Formaldehyde remover-containing E0-grade glue for veneer paper
By adding formaldehyde removers of 5,5-dimethylhydantoin, ε-polylysine hydrochloride and ammonium salt into the mixture of melamine formaldehyde and urea formaldehyde, the existing technology can solve the problem that the existing technology cannot meet the new national standard E0 level formaldehyde release It solves the problem of quantity and achieves formaldehyde removal effect at low cost without affecting the physical and chemical properties.
Patent Information
- Application Number
- CN202410943422.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-01
AI Technical Summary
The existing technology cannot effectively meet the stringent requirements of the new national standard E0 level formaldehyde emission, and the existing aldehyde removers affect the physical and chemical properties of the resin or are costly.
Melamine-formaldehyde mixture and urea-formaldehyde mixture are used as glue raw materials. Through specific preparation steps and the addition of formaldehyde remover 5,5-dimethylhydantoin, ε-polylysine hydrochloride and ammonium salt, the pH value is adjusted to medium. properties, control the amount of formaldehyde remover added to ensure that the physical and chemical properties of the glue are not affected.
It achieves stable control of formaldehyde release within the E0 level range, is easy to use, has low cost, does not affect the physical and chemical properties of the glue, and has better development prospects.
Smart Images

Figure BDA0004944893340000071 
Figure BDA0004944893340000081 
Figure BDA0004944893340000082
Abstract
Description
Technical Field
[0001] The invention relates to the field of formaldehyde removal, and in particular to an E0-grade glue containing a formaldehyde remover for veneer paper of decorative panels. Background Art
[0002] With the development of society, people's food, clothing, housing and transportation are closely related to chemical substances. In life, the most common one is formaldehyde. Formaldehyde can cause many diseases in the human body, such as asthma, bronchitis, dermatitis, etc. Long-term contact can even cause malignant tumors. When the artificial boards used in interior decoration contain formaldehyde-extending resins such as formaldehyde resin, the free formaldehyde remaining in the board that does not participate in the reaction will gradually release into the surrounding environment, thereby forming the main body of formaldehyde in the indoor ambient air. The formaldehyde release of artificial boards is mainly composed of two parts. One is that the substrate itself is made of urea-formaldehyde or triamine glue, which contains a large amount of formaldehyde; the other is that the amino resin formaldehyde in the veneer material exceeds the standard. In terms of substrates, formaldehyde-free substrates can now be prepared using MDI or polyurethane adhesives, but in terms of veneer materials, melamine formaldehyde resin and urea formaldehyde resin have excellent physical and chemical properties and low prices, and other glues cannot replace them. The existing formaldehyde-reducing additives for melamine formaldehyde resin and urea formaldehyde resin are mainly reacted with strong alkaline organic matter, which affects the curing rate and surface properties of the resin. Another method is to use nanomaterials for removal, but the effect is not obvious and the price is expensive.
[0003] According to the latest national standard GB / T 39600-2021, the formaldehyde emission classification requirements for artificial boards and their products have been added. The E0 grade formaldehyde standard of 0.05 mg / m3 has been added. Compared with the previous E1 grade of 0.124 mg / m3, it is more stringent, but it is also the standard that is more recognized by consumers in the market. Under the new standard, the previous formaldehyde removal methods cannot meet the requirements of the latest regulations, which poses great challenges to the research and development of formaldehyde removal agents and the improvement of new glue formulas.
[0004] Chinese patent (CN110615879B) discloses a method for preparing water-soluble phenolic resin, which effectively removes free formaldehyde in the resin by ultrasonically mixing the reaction materials and adding a specific formaldehyde remover after the reaction is completed, thereby improving the safety and environmental protection of the product. The water-soluble phenolic resin prepared by this method has a high solid content and good performance. However, the formaldehyde remover used will affect the physicochemical properties of the resin, and the amount of addition is large and the cost is high. Chinese patent (CN108939388A) discloses the use of chitosan or other amino-containing substances as formaldehyde capture agents to remove formaldehyde. Although this technology has a good rapid adsorption effect, it will no longer have the formaldehyde removal function after reaching adsorption saturation as the use time passes.
