Preparation method and application of composite molten salt phase change material
Through the ball milling method, high-frequency and high-speed impact and friction are carried out during the crushing process of the composite molten salt, which solves the problems of high energy consumption and delamination in the traditional composite molten salt production process, and prepares composite molten salt with low energy consumption and high melting degree. Improved performance and safety of energy storage materials.
Patent Information
- Application Number
- CN202310330360.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
AI Technical Summary
The traditional production process of composite molten salt consumes high energy, which causes the composite molten salt to easily delaminate when used in non-flow conditions, affecting the service life and safety of energy storage products.
The ball milling method is used to fully mix the composite molten salt components during the crushing process through high-frequency and high-speed impact and friction to generate a uniform eutectic eutectic mixture, thus avoiding the high energy consumption of traditional melting processes.
It achieves the preparation of composite molten salt with low energy consumption, improves the degree of miscibility and eutectic, and the melting point is close to the theoretical eutectic point, which enhances material performance, prevents phase delamination, and improves the safety and service life of energy storage devices.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of phase change energy storage, and in particular to a preparation method and application of a composite molten salt phase change material for energy storage. Background Art
[0002] Solar energy and wind energy are excellent renewable energy sources with great economic value. However, due to the huge volatility of solar energy and wind energy, there is a serious mismatch between the supply and demand of solar energy and wind energy in terms of time, space and intensity. In the process of utilizing solar energy and wind energy, supporting energy storage technology is needed to solve the above problems in order to improve the regulation ability, comprehensive efficiency and safety of the energy system.
[0003] Molten salt has the characteristics of high boiling point, low viscosity, low vapor pressure, and high volume heat, and is an excellent heat transfer and heat storage medium. Its application in the process of solar thermal power generation is relatively mature. However, pure salt (monovalent molten salt) has a high melting point, so in industrial applications, two or more pure salts are generally prepared into a eutectic mixture (composite molten salt) with a low eutectic point by mixing.
[0004] The production process of traditional composite molten salt is to heat and melt the different components of the composite molten salt to form a eutectic mixture with a low eutectic point. Although the traditional method can produce a uniformly mixed composite molten salt, the components of the composite molten salt after proportioning need to be physically mixed and heated to completely melt, then stirred and mixed evenly, and finally cooled and crushed. The production process is extremely energy-intensive. Taking Solar Salt binary composite molten salt (compounded by sodium nitrate and potassium nitrate in a mass ratio of 6:4, with a theoretical low eutectic point of 220.0℃) as an example, it takes about 1kWh of energy to heat 4.5 kg of Solar Salt binary molten salt from room temperature to a molten state. If it is not melted, only physically stirred, the components cannot be mixed. When used, especially when used in a non-fluid state, due to the difference in melting points between the components, the composite molten salt phase change material will be stratified during use, seriously affecting the physicochemical properties of the material, and affecting the service life and safety of energy storage products. Summary of the invention
[0005] In view of the above-mentioned shortcomings, the object of the present invention is to provide a method for preparing a composite molten salt phase change material with low energy consumption and high miscibility of each component. It is not necessary to heat the components of the composite molten salt phase change material to complete melting, so as to obtain a composite molten salt phase change material with uniform miscibility and a low eutectic point.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is: The preparation method of the composite molten salt phase change material according to an embodiment of the present invention is: By ball milling, high-frequency and high-speed collision and friction between ball milling beads and between ball milling jars are utilized during the ball milling process, so that different components in the composite molten salt phase change material are fully mixed and melted during the pulverizing process to generate a eutectic mixture with uniform melting and low eutectic point.
[0007] Furthermore, the ball milling process is dry ball milling, during which powders of different components are directly added into a ball milling tank for ball milling without using liquid ball milling media.
[0008] Furthermore, during the dry ball milling process, the filling ratio of the ball mill is 50% to 80%, the material / ball mass ratio (mass ratio of the composite molten salt component to the ball milling beads) is 1:1 to 3:1, the specific gravity of the ball milling beads is 6.0 to 7.8, the rotation speed is 200 to 500 r / min, and the ball milling time is 25 to 50 min.
