a hydrogen sulfide-resistant anticorrosive paint and a preparation method of a coating. The anticorrosive paint is composed of a component A and a component B. The component A comprises novolac epoxy resin, chromium oxide green, talcum powder, barium sulfate, graphite powder, zinc phosphomolybdate, polysiloxane, fluorine modified acrylate and a diluent. And the component B comprises a phenolic aldehyde amine epoxy curing agent and a diluent. By optimizing the formula of the paint, the paint with excellent acid resistance, wear resistance, high temperature resistance and hydrogen sulfide resistance is obtained, and an anticorrosive coating prepared from the paint can effectively solve the problem of corrosion protection of underground oil casings and ground carbon steel pipelines working in a hydrogen sulfide-related environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a liquid anticorrosion paint and a method for preparing a coating, and in particular to a method for preparing a hydrogen sulfide resistant anticorrosion paint and a coating. Background Art

[0002] Hydrogen sulfide is a toxic and harmful gas widely found in natural oil and gas fields. During the development and transportation of hydrogen sulfide-containing oil and gas fields, the hydrogen sulfide component in the produced oil and gas will cause great damage to downhole pipes and ground transportation facilities. When hydrogen sulfide coexists with water vapor, it will form an extremely corrosive acidic environment, posing a serious threat to metal materials such as steel. In this environment, hydrogen sulfide not only acts directly on the metal surface, accelerating the electrochemical corrosion process and causing gradual erosion of the metal substrate, but also causes serious hydrogen embrittlement problems through hydrogen permeation, that is, hydrogen atoms penetrate into the internal lattice structure of the metal. The hydrogen embrittlement phenomenon greatly reduces the mechanical strength and toughness of steel, causing the originally strong metal material to undergo brittle fracture without obvious external force, which greatly threatens the safe operation of oil and gas field production facilities.

[0003] In order to solve the above problems, it is necessary to develop a coating with excellent high temperature resistance, wear resistance, hydrogen sulfide corrosion resistance, adhesion and other properties according to actual field applications to meet the actual working conditions. Summary of the invention

[0004] The first aspect of the present invention provides a coating composition resistant to hydrogen sulfide corrosion, so that downhole oil casing and ground carbon steel pipeline can be used for a long time in a hydrogen sulfide environment. The specific technical scheme of the present invention is as follows, comprising the following raw materials in weight percentage:

[0005] Component A includes the following raw materials in weight percentage:

[0006] Phenolic epoxy resin: 50-60%

[0007] Filler: 15~25%

[0008] Leveling agent: 0.2~0.8%

[0009] Defoamer: 0.2~0.8%

[0010] Diluent: 20-25%

[0011] Component B includes the following raw materials in weight percentage:

[0012] Phenolic amine epoxy curing agent: 45-55%

[0013] Diluent: 45-55%

[0014] Furthermore, the phenolic epoxy resin has an epoxy equivalent of 150 to 200 and a softening point of 20 to 30° C. F51 phenolic epoxy resin can be used.

[0015] Furthermore, the filler is a filler that can improve the acid resistance and wear resistance of the coating, such as chromium oxide green, talcum powder, barium sulfate, graphite powder, zinc phosphomolybdate, etc.

[0016] Furthermore, the leveling agent is an acrylate leveling agent selected from fluorine-modified acrylate, phosphate-modified acrylate, and the like.

[0017] Furthermore, the defoaming agent is a polysiloxane defoaming agent selected from polysiloxane, silicone defoaming agent, silicone defoaming agent and the like.

[0018] Furthermore, the diluent is a commercial diluent.

[0019] Furthermore, the phenolic amine epoxy curing agent has an amine value of 460 to 550 mgKOH / g. T31 phenolic amine epoxy curing agent can be used.

[0020] The materials used in the present invention are all commercially available materials.

[0021] The phenolic epoxy resin used in the present invention has a higher crosslinking density due to the presence of multiple epoxy groups and phenolic hydroxyl groups in its molecule, and exhibits better hardness, chemical corrosion resistance and adhesion. By adding a variety of fillers, the hydrogen sulfide corrosion resistance and wear resistance of the coating are improved.