[0005] In view of the problems existing in the prior art, how to provide an E0 grade glue containing a formaldehyde remover, the prepared E0 grade glue meets the requirements of the new international standard E0 grade, the formaldehyde remover does not affect the physical and chemical properties of the glue, and the added amount is small, the cost is low, and it has a better development prospect. This is a problem to be urgently solved in the present invention. Summary of the invention
[0006] Purpose of the invention: The purpose of the present invention is to provide an E0-grade glue containing a formaldehyde remover for veneer paper of decorative panels. The E0-grade glue can stably control the formaldehyde emission within the range of the new national standard E0. The formaldehyde remover is easy to use, has a neutral pH value, does not affect the physical and chemical properties of the glue, and has a small amount of addition, and the cost increase is not obvious, so it has a better development prospect.
[0007] The technical solution of the present invention:
[0008] The invention discloses an E0-grade glue containing a formaldehyde remover for veneer paper of decorative panels, characterized in that the raw materials of the E0-grade glue containing a formaldehyde remover for veneer paper of decorative panels include a melamine-formaldehyde mixture and a urea-formaldehyde mixture.
[0009] Further, the preparation of the melamine formaldehyde mixture comprises the following steps:
[0010] (1) In a stirred reactor, add water and formaldehyde, stir evenly, adjust the pH value to 9-9.5, then add melamine, adjust the temperature to 75-80°C, and react until the reaction liquid becomes clear;
[0011] (2) heating the reaction solution of step (1) to 90-95° C., adding diethylene glycol and caprolactam, and stirring evenly to obtain a mixture A;
[0012] (3) Cooling the mixture A obtained in step (2) with cooling water, adjusting the pH value to 8.5-8.8, adding a formaldehyde remover when cooled to 35-40° C., stirring evenly, and standing for 2-4 hours to obtain the melamine formaldehyde mixture.
[0013] Further, the preparation of the urea formaldehyde mixture comprises the following steps:
[0014] (1) Add formaldehyde and urea to a reaction kettle, stir evenly, then add triethanolamine, and adjust the pH value to 7.5-8.0 to obtain glue;
[0015] (2) heating the glue prepared in step (1) to 50-55° C., sealing and keeping warm for 60-80 minutes;
[0016] (3) In step (2), the temperature of the glue is naturally raised to 82-86° C., and formic acid is added to adjust the pH to 4.5-5.2;
[0017] (4) In step (3), the temperature of the glue is naturally raised to 90-95° C., reacted for 60-80 min, and the water solubility ratio is measured;
[0018] (5) adding ammonia water and triethanolamine to the glue in step (4), stirring evenly, and measuring the pH value to be 7 to 8;
[0019] (6) Add deionized water and urea to the glue in step (5) and stir evenly;
[0020] (7) Turn on the cooling water, and when the glue in step (6) is cooled to 70-75° C., add urea;
[0021] (8) When cooled to 40°C, add formaldehyde remover and deionized water and stir evenly;
[0022] (9) Cooling the glue to room temperature to obtain a urea-formaldehyde mixture.
[0023] Furthermore, the raw materials of the formaldehyde remover include 5,5-dimethylhydantoin, ε-polylysine hydrochloride, ammonium salt, and deionized water.
[0024] Furthermore, the raw materials of the formaldehyde remover, calculated as 100% by mass, include: 10-13% 5,5-dimethylhydantoin, 1-5% ε-polylysine hydrochloride, 0.1-2% ammonium salt, and 80-88% deionized water.
[0025] Furthermore, the preparation of the formaldehyde remover includes the following steps: first weigh deionized water, slowly add 5,5-dimethylhydantoin to the deionized water in batches, stir evenly, then add ε-polylysine hydrochloride and ammonium salt, stir and dissolve, and obtain the formaldehyde remover.
