Stearic acid coated red fluorescent powder as well as preparation method and application thereof

By coating the surface of Mn4+-doped fluoride red phosphor with a stearic acid layer, the problems of insufficient thermal stability and water resistance are solved, and efficient red light emission and stable white light LED applications are achieved.

CN118725855APending Publication Date: 2024-10-01SHANGHAI INST OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410765378.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Mn4+-doped fluoride red phosphor has problems with poor thermal stability and water resistance in solid-state light-emitting devices, resulting in reduced luminous efficiency and color shift, limiting its application in lighting and display fields.

Method used

By coating the surface of Mn4+-doped fluoride red phosphor with a hydrophobic stearic acid layer, using co-precipitation method and stearic acid emulsification reaction, an organic layer with excellent hydrophobicity and high boiling point is formed to improve its thermal stability and Water resistance.

Benefits of technology

It significantly improves the fluorescence thermal stability and water resistance stability of the red phosphor, maintains high luminous efficiency, and matches a variety of chips, making it suitable for the production of commercial white light LEDs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725855A_ABST
    Figure CN118725855A_ABST
Patent Text Reader

Abstract

The invention relates to stearic acid coated red fluorescent powder and a preparation method and application thereof, the red fluorescent powder is Mn < 4 + > doped fluoride, and the typical representative general formula of the red fluorescent powder is K2SiF6: Mn < 4 + >, the outer layer of the red fluorescent powder is coated with hydrophobic stearic acid, and the molar ratio of the stearic acid to the precursor K2MnF6 is (0.242-0.605): 0.3. The preparation method comprises the following steps: dissolving KHF2 and KMnO4 in an HF solution, continuously stirring, then adding H2O2 until a solid is separated out, washing and drying to obtain a precursor K2MnF6; the preparation method comprises the following steps: dissolving a precursor K2MnF6 in a fluosilicic acid solution, and then adding KF until the KF is dissolved; and adding a stearic acid ethanol solution into the mixed solution, continuously stirring until complete reaction, washing, and drying to obtain the stearic acid coated red fluorescent powder. Compared with the prior art, the surface of the Mn < 4 + >-doped fluoride red fluorescent powder is coated with the hydrophobic organic high-boiling-point stearic acid layer, so that the fluorescence thermal stability and the water-resistant stability of the red fluorescent powder can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fluorescent materials, and in particular relates to a stearic acid-coated red fluorescent powder and a preparation method and application thereof. Background Art

[0002] Solid-state white light emitting diodes (LEDs) are the next generation of lighting equipment that will replace traditional incandescent and fluorescent lamps due to their advantages of energy saving, durability, long life and environmental protection. At present, there are two main ways to obtain white light LEDs. One is to excite red, green and blue phosphors with near-ultraviolet light chips, but its luminous efficiency is low. The other is to excite multi-color phosphors with blue light chips, and the obtained white light LEDs have high luminous efficiency and high light conversion efficiency. However, only using Y3Al5O 12 :Ce 3+ (YAG:Ce 3+ ) When yellow phosphor is used, the lack of red light component will result in a low color rendering index and high correlated color temperature, which limits the application of white light LEDs. Therefore, it is necessary to add appropriate red phosphor to the LED to supplement the red light component to overcome this difficulty.

[0003] Manganese(IV)-doped fluoride is one of the most promising red phosphors for white light emitting diodes (WLEDs). 2+ and LuVO4:Eu 3+ Compared with rare earth doped sulfides, nitrides and oxides, manganese (IV) doped fluoride phosphors show superior luminescence performance and thermal stability than organic compounds or quantum dots, and also show excellent narrow-band red emission under ambient conditions. Sulfide phosphors are hygroscopic and easily produce toxic gases and Eu upon hydrolysis. 2+ Doped nitride and oxide-based red phosphors, but this type of phosphor has shortcomings such as too wide emission bandwidth and harsh preparation process. In addition, phosphors used for LEDs must not only have high ultraviolet or blue light absorption ability and appropriate emission color, but also have high thermal stability and moisture stability. Therefore, Mn with excellent stability and luminescence performance 4+ The research and development of fluoride-doped phosphors has attracted much attention.