[0022] The second aspect of the present invention provides a method for preparing the hydrogen sulfide resistant anticorrosive coating and coating as described above, comprising the following steps:

[0023] In a mixing container, add phenolic epoxy resin, diluent, chromium oxide green, talcum powder, barium sulfate, graphite powder, zinc phosphomolybdate in proportion, stir and disperse at high speed for 30 minutes under the action of high-speed stirring, so that the pigments and fillers are fully dispersed in the resin, and then add polysiloxane, fluorine-modified acrylate and other additives in turn, and disperse at high speed for 30 minutes to make the pigments and fillers fully wetted and evenly dispersed; then add zirconium dioxide grinding balls, continue to grind in the container for 60 minutes, filter the grinding balls, and obtain component A. Then, mix the two components of A and B in a mass ratio of A:B=10:3, and then stir them fully for 5 to 10 minutes using a high-speed mixer to obtain an anti-hydrogen sulfide anti-corrosion coating. The viscosity of the coating is controlled at 30000 to 36000 mPa·s to better meet the subsequent construction requirements. Q235 steel is used as the substrate, and its surface is sandblasted. Brown corundum with a particle size of 24 mesh is selected for sandblasting, so that the surface roughness of the substrate reaches 80 to 100 mm to enhance the bonding strength between the coating and the substrate. After the sandblasting is completed, ethanol is used as a cleaning agent to clean the sandblasted surface. Finally, the above coating is brushed on the substrate surface and placed at room temperature for 10 hours or at 60°C for 5 to 6 hours to complete curing to obtain a hydrogen sulfide anti-corrosion coating.

[0024] The present invention has the advantages that:

[0025] 1. The hardness (pencil hardness method) of the hydrogen sulfide resistant anti-corrosion coating prepared by the present invention is 5H, the adhesion (cross-cut method) is ≥3A, the wear resistance (falling sand method) is ≥2.0L / μm, and the coating does not change after the chemical medium resistance test. The above indicators all meet the relevant requirements of SY / T6717-2016 "Technical Conditions for Internal Coatings of Oil Pipes and Casings".

[0026] 2. The present invention tests the actual protective performance of the coating by simulating the actual working conditions of the oil field through a high-temperature and high-pressure reactor, and designs a variety of test conditions of temperature, pressure, and hydrogen sulfide concentration. The coating of the present invention can meet the corrosion protection requirements of most materials under actual corrosion conditions containing hydrogen sulfide.

[0027] 3. The liquid coating and coating prepared by the present invention can be applied to the corrosion protection of downhole oil casing and ground carbon steel pipelines, thereby greatly improving the service life of the coating of downhole oil casing and ground carbon steel pipelines in a hydrogen sulfide environment, and protecting the downhole oil casing and ground carbon steel pipelines from corrosion by corrosive media containing hydrogen sulfide. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a comparison diagram of the corrosion morphology of the hydrogen sulfide corrosion resistant coating of the present invention before and after immersion for 90 days in a simulated ground pipeline corrosion environment (0.5Mpa, pH=4, 35°C, 35000ppm (Cl-) mineralization);

[0029] Figure 2 This is a comparison diagram of the corrosion morphology of the hydrogen sulfide corrosion resistant coating of the present invention before and after immersion for 90 days in a simulated downhole oil casing corrosion environment (0.5Mpa, pH=4, 35°C, 35000ppm (Cl-) mineralization, 20ppm hydrogen sulfide content);

[0030] Figure 3 This is a comparison diagram of the corrosion morphology of the hydrogen sulfide corrosion resistant coating of the present invention before and after being immersed in a chemical medium corrosion environment (3.5% NaCl, 25° C.) for 90 days;

[0031] Figure 4 This is a comparison diagram of the corrosion morphology of the hydrogen sulfide corrosion resistant coating of the present invention before and after immersion in a chemical medium corrosion environment (crude oil, 80° C.) for 90 days; DETAILED DESCRIPTION

[0033] The specific implementation methods provided by the present invention are described in detail below with reference to specific examples.