[0026] Furthermore, the added mass of the formaldehyde remover accounts for 1-10% of the mass of the melamine-formaldehyde mixture.
[0027] Furthermore, the added mass of the formaldehyde remover accounts for 5-20% of the mass of the urea-formaldehyde mixture.
[0028] Furthermore, the mass ratio of the melamine formaldehyde mixture to the urea formaldehyde mixture is 1:1-2.
[0029] Furthermore, the water solubility ratio of the melamine formaldehyde mixture is 1:1.6-1.8, and the water solubility ratio of the urea formaldehyde mixture is 1:4-4.5.
[0030] Furthermore, the ammonium salt includes one or more of ammonium bicarbonate, ammonium borate, and ammonium bisulfate.
[0031] Furthermore, the mass concentration of the ammonia water is 25%.
[0032] The invention provides an E0-grade glue containing a formaldehyde remover for decorative panel veneer paper. The E0-grade glue containing a formaldehyde remover for decorative panel veneer paper comprises the following steps: adding the formaldehyde remover in the process of preparing the glue; 5,5-dimethylhydroxyethylamine and ε-polylysine hydrochloride are acidic and are adjusted with ammonium salt so that the pH value of the prepared formaldehyde remover is neutral, which will not affect the physicochemical properties and mechanical strength of the glue; the optimal addition amount of the formaldehyde remover is obtained through experimental proportioning, which can control the cost and is economical; the prepared glue can meet the new national standard E0 grade, has less safety hazards, and the prepared decorative panel veneer paper has more application prospects.
[0033] The mass ratio of formaldehyde remover added to the melamine formaldehyde mixture and the urea formaldehyde mixture is inconsistent. Adding formaldehyde removers separately to prepare the resin mixture has a greater effect on formaldehyde removal than mixing the two resin mixtures first and then adding them, so that the formaldehyde remover can be more fully mixed with the resin mixture, thereby achieving the effect of effectively removing formaldehyde and protecting the resin properties.
[0034] Beneficial effects:
[0035] The invention provides an E0-grade glue containing a formaldehyde remover for veneer paper of decorative panels. The prepared E0-grade glue can stably control the formaldehyde release within the range of the new national standard E0. The formaldehyde remover is easy to use, has a neutral pH value, does not affect the physical and chemical properties of the glue, and has a small addition amount, does not significantly increase the cost, and has a better development prospect. DETAILED DESCRIPTION
[0036] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0037] 5,5-Dimethylhydantoin was purchased from Shandong Xinghai Chemical Co., Ltd. with a purity of 99%; ε-polylysine hydrochloride was purchased from Shandong Siyang Biotechnology Co., Ltd.; melamine was purchased from Jinan Zhongcheng Chemical Co., Ltd. with a purity of 99%; caprolactam was purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd.; urea was purchased from Shandong Baihua Chemical Co., Ltd. Industrial urea; amino resin was purchased from Shandong Zhijia Chemical Technology Co., Ltd.; urea-formaldehyde resin, melamine formaldehyde resin, and urea formaldehyde resin were purchased from Shandong Lingchuang Biotechnology Co., Ltd. (excluding formaldehyde remover).
[0038] Unless otherwise specified, the chemical reagents used in the present invention are all commercially available analytically pure.
[0039] Preparation of formaldehyde remover A:
[0040] First weigh 88g of deionized water, slowly add 10g of 5,5-dimethylhydantoin in batches into the deionized water, stir evenly, then add 1g of ε-polylysine hydrochloride and 1g of ammonium bicarbonate, stir to dissolve, and prepare a veneer paper formaldehyde remover.
[0041] Preparation of formaldehyde remover B:
[0042] First weigh 80g of deionized water, slowly add 12g of 5,5-dimethylhydantoin into the deionized water in batches, stir evenly, then add 6g of ε-polylysine hydrochloride and 2g of ammonium bicarbonate, stir to dissolve, and prepare a veneer paper formaldehyde remover.