[0004] As we all know, when using Mn 4+ When solid-state light-emitting devices are made by doping fluoride phosphors, the large amount of heat generated by the device itself will cause the material to fail quickly, resulting in irreversible color shift of the device, which will seriously affect the Mn 4+ Doped fluoride phosphors are used in lighting and display fields. 4+ Another major problem with fluoride-doped phosphors is their inherent poor water stability. Studies have found that the dopant [MnF6]2- It is extremely sensitive to humidity and is easily hydrolyzed into mixed-valence manganese oxides and hydroxides during the degradation process of the fluorinated phosphor, causing the color of the fluorinated phosphor to darken and the red light emission intensity to weaken.

[0005] At present, the main strategy for improving degradation in domestic and foreign research is to form an organic or inorganic protective layer on the surface of the phosphor to make the humidity-sensitive [MnF6] 2- The groups are not exposed to a humid environment. However, inorganic surface passivation methods improve moisture resistance while reducing luminescence efficiency. For the core-shell structure method, most preparation processes are complicated and time-consuming, affecting actual production efficiency. Organic coatings are considered to be a method that can accurately control the thickness of the coating, have better moisture resistance, and do not affect luminescence efficiency.

[0006] Therefore, it is urgent to develop new red phosphors with better thermal stability and water resistance. Summary of the invention

[0007] The purpose of the present invention is to provide a stearic acid coated red phosphor and a preparation method and application thereof in order to overcome the defects of poor fluorescence thermal stability and water resistance stability of the red phosphor.

[0008] The purpose of the present invention can be achieved by the following technical solutions:

[0009] The present invention provides a stearic acid-coated red phosphor, wherein the red phosphor is Mn 4+ Doped fluoride, the typical representative formula is K2SiF6:Mn 4+ ;

[0010] The outer layer of the red phosphor is coated with hydrophobic stearic acid, and the molar ratio of stearic acid to K2MnF6 is (0.242-0.605):0.3.

[0011] Furthermore, the molar ratio of stearic acid to K2MnF6 is (0.242-0.605):0.3.

[0012] Furthermore, the excitation band of the red phosphor is in the range of 320-500 nm, and can be excited by ultraviolet light, violet light or blue light.

[0013] Furthermore, the emission band of the red phosphor is in the range of 580-680 nm, and the emission center is at 632 nm.

[0014] The present invention also provides a method for preparing a stearic acid-coated red phosphor, comprising the following steps:

[0015] S1: Dissolve KHF2 and KMnO4 in HF solution and keep stirring, then add H2O2 until solid precipitates, wash and dry to obtain the precursor K2MnF6;

[0016] S2: Dissolve the precursor K2MnF6 obtained in S1 in a fluosilicic acid solution, and then add KF until dissolved;

[0017] S3: Add stearic acid ethanol solution to the mixed solution in S2, continue stirring until the reaction is complete, and obtain the stearic acid-coated red phosphor after washing and drying.

[0018] Furthermore, in step S1, the mass ratio of KHF2 to KMnO4 is 20:1.

[0019] Furthermore, in step S1, the stirring time is 1-2 hours.

[0020] Furthermore, in step S1, the stirring speed is 400-600 rpm.

[0021] Furthermore, the drying temperature is 50-70° C., and the drying time is 8-12 hours.

[0022] Furthermore, in step S2, the molar ratio of KF to the precursor K2MnF6 is 100:3.

[0023] Furthermore, in step S3, the stirring speed is 500-900 rpm.

[0024] Furthermore, in step S3, the stirring time is 15-60 min.

[0025] The present invention adopts a simple coprecipitation method, and through emulsification reaction with stearic acid, the prepared Mn 4+ The surface of the fluoride-doped red phosphor is coated with a hydrophobic organic high-boiling-point stearic acid layer.

[0026] The chemical formula of stearic acid is C 18 H 36 O2 is an 18-carbon saturated fatty acid lipid with excellent hydrophobicity. The hydrophobicity of stearic acid mainly comes from its long-chain fatty acid structure, which makes it difficult to interact with water molecules, thus showing hydrophobic properties. In addition, the boiling point of stearic acid is about 361°C, which is also the reason why it has good thermal stability.

[0027] The present invention also provides an application of a stearic acid-coated red phosphor, wherein the red phosphor is used for preparing a warm white light LED.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] (1) The red phosphor of the present invention can be prepared by emulsifying with stearic acid. 4+ The surface of the fluoride-doped red phosphor is coated with a hydrophobic organic high-boiling-point stearic acid layer, which can significantly improve the fluorescence thermal stability and water resistance stability of the red phosphor.