[0009] Furthermore, the ball milling process is wet ball milling, and in addition to the composite molten salt phase change material components, a liquid that does not react with the components of the composite molten salt phase change material is added to the ball milling tank as a ball milling medium for wet ball milling.
[0010] Furthermore, during the wet ball milling process, the filling ratio of the ball mill is 50% to 80%, the material / liquid mass ratio (the mass ratio of the composite molten salt component to the liquid ball milling medium) is 1:1 to 4:1, the material / ball mass ratio (the mass ratio of the sum of the mass of the composite molten salt component and the liquid ball milling medium to the mass of the ball milling beads) is 1:1 to 3:1, the specific gravity of the ball milling beads is 6.0 to 7.8, the rotation speed is 200 to 500 r / min, and the ball milling time is 25 to 50 min.
[0011] Furthermore, in the wet ball milling process, the liquid ball milling medium is an inorganic liquid, such as pure water.
[0012] Furthermore, in the wet ball milling process, the liquid ball milling medium is an organic liquid, such as anhydrous ethanol or anhydrous acetone.
[0013] The above technical solution of the present invention has at least one of the following beneficial effects: According to the preparation method of the embodiment of the present invention, the composite molten salt preparation process has low energy consumption, the prepared composite molten salt phase change material has high miscibility, high eutectic degree, melting point close to the theoretical low eutectic point, and excellent performance. Especially when used in a static non-flowing energy storage device, although the molten salt phase change material will not be forcibly disturbed during the use of the above energy storage device, the composite molten salt phase change material prepared by the preparation method of the embodiment of the present invention can still effectively prevent phase stratification caused by uneven mixing of the components in the composite molten salt phase change material. DETAILED DESCRIPTION
[0014] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the described embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0015] First, the preparation method according to an embodiment of the present invention is described in detail below.
[0016] According to the preparation method of the composite molten salt phase change material of the embodiment of the present invention, the traditional melt mixing method is not adopted, but the ball milling method is used, and the high-frequency and high-speed collision and friction between the ball milling beads and the ball milling jar are used in the ball milling process, so that the different components in the composite molten salt phase change material are fully mixed and melted during the crushing process, and a eutectic composite molten salt phase change material with uniform melting and low eutectic point is generated. A differential scanning calorimeter (DSC) is used to test the melting point of the composite molten salt phase change material prepared by the preparation method of the embodiment of the present invention to characterize the preparation effect. The more uniform the melting of the components of the composite molten salt, the higher the degree of eutectic, and the closer its melting point is to the theoretical low eutectic point. Embodiment 1:
[0017] Sodium nitrate and potassium nitrate powders were prepared according to the component ratio (sodium nitrate and potassium nitrate mass ratio 6:4), and Solar Salt binary molten salt was prepared by dry ball milling. During ball milling, the filling ratio of the ball mill was 65%; the material / ball mass ratio was 2:1; the specific gravity of the ball mill was 6.0; the rotation speed was 350r / min; and the ball milling time was 35min. The melting point of the obtained Solar Salt binary molten salt was 220.7℃. Embodiment 2:
[0018] Sodium nitrate and potassium nitrate powders were prepared according to the component ratio (sodium nitrate and potassium nitrate mass ratio 6:4), and Solar Salt binary molten salt was prepared by dry ball milling. During ball milling, the filling ratio of the ball mill was 75%; the material / ball mass ratio was 3:1; the specific gravity of the ball mill was 6.0; the rotation speed was 350r / min; and the ball milling time was 35min. The melting point of the obtained Solar Salt binary molten salt was 232.4℃. Embodiment 3:
[0019] Sodium nitrate and potassium nitrate powders were prepared according to the component ratio (sodium nitrate and potassium nitrate mass ratio 6:4), and Solar Salt binary molten salt was prepared by dry ball milling. During ball milling, the filling ratio of the ball mill was 75%; the material / ball mass ratio was 3:1; the specific gravity of the ball mill was 7.8; the rotation speed was 350r / min; and the ball milling time was 30min. The melting point of the obtained Solar Salt binary molten salt was 225.3℃. Embodiment 4:
[0020] Sodium nitrate and potassium nitrate powders were prepared according to the component ratio (sodium nitrate and potassium nitrate mass ratio 6:4), and Solar Salt binary molten salt was prepared by wet ball milling. During ball milling, the filling ratio of the ball mill was 75%; the material / liquid mass ratio was 3:1; the material / ball mass ratio was 3:1; the ball milling bead specific gravity was 6; the rotation speed was 350r / min; and the ball milling time was 25min. The melting point of the obtained Solar Salt binary molten salt was 230.6℃. Embodiment 5:
[0021] Sodium nitrate and potassium nitrate powders were prepared according to the component ratio (sodium nitrate and potassium nitrate mass ratio 6:4), and Solar Salt binary molten salt was prepared by wet ball milling. During ball milling, the filling ratio of the ball mill was 80%; the material / liquid mass ratio was 1:1; the material / ball mass ratio was 3:1; the ball milling bead specific gravity was 6; the rotation speed was 350r / min; and the ball milling time was 45min. The melting point of the obtained Solar Salt binary molten salt was 228.5℃. Example 6
[0022] Potassium nitrate, sodium nitrite and sodium nitrate powders were prepared according to the component ratio (mass ratio of potassium nitrate, sodium nitrite and sodium nitrate was 53:40:7, theoretical eutectic point was 142.0°C), and the ternary molten salt was prepared by dry ball milling. During ball milling, the filling ratio of the ball mill was 70%; the material / ball mass ratio was 2:1; the specific gravity of the ball mill was 6; the rotation speed was 350r / min; and the ball milling time was 45min. The melting point of the obtained ternary molten salt was 142.8°C. Embodiment 7:
[0023] Potassium nitrate, sodium nitrite and sodium nitrate powders were prepared according to the component ratio (mass ratio of potassium nitrate, sodium nitrite and sodium nitrate was 53:40:7, theoretical eutectic point was 142.0°C), and the ternary molten salt was prepared by wet ball milling. During ball milling, the filling ratio of the ball mill was 80%; the material / liquid mass ratio was 2:1; the material / ball mass ratio was 2:1; the specific gravity of the ball mill was 6; the rotation speed was 500r / min; and the ball milling time was 25min. The melting point of the obtained ternary molten salt was 143.1°C. Comparative Example 1:
[0024] Sodium nitrate and potassium nitrate powders were prepared according to the component ratio (sodium nitrate and potassium nitrate mass ratio 6:4), and Solar Salt binary molten salt was prepared by dry ball milling. During ball milling, the filling ratio of the ball mill was 45%; the material / ball mass ratio was 1:1; the specific gravity of the ball mill was 6.0; the rotation speed was 350r / min; and the ball milling time was 45min. The powder filling amount was too low to effectively grind and disperse, and the melting point of the obtained Solar Salt binary molten salt was 268.3℃. Comparative Example 2:
[0025] Sodium nitrate and potassium nitrate powders were prepared according to the component ratio (sodium nitrate and potassium nitrate mass ratio 6:4), and Solar Salt binary molten salt was prepared by dry ball milling. During ball milling, the filling ratio of the ball mill was 85%; the material / ball mass ratio was 5:1; the specific gravity of the ball mill was 6.0; the rotation speed was 350r / min; and the ball milling time was 45min. The powder filling amount was too high and the powder proportion was too large, so it was impossible to disperse effectively. The melting point of the obtained Solar Salt binary molten salt was 291.0℃. Comparative Example 3:
[0026] Sodium nitrate and potassium nitrate powders were prepared according to the component ratio (sodium nitrate and potassium nitrate mass ratio 6:4), and Solar Salt binary molten salt was prepared by dry ball milling. During ball milling, the filling ratio of the ball mill was 75%; the material / ball mass ratio was 3:1; the specific gravity of the ball mill was 6.0; the speed was 800r / min; and the ball milling time was 45min. The speed was too high and the collision energy was too high, which caused some powders to melt and agglomerate, and the powders could not be effectively dispersed, resulting in uneven mixing of the molten salt. The melting point of the obtained Solar Salt binary molten salt was 280.2℃. Comparative Example 4:
[0027] Sodium nitrate and potassium nitrate powders were prepared according to the component ratio (sodium nitrate and potassium nitrate mass ratio 6:4), and Solar Salt binary molten salt was prepared by dry ball milling. During ball milling, the filling ratio of the ball mill was 70%; the material / ball mass ratio was 2:1; the specific gravity of the ball mill was 6.0; the rotation speed was 400r / min; and the ball milling time was 15min. The ball milling time was too short, resulting in uneven mixing of the molten salt, and the melting point of the obtained Solar Salt binary molten salt was 263.1℃. Comparative Example 5:
[0028] Sodium nitrate and potassium nitrate powders were prepared according to the component ratio (sodium nitrate and potassium nitrate mass ratio 6:4), and Solar Salt binary molten salt was prepared by wet ball milling. During ball milling, the filling ratio of the ball mill was 70%; the material / liquid mass ratio was 5:1; the material / ball mass ratio was 3:1; the ball specific gravity was 6; the rotation speed was 350r / min; and the ball milling time was 45min. If the material / liquid mass ratio was too high, the powder would agglomerate, resulting in insufficient grinding, and the melting point of the obtained Solar Salt binary molten salt was 241.2℃.