[0043] Preparation of formaldehyde remover C:
[0044] First weigh 85g of deionized water, slowly add 8g of 5,5-dimethylhydantoin into the deionized water in batches, stir evenly, then add 6g of ε-polylysine hydrochloride and 1g of ammonium bicarbonate, stir to dissolve, and prepare a veneer paper formaldehyde remover for decorative panels.
[0045] Preparation of melamine formaldehyde mixture A:
[0046] (1) In a stirred reactor, add 200 g of water and 480 g of formaldehyde, stir evenly, adjust the pH value to 9.2, then add 400 g of melamine, adjust the temperature to 78° C., and react until the reaction liquid becomes clear;
[0047] (2) heating the reaction solution of step (1) to 90° C., adding 30 g of diethylene glycol and 10 g of caprolactam, and stirring evenly to obtain a mixture A;
[0048] (3) Cooling 1000 g of the mixture A obtained in step (2) with cooling water, adjusting the pH value to 8.5, adding 80 g of formaldehyde to remove A when cooled to 40° C., stirring evenly, and standing for 2 hours to obtain the melamine formaldehyde mixture A.
[0049] Preparation of melamine formaldehyde mixture B:
[0050] (1) In a stirred reactor, add 200 g of water and 480 g of formaldehyde, stir evenly, adjust the pH value to 9.2, then add 400 g of melamine, adjust the temperature to 78° C., and react until the reaction liquid becomes clear;
[0051] (2) heating the reaction solution of step (1) to 90° C., adding 30 g of diethylene glycol and 10 g of caprolactam, and stirring evenly to obtain a mixture A;
[0052] (3) Cooling 1000 g of the mixture A obtained in step (2) with cooling water, adjusting the pH value to 8.5, adding 120 g of formaldehyde remover A when cooled to 40° C., stirring evenly, and standing for 2 hours to obtain the melamine formaldehyde mixture B.
[0053] Preparation of melamine formaldehyde mixture C:
[0054] (1) In a stirred reactor, add 400 g of water and 480 g of formaldehyde, stir evenly, adjust the pH value to 9.2, then add 400 g of melamine, adjust the temperature to 78° C., and react until the reaction liquid becomes clear;
[0055] (2) heating the reaction solution of step (1) to 90° C., adding 30 g of diethylene glycol and 10 g of caprolactam, and stirring evenly to obtain a mixture A;
[0056] (3) Cooling 1000 g of the mixture A obtained in step (2) with cooling water, adjusting the pH value to 8.5, adding 80 g of formaldehyde remover B when cooled to 40° C., stirring evenly, and standing for 2 hours to obtain the melamine formaldehyde mixture C.
[0057] Preparation of melamine formaldehyde mixture D:
[0058] (1) In a stirred reactor, add 400 g of water and 480 g of formaldehyde, stir evenly, adjust the pH value to 9.2, then add 400 g of melamine, adjust the temperature to 78° C., and react until the reaction liquid becomes clear;
[0059] (2) heating the reaction solution of step (1) to 90° C., adding 30 g of diethylene glycol and 10 g of caprolactam, and stirring evenly to obtain a mixture A;
[0060] (3) Cooling 1000 g of the mixture A obtained in step (2) with cooling water, adjusting the pH value to 8.5, adding 80 g of formaldehyde remover C when cooled to 40° C., stirring evenly, and standing for 2 hours to obtain the melamine formaldehyde mixture D.