[0034] Embodiment 1:

[0035] The coating composition is prepared according to the following composition ratio

[0036] Component A: F51 epoxy resin 55%, chromium oxide green 10%, graphite powder 0.5%, talc 1%, barium sulfate 2.5%, phosphomolybdic acid 6.5%, polysiloxane 0.5%, fluorine-modified acrylate 0.5%, diluent 23.5%.

[0037] Component B: T31 phenolic amine epoxy curing agent 55%, diluent 45%.

[0038] Preparation method: add phenolic epoxy resin, diluent, chromium oxide green, talcum powder, barium sulfate, graphite powder, zinc phosphomolybdate in a mixing container in proportion, stir and disperse at high speed for 30 minutes under the action of high-speed stirring, so that the pigments and fillers are fully dispersed in the resin, and then add polysiloxane, fluorine-modified acrylate and other additives in turn, disperse at high speed for 30 minutes to make the pigments and fillers fully wet and dispersed evenly; then add zirconium dioxide grinding balls, continue to grind in the container for 60 minutes, filter the grinding balls to obtain component A. Then, the A and B components are mixed in a mass ratio of A:B=10:3, and then fully stirred for 10 minutes using a high-speed mixer, and the viscosity of the coating is controlled at 30000-36000mPa·s to better meet the subsequent construction requirements. Q235 steel is used as the substrate, and its surface is sandblasted. Brown corundum with a particle size of 24 mesh is selected for sandblasting, so that the surface roughness of the substrate reaches 80-100mm to enhance the bonding strength between the coating and the substrate. After the sandblasting is completed, ethanol is used as a cleaning agent to clean the sandblasted surface. Finally, the above coating is brushed on the substrate surface and placed at room temperature for 10 hours or at 60°C for 5 to 6 hours to complete curing, thereby obtaining the anti-hydrogen sulfide anticorrosion coating.

[0039] The prepared coating has a coating adhesion of 5A, a hardness of 5H, and a wear resistance of 5.5L / μm according to the standard. It meets the chemical medium corrosion resistance and high temperature and high pressure resistance requirements of SY / T6717-2016 "Technical Conditions for Internal Coatings of Oil Pipes and Casings". The hydrogen sulfide resistance performance test was carried out by simulating the field environment in a high temperature and high pressure reactor, with a set pressure of 0.5MPa, a pH of 4, a test time of 90 days, and a temperature of 35°C. The H2S content is 25ppm, the mineralization is 35000ppm (Cl-), the coating has no softening, blistering, cracking, or shedding, and the underlying steel plate has no corrosion.

[0040] Example 2: The coating composition is prepared according to the following composition ratio:

[0041] Component A: F51 epoxy resin 55%, chromium oxide green 10%, graphite powder 0.5%, talc 4%, barium sulfate 3%, phosphomolybdic acid 3%, polysiloxane 0.5%, fluorine-modified acrylate 0.5%, diluent 23.5%.

[0042] Component B: T31 phenolic amine epoxy curing agent 55%, diluent 45%.

[0043] Preparation method: add phenolic epoxy resin, diluent, chromium oxide green, talcum powder, barium sulfate and graphite powder in a mixing container in proportion, stir and disperse at high speed for 30 minutes under the action of high-speed stirring, so that the pigments and fillers are fully dispersed in the resin, and then add polysiloxane, fluorine-modified acrylate and other additives in turn, disperse at high speed for 30 minutes to make the pigments and fillers fully wet and dispersed evenly; then add zirconium dioxide grinding balls, continue to grind in the container for 60 minutes, filter the grinding balls to obtain component A. Then, mix the A and B components in a mass ratio of A:B=10:3, and then stir them for 10 minutes with a high-speed mixer, control the viscosity of the coating to 30000-36000mPa·s to better meet the subsequent construction requirements, use Q235 steel as the substrate, sandblast its surface, select 24 mesh brown corundum for sandblasting, so that the surface roughness of the substrate reaches 80-100mm to enhance the bonding strength between the coating and the substrate. After the sandblasting is completed, ethanol is used as a cleaning agent to clean the sandblasted surface. Finally, the above coating is brushed on the substrate surface and placed at room temperature for 10 hours or at 60°C for 5 to 6 hours to complete curing, thereby obtaining the anti-hydrogen sulfide anticorrosion coating.