[0029] By comparison, it was found that the composite molten salt prepared by the preparation method of the composite molten salt phase change material in the embodiment of the present invention was uniformly mixed and had a high degree of eutectic. The difference between the melting point of the molten salt and the theoretical low eutectic point was about 10°C. The difference between the melting point of the composite molten salt phase change material prepared by the preparation method of the preferred embodiment and the theoretical low eutectic point was within 1°C.
[0030] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a composite molten salt phase change material, characterized in that: The composite molten salt phase change material includes two or more different components and is prepared by ball milling. During the ball milling process, the collision and friction between ball milling beads and between ball milling beads and ball milling jars are utilized to fully mix and melt the different components in the composite molten salt phase change material to form a eutectic mixture with a low eutectic point.
2. The method for preparing the composite molten salt phase change material according to claim 1, characterized in that: The ball milling method is dry ball milling, and no liquid ball milling medium is used during ball milling.
3. The method for preparing the composite molten salt phase change material according to claim 2, characterized in that: In the dry ball milling process, the filling ratio of the ball mill is 50% to 80%, the material / ball mass ratio is 1:1 to 3:1, the specific gravity of the ball mill is 6.0 to 7.8, the rotation speed is 200 to 500 r / min, and the ball milling time is 25 to 50 min.
4. The method for preparing the composite molten salt phase change material according to claim 1, characterized in that: The ball milling process is wet ball milling, and during the ball milling process, a liquid that does not chemically react with the components of the composite molten salt phase change material is used as a ball milling medium.
5. The method for preparing the composite molten salt phase change material according to claim 4, characterized in that: During the wet ball milling process, the filling ratio of the ball mill is 50% to 80%, the material / liquid mass ratio is 1:1 to 4:1, the material / ball mass ratio is 1:1 to 3:1, the ball milling bead specific gravity is 6.0 to 7.8, the rotation speed is 200 to 500 r / min, and the ball milling time is 25 to 50 min.
6. The method for preparing the composite molten salt phase change material according to claim 5, characterized in that: The liquid milling medium is an inorganic liquid, such as pure water.
7. The method for preparing the composite molten salt phase change material according to claim 6, characterized in that: The liquid ball milling medium is an organic liquid, such as anhydrous ethanol or anhydrous acetone.
8. The method for preparing a composite molten salt phase change material according to claims 1 to 7, characterized in that: The composite molten salt phase change material is composited from sodium nitrate and potassium nitrate in a mass ratio of 6:
4.
9. The method for preparing a composite molten salt phase change material according to claims 1 to 7, characterized in that: The composite molten salt phase change material is composited from potassium nitrate, sodium nitrite and sodium nitrate in a mass ratio of 53:40:
7.
10. An application of a composite molten salt phase change material, characterized in that: The composite molten salt phase change material is prepared by the preparation method of the composite molten salt phase change material as described in claims 1 to 9, and is applied to a static energy storage product in which the composite molten salt phase change material will not be forcibly disturbed during the process of storing / releasing energy.