[0061] Preparation of urea formaldehyde mixture A:
[0062] (1) Add 600 g of formaldehyde and 200 g of urea into a reaction kettle, stir evenly, and then add triethanolamine to adjust the pH value to 7.5 to obtain glue;
[0063] (2) heating the glue prepared in step (1) to 55° C., sealing and keeping warm for 60 min;
[0064] (3) In step (2), the temperature of the glue is naturally raised to 82° C., and formic acid is added to adjust the pH to 5.2;
[0065] (4) The glue in step (3) is naturally heated to 90° C., reacted for 60 min, and the water solubility ratio is measured;
[0066] (5) Add 10 kg of 25% ammonia water and 400 ml of triethanolamine to the glue in step (4), stir evenly, and measure the pH to 7.5;
[0067] (6) Add 100 g of deionized water and 90 g of urea to the glue in step (5) and stir evenly;
[0068] (7) Turn on the cooling water, cool the glue in step (6) to 72° C., add 120 g of urea, and stir evenly to obtain a glue mixture;
[0069] (8) When cooled to 40° C., add 25 g of formaldehyde remover A and 50 g of deionized water to 250 g of the glue mixture prepared in step (7), and stir evenly;
[0070] (9) The glue is cooled to room temperature to obtain a urea-formaldehyde mixture A.
[0071] Preparation of urea formaldehyde mixture B:
[0072] (1) Add 600 g of formaldehyde and 200 g of urea into a reaction kettle, stir evenly, and then add triethanolamine to adjust the pH value to 7.5 to obtain glue;
[0073] (2) heating the glue prepared in step (1) to 55° C., sealing and keeping warm for 60 min;
[0074] (3) In step (2), the temperature of the glue is naturally raised to 82° C., and formic acid is added to adjust the pH to 5.2;
[0075] (4) The glue in step (3) is naturally heated to 90° C., reacted for 60 min, and the water solubility ratio is measured;
[0076] (5) Add 10 g of 25% ammonia water and 400 ml of triethanolamine to the glue in step (4), stir evenly, and measure the pH to 7.5;
[0077] (6) Add 100 g of deionized water and 90 g of urea to the glue in step (5) and stir evenly;
[0078] (7) Turn on the cooling water, cool the glue in step (6) to 72° C., add 120 g of urea, and stir evenly to obtain a glue mixture;
[0079] (8) When cooled to 40° C., add 5 g of formaldehyde remover A and 50 g of deionized water to 250 g of the glue mixture prepared in step (7), and stir evenly;
[0080] (9) The glue is cooled to room temperature to obtain a urea-formaldehyde mixture B.
[0081] Preparation of urea formaldehyde mixture C:
[0082] (1) Add 600 g of formaldehyde and 200 g of urea into a reaction kettle, stir evenly, and then add triethanolamine to adjust the pH value to 7.5 to obtain glue;
[0083] (2) heating the glue prepared in step (1) to 55° C., sealing and keeping warm for 60 min;
[0084] (3) In step (2), the temperature of the glue is naturally raised to 82° C., and formic acid is added to adjust the pH to 5.2;
[0085] (4) The glue in step (3) is naturally heated to 90° C., reacted for 60 min, and the water solubility ratio is measured;
[0086] (5) Add 10 kg of 25% ammonia water and 400 ml of triethanolamine to the glue in step (4), stir evenly, and measure the pH to 7.5;
[0087] (6) Add 100 g of deionized water and 90 g of urea to the glue in step (5) and stir evenly;
[0088] (7) Turn on the cooling water, cool the glue in step (6) to 72° C., add 120 g of urea, and stir evenly to obtain a glue mixture;
[0089] (8) When cooled to 40° C., add 60 g of formaldehyde remover B and 50 g of deionized water to 250 g of the glue mixture prepared in step (7), and stir evenly;
[0090] (9) The glue is cooled to room temperature to obtain a urea-formaldehyde mixture C.
[0091] Preparation of urea formaldehyde mixture D:
[0092] (1) Add 600 g of formaldehyde and 200 g of urea into a reaction kettle, stir evenly, and then add triethanolamine to adjust the pH value to 7.5 to obtain glue;
[0093] (2) heating the glue prepared in step (1) to 55° C., sealing and keeping warm for 60 min;
[0094] (3) In step (2), the temperature of the glue is naturally raised to 82° C., and formic acid is added to adjust the pH to 5.2;
[0095] (4) The glue in step (3) is naturally heated to 90° C., reacted for 60 min, and the water solubility ratio is measured;
[0096] (5) Add 10 kg of 25% ammonia water and 400 ml of triethanolamine to the glue in step (4), stir evenly, and measure the pH to 7.5;
[0097] (6) Add 100 g of deionized water and 90 g of urea to the glue in step (5) and stir evenly;
[0098] (7) Turn on the cooling water, cool the glue in step (6) to 72° C., add 120 g of urea, and stir evenly to obtain a glue mixture;
[0099] (8) When cooled to 40° C., add 25 g of formaldehyde remover B and 50 g of deionized water to 250 g of the glue mixture prepared in step (7), and stir evenly;
[0100] (9) The glue is cooled to room temperature to obtain a urea-formaldehyde mixture D.