[0044] The prepared coating has a coating adhesion of 5A, a hardness of 5H, and a wear resistance of 5.2L / μm according to the standard. It meets the chemical medium corrosion resistance and high temperature and high pressure resistance requirements of SY / T6717-2016 "Technical Conditions for Internal Coatings of Oil Pipes and Casings". The hydrogen sulfide resistance performance test was carried out by simulating the field environment in a high temperature and high pressure reactor, with a set pressure of 0.5MPa, a pH of 4, a test time of 90 days, and a temperature of 35°C. The H2S content is 25ppm, the mineralization is 35000ppm (Cl-), the coating has no softening, blistering, cracking, or shedding, and the underlying steel plate has no corrosion.

Claims

1. A method for preparing a hydrogen sulfide resistant anticorrosive coating and a coating, characterized in that Add components A and B into different mixers respectively and stir evenly, then add components A and B into a high-speed mixer at a mass ratio of A:B=10:3 and stir and disperse them fully. After uniform dispersion, apply the coating on the surface of the substrate to form a coating on the surface of the substrate.

2. The method for preparing the hydrogen sulfide resistant anticorrosive coating according to claim 1, characterized in that The raw materials respectively contain the following weight percentages; Component A includes the following raw materials in weight percentage: Phenolic epoxy resin: 50-60% Filler: 15~25% Leveling agent: 0.2~0.8% Defoamer: 0.2~0.8% Diluent: 20-25% Component B includes the following raw materials in weight percentage: Phenolic amine epoxy curing agent: 45-55% Diluent: 45-55%.

3. The method for preparing the hydrogen sulfide resistant anticorrosive coating and coating according to claim 2, characterized in that The phenolic epoxy resin has an epoxy equivalent of 150 to 200 and a softening point of 20 to 30°C.

4. The method for preparing the hydrogen sulfide resistant anticorrosive paint and coating according to claim 2, characterized in that The phenolic amine epoxy curing agent adopts a phenolic amine epoxy curing agent with an amine value of 460-550 mgKOH / g.

5. The method for preparing the hydrogen sulfide resistant anticorrosive paint and coating according to claim 2, characterized in that The filler is selected from chromium oxide green, talcum powder, barium sulfate, graphite powder, and zinc phosphomolybdate.

6. The method for preparing the hydrogen sulfide resistant anticorrosive paint and coating according to claim 2, characterized in that The leveling agent is acrylic acid ester.

7. The method for preparing the hydrogen sulfide resistant anticorrosive paint and coating according to claim 2, characterized in that The defoaming agent is a polysiloxane defoaming agent.

8. A method for preparing the hydrogen sulfide resistant anticorrosive coating according to any of claims 1 to 7, characterized in that: The following steps are involved: Add resin, diluent and pigment filler in the mixing container in proportion, stir and disperse at high speed under the action of high-speed stirring, then add leveling agent, defoamer and other additives in turn, and disperse at high speed to make the pigment filler fully wet and evenly dispersed; then add zirconium dioxide grinding balls, continue to grind in the container, filter the grinding balls to obtain component A. Then, mix the two components of A and B in a mass ratio of A:B=10:3, and then stir them fully with a high-speed mixer to obtain the anti-hydrogen sulfide anti-corrosion coating. The viscosity of the coating is controlled at 30000~36000mPa·s to better meet the subsequent construction requirements. Q235 steel is used as the substrate, and its surface is sandblasted. Brown corundum with a particle size of 24 mesh is selected for sandblasting, so that the surface roughness of the substrate reaches 80~100μm to enhance the bonding strength between the coating and the substrate. After the sandblasting is completed, ethanol is used as a cleaning agent to clean the sandblasted surface. Finally, the coating is brushed on the surface of the substrate and placed at room temperature for 10 hours or at 60° C. for 5 to 6 hours to complete curing, thereby obtaining a hydrogen sulfide resistant and anti-corrosion coating.

Citation Information

Patent Citations

  • Solvent-free epoxy primer for high temperature corrosion prevention of steel pipeline welded junction position

    CN102382553A

Cited By

  • Preparation process of blowout preventer rubber core with excellent corrosion resistance

    CN119119520A