[0030] (2) The present invention adopts a simple coprecipitation method to obtain Mn 4+ The surface of the fluoride-doped red phosphor is coated with a stearic acid layer, the preparation process is simple, and it is conducive to industrial production.

[0031] (3) The red phosphor prepared by the present invention has a wide excitation band, can be excited by ultraviolet light, purple light, and blue light, and can achieve narrow-band red light emission with an emission center at about 632 nm. Moreover, the stearic acid coating does not affect the fluorescence properties of the red phosphor itself.

[0032] (4) The red phosphor of the present invention can be well matched with various existing ultraviolet, purple, blue and other chips to meet the needs of the commercial market, and can be used to prepare white light LEDs with stable color temperature excited by blue light. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the XRD diagram of the red phosphor of Example 2 of the present invention.

[0034] Figure 2 The excitation spectra and emission spectra of the red phosphors of Examples 1-3 and Comparative Example 1 of the present invention (excitation wavelength is 455 nm) are shown.

[0035] Figure 3 The emission spectra of the red phosphors prepared in Comparative Example 1 and Example 2 vary with temperature under 455 nm excitation.

[0036] Figure 4 The emission spectra of the red phosphors prepared in Comparative Example 1 and Example 2 under 455 nm excitation after being immersed in deionized water for 18 days. DETAILED DESCRIPTION

[0037] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0038] Unless otherwise specified, the reagents, methods, instruments and equipment used in the present invention are conventional reagents, methods, instruments and equipment in the art. Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0039] Embodiment 1:

[0040] This embodiment provides a stearic acid-coated Mn 4+ The preparation method of fluoride-doped red phosphor is as follows:

[0041] S1 Precursor preparation: 18.00g KHF2 and 0.9g KMnO4 were dissolved in 60ml 40% HF solution, stirred continuously at 500rpm for 1h, and then a small amount of 30% H2O2 was added dropwise to the mixture until yellow powder precipitated. The precipitate was collected by centrifugation at 8000rpm, washed with acetone, and vacuum dried at 60℃ for 10h to obtain the precursor K2MnF6.

[0042] S2: Place the above-mentioned precursor K2MnF6 in a plastic beaker filled with 30% fluorosilicic acid solution and stir until completely dissolved; weigh the raw material KF according to the molar ratio of K2MnF6 to KF of 3:100, add it to an appropriate amount of deionized water, stir until completely dissolved, and then add it to the above-mentioned fluorosilicic acid solution.

[0043] S3: Stearic acid was weighed according to the molar ratio of stearic acid to K2MnF6 of 0.242:0.3, placed in a glass beaker filled with hot ethanol, cooled, added to the mixed solution of S2, and stirred vigorously at 800rpm for 15min until the reaction was complete. Centrifuged at 8000rpm to obtain a precipitate, which was washed with ethanol 2-3 times, and the obtained precipitate was placed in a 60℃ oven and dried for 12h to obtain stearic acid-coated Mn 4+ Fluoride-doped red phosphor.

[0044] Embodiment 2:

[0045] This embodiment provides a stearic acid-coated Mn 4+ The preparation method of fluoride-doped red phosphor is as follows:

[0046] S1 Precursor preparation: 18.00g KHF2 and 0.9g KMnO4 were dissolved in 60ml 40% HF solution, stirred continuously at 500rpm for 1h, and then a small amount of 30% H2O2 was added dropwise to the mixture until yellow powder precipitated. The precipitate was collected by centrifugation at 8000rpm, washed with acetone, and vacuum dried at 60℃ for 10h to obtain the precursor K2MnF6.

[0047] S2: Place the above-mentioned precursor K2MnF6 in a plastic beaker filled with 30% fluorosilicic acid solution and stir until completely dissolved; weigh the raw material KF according to the molar ratio of K2MnF6 to KF of 3:100, add it to an appropriate amount of deionized water, stir until completely dissolved, and then add it to the above-mentioned fluorosilicic acid solution.

[0048] S3: Stearic acid was weighed according to the molar ratio of stearic acid to K2MnF6 of 0.484:0.3, placed in a glass beaker filled with hot ethanol, cooled, added to the mixed solution of S2, and stirred vigorously at 800rpm for 15min until the reaction was complete. Centrifuged at 8000rpm to obtain a precipitate, which was washed with ethanol 2-3 times, and the obtained precipitate was placed in a 60℃ oven and dried for 12h to obtain stearic acid-coated Mn 4+ Fluoride-doped red phosphor.