[0101] Preparation of urea formaldehyde mixture E:
[0102] (1) Add 600 g of formaldehyde and 200 g of urea into a reaction kettle, stir evenly, and then add triethanolamine to adjust the pH value to 7.5 to obtain glue;
[0103] (2) heating the glue prepared in step (1) to 55° C., sealing and keeping warm for 60 min;
[0104] (3) In step (2), the temperature of the glue is naturally raised to 82° C., and formic acid is added to adjust the pH to 5.2;
[0105] (4) The glue in step (3) is naturally heated to 90° C., reacted for 60 min, and the water solubility ratio is measured;
[0106] (5) Add 10 kg of 25% ammonia water and 400 ml of triethanolamine to the glue in step (4), stir evenly, and measure the pH to 7.5;
[0107] (6) Add 100 g of deionized water and 90 g of urea to the glue in step (5) and stir evenly;
[0108] (7) Turn on the cooling water, cool the glue in step (6) to 72° C., add 120 g of urea, and stir evenly to obtain a glue mixture;
[0109] (8) When cooled to 40° C., add 25 g of formaldehyde remover C and 50 g of deionized water to 250 g of the glue mixture prepared in step (7), and stir evenly;
[0110] (9) The glue is cooled to room temperature to obtain a urea-formaldehyde mixture E.
[0111] Examples 1 to 11
[0112] The E0-grade glue containing formaldehyde remover for veneer paper of veneer board was prepared by simple mixing. Table 1 is the ingredient list of the E0-grade glue of Examples 1 to 11.
[0113] Table 1:
[0114]
[0115]
[0116] Comparative Examples 1 to 4
[0117] The E0-grade glue containing formaldehyde remover for veneer paper of decorative panels was prepared by simple mixing. Table 2 is the ingredient list of the E0-grade glue of comparative examples 1 to 4.
[0118] Table 2:
[0119]
[0120] Performance test experiment:
[0121] 1. Viscosity test: Viscosity refers to the measurement of the fluidity of glue, which can be tested by a viscometer. First, put 5 ml of glue into the viscometer and measure the flow time of the glue at 25°C. Determine the viscosity of the glue based on the flow time.
[0122] 2. Water solubility ratio test: According to the evaporation capacity method, put 100g of glue into a beaker with a fixed capacity. By heating the glue sample, the water in it evaporates until the weight of the sample remains unchanged. The water solubility ratio can be calculated based on the weight difference of different samples.
[0123] 3. pH test: After diluting 5g of glue sample 10 times, measure its pH value with a pH meter.
[0124] 4. Shear strength test: Shear strength refers to the ability of the glue bonded part to resist shear force when shear force is applied. It can be tested by a shear tester. First, prepare the two materials to be bonded, apply glue to them, and then apply shear force through a shear tester to record the shear force at which the glue fails.
[0125] Shear strength test is an important indicator for evaluating the bonding strength of glue.
[0126] 5. Drying time test: Drying time refers to the time it takes for the glue to completely dry after application.
[0127] 6. Formaldehyde content test: Climate chamber method, cut the decorative panel into 1 square meter pieces, place the sample at 23℃ and 50% relative humidity for 15 days to reach equilibrium. During the equilibrium process, ensure that the formaldehyde concentration in the air does not exceed 0.05mg / m3. After equilibrium, use formaldehyde-free aluminum tape to seal the edge of the sample. The ratio of the edge sealing length to the surface area of the specimen is 1.5m / m 2 Place the sealed samples in a climate chamber at 23°C and 80% relative humidity. Use an air sampler to connect two sampling bottles for sampling. Sampling should be done twice a day in the morning and afternoon. The sampling interval should be more than 3 hours. After multiple samplings, calculate the stable release of formaldehyde.
[0128] The following are the test results Table 3, Table 4, Table 5.
[0129] Table 3:
[0130] Material pH Formaldehyde Remover A 7.2 Formaldehyde remover B 8.0 Formaldehyde remover C 8.5
[0131] Table 4:
[0132]
[0133]
[0134] Table 5:
[0135] experiment Viscosity / s Drying time / h Shear strength / MPa Example 1 15 8 95 Example 2 16 8 105 Example 3 12 8 100 Example 4 18 8 95 Example 5 12 10 85 Example 6 15 10 85 Example 7 15 10 85 Example 8 16 10 80 Example 9 16 10 85 Example 10 17 10 85 Embodiment 11 20 10 80 Comparative Example 1 15 12 70 Comparative Example 2 16 12 75 Comparative Example 3 14 11 80 Comparative Example 4 10 12 80
[0136] From the above data, it can be seen that unreasonable content of the prepared formaldehyde remover 5,5-dimethylhydantoin and ε-polylysine hydrochloride will affect the pH value of the formaldehyde remover; from the comparison between Example 1 and Example 3-4, it can be seen that the physical and chemical properties of the E0-grade glue prepared by unreasonable content of the melamine formaldehyde mixture and the urea formaldehyde mixture are low, the drying time is prolonged, the shear strength is reduced, the viscosity is weakened, and the expected requirements are not met; from the comparison between Example 5 and Example 1, it can be seen that when the amount of formaldehyde remover in the prepared melamine formaldehyde mixture is too much, it will The physicochemical properties of the prepared E0-grade glue are low, the drying time is long, the shear strength is low, and the expected requirements are not met; from the comparison of Example 6-7 with Example 1, it can be seen that when the formaldehyde remover formula in the prepared melamine formaldehyde mixture is unreasonable, the physicochemical properties of the prepared E0-grade glue are low, the drying time is long, the shear strength is low, and the expected requirements are not met; from the comparison of Example 8-9 with Example 1, it can be seen that when the amount of formaldehyde remover in the prepared urea formaldehyde mixture is unreasonable, the physicochemical properties of the prepared E0-grade glue are low. The physicochemical properties of the prepared E0-grade glue are low, the drying time is long, the shear strength is low, and the expected requirements are not met; from the comparison of Examples 9-11 with Example 1, it can be seen that when the formaldehyde remover formula in the prepared melamine formaldehyde mixture is unreasonable, the physicochemical properties of the prepared E0-grade glue are low, the drying time is long, and the shear strength is low, which cannot meet the expected requirements; from Comparative Example 1 and Example 1, it can be seen that the total number of parts is the same, and only the prepared melamine mixture is used, and the viscosity, drying time and shear strength of the prepared E0-grade glue are all worse; from Comparative Example 2 As can be seen from Example 1, the total number of parts is the same, but the viscosity, drying time and shear strength of the prepared E0 grade glue are all deteriorated by using the prepared urea formaldehyde mixture, indicating that the melamine formaldehyde mixture prepared by the present invention and the urea formaldehyde mixture have a synergistic effect; from Comparative Example 3 and Example 1, it can be seen that the melamine formaldehyde mixture and the urea formaldehyde mixture are mixed, and then mixed with the formaldehyde remover prepared by the present invention, the shear strength of the prepared glue becomes lower, the drying time becomes longer, and the formaldehyde release does not meet the requirements of E0 grade glue.
[0137] The present invention can also have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.
Claims
1. An E0-grade glue containing formaldehyde remover for veneer paper. It is characterized in that The raw materials of the E0-grade glue containing formaldehyde remover used for the veneer paper of the decorative panel include melamine formaldehyde mixture and urea formaldehyde mixture.
2. The E0-grade glue containing formaldehyde remover for veneer paper according to claim 1, It is characterized in that The preparation of the melamine formaldehyde mixture comprises the following steps: (1) In a stirred reactor, add water and formaldehyde, stir evenly, adjust the pH value to 9-9.5, then add melamine, adjust the temperature to 75-80°C, and react until the reaction liquid becomes clear; (2) heating the reaction solution of step (1) to 90-95° C., adding diethylene glycol and caprolactam, and stirring evenly to obtain a mixture A; (3) Cooling the mixture A obtained in step (2) with cooling water, adjusting the pH value to 8.5-8.8, adding a formaldehyde remover when cooled to 35-40° C., stirring evenly, and standing for 2-4 hours to obtain the melamine formaldehyde mixture.
3. The E0-grade glue containing formaldehyde remover for veneer paper according to claim 1, It is characterized in that The preparation of the urea formaldehyde mixture comprises the following steps: (1) Add formaldehyde and urea to a reaction kettle, stir evenly, then add triethanolamine, and adjust the pH value to 7.5-8.0 to obtain glue; (2) heating the glue prepared in step (1) to 50-55° C., sealing and keeping warm for 60-80 minutes; (3) In step (2), the temperature of the glue is naturally raised to 82-86° C., and formic acid is added to adjust the pH to 4.5-5.2; (4) In step (3), the temperature of the glue is naturally raised to 90-95° C., reacted for 60-80 min, and the water solubility ratio is measured; (5) adding ammonia water and triethanolamine to the glue in step (4), stirring evenly, and measuring the pH value to be 7 to 8; (6) Add deionized water and urea to the glue in step (5) and stir evenly; (7) Turn on the cooling water, and when the glue in step (6) is cooled to 70-75° C., add urea; (8) When cooled to 40°C, add formaldehyde remover and deionized water and stir evenly; (9) Cooling the glue to room temperature to obtain a urea-formaldehyde mixture.
4. The E0-grade glue containing formaldehyde remover for veneer paper of veneer according to claim 2 or 3, It is characterized in that The raw materials of the formaldehyde remover include 5,5-dimethylhydantoin, ε-polylysine hydrochloride, ammonium salt and deionized water.
5. The E0-grade glue containing formaldehyde remover for veneer paper according to claim 4, It is characterized in that The raw materials of the formaldehyde remover are 100% by mass, including: 10-13% of 5,5-dimethylhydantoin, 1-5% of ε-polylysine hydrochloride, 0.1-2% of ammonium salt, and 80-88% of deionized water.
6. The E0-grade glue containing formaldehyde remover for veneer paper according to claim 5, It is characterized in that The preparation of the formaldehyde remover comprises the following steps: first weighing deionized water, slowly adding 5,5-dimethylhydantoin in batches into the deionized water, stirring evenly, then adding ε-polylysine hydrochloride and ammonium salt, stirring and dissolving, and preparing the formaldehyde remover.
7. The E0-grade glue containing formaldehyde remover for veneer paper according to claim 2, It is characterized in that The added mass of the formaldehyde remover accounts for 1-10% of the mass of the melamine-formaldehyde mixture.
8. The E0-grade glue containing formaldehyde remover for veneer paper according to claim 3, It is characterized in that The added mass of the formaldehyde remover accounts for 5-20% of the mass of the urea-formaldehyde mixture.
9. The E0-grade glue containing formaldehyde remover for veneer paper according to claim 1, It is characterized in that The mass ratio of the melamine formaldehyde mixture to the urea formaldehyde mixture is 1:1-2.
10. The E0-grade glue containing formaldehyde remover for veneer paper according to claim 1, It is characterized in that The water solubility ratio of the melamine formaldehyde mixture is 1:1.6-1.8, and the water solubility ratio of the urea formaldehyde mixture is 1:4-4.5.