[0049] Embodiment 3:

[0050] This embodiment provides a stearic acid-coated Mn 4+ The preparation method of fluoride-doped red phosphor is as follows:

[0051] S1 Precursor preparation: 18.00g KHF2 and 0.9g KMnO4 were dissolved in 60ml 40% HF solution, stirred continuously at 500rpm for 1h, and then a small amount of 30% H2O2 was added dropwise to the mixture until yellow powder precipitated. The precipitate was collected by centrifugation at 8000rpm, washed with acetone, and vacuum dried at 60℃ for 10h to obtain the precursor K2MnF6.

[0052] S2: Place the above-mentioned precursor K2MnF6 in a plastic beaker filled with 30% fluorosilicic acid solution and stir until completely dissolved; weigh the raw material KF according to the molar ratio of K2MnF6 to KF of 3:100, add it to an appropriate amount of deionized water, stir until completely dissolved, and then add it to the above-mentioned fluorosilicic acid solution.

[0053] S3: Stearic acid was weighed according to the molar ratio of stearic acid to K2MnF6 of 0.605:0.3, placed in a glass beaker filled with hot ethanol, cooled, added to the mixed solution of S2, and stirred vigorously at 800rpm for 15min until the reaction was complete. Centrifuged at 8000rpm to obtain a precipitate, which was washed with ethanol 2-3 times, and the obtained precipitate was placed in a 60℃ oven and dried for 12h to obtain stearic acid-coated Mn 4+ Fluoride-doped red phosphor.

[0054] Comparative Example 1:

[0055] This comparative example provides a Mn that is not coated with stearic acid. 4+ The preparation method of fluoride-doped red phosphor is as follows:

[0056] S1 Precursor preparation: 18.00g KHF2 and 0.9g KMnO4 were dissolved in 60ml 40% HF solution, stirred continuously at 500rpm for 1h, and then a small amount of 30% H2O2 was added dropwise to the mixture until yellow powder precipitated. The precipitate was collected by centrifugation at 8000rpm, washed with acetone, and vacuum dried at 60℃ for 10h to obtain the precursor K2MnF6.

[0057] S2: Place the above-mentioned precursor K2MnF6 in a plastic beaker filled with 30% fluorosilicic acid solution and stir until completely dissolved; weigh the raw material KF according to the molar ratio of K2MnF6 to KF of 3:100, add it to an appropriate amount of deionized water, stir until completely dissolved, and then add it to the above-mentioned fluorosilicic acid solution.

[0058] S3: Centrifuge at 8000 rpm to obtain a precipitate, wash with ethanol 2-3 times, and dry the precipitate in a 60°C oven for 12 h to obtain Mn without stearic acid coating. 4+ Fluoride-doped red phosphor.

[0059] The present invention uses X-ray diffraction (Ultima IV-185) to study the crystal structure of the product coated with stearic acid in Example 2, with a scanning angle 2θ ranging from 10 to 70°, to obtain the XRD test data of the sample in Example 2. Figure 1 It can be seen that the sample is consistent with the standard card, indicating that the stearic acid coating does not have a significant effect on the crystal structure, and the obtained red phosphor is a pure phase substance.

[0060] The present invention uses a fluorescence spectrometer (HITACHI F-7000) to test the spectral properties of the phosphors of Examples 1-3 and the comparative example. Figure 2 The results show that K2SiF6:Mn4 + The red phosphor of the system has a wide excitation band, covering the ultraviolet, purple and blue light regions, with peaks near 353nm and 455nm. The spectral peak is high, indicating that it can be effectively excited by ultraviolet, purple and blue light chips, and matches well with a variety of commercial chips. Under the excitation of 455nm blue light, the phosphor emits bright red light, and the emission spectrum is a very narrow emission band (580-680nm), with a peak at 632nm. And the stearic acid coating on the outer layer of the red phosphor will not affect the excitation and emission bands of the phosphor.

[0061] The present invention conducts thermal stability and water resistance tests on the red phosphor coated with stearic acid in Example 2 and the red phosphor not coated with stearic acid in Comparative Example 1. The specific test process is as follows:

[0062] (1) Thermal stability test: The samples were placed on a heating stage (77-873 K, THMS 600, Linkam Scientific instrument), and the emission spectra of the samples were recorded at 303-483 K using a Hitachi F-7000 spectrometer.

[0063] (2) Water resistance test: After the red phosphor was immersed in deionized water for 18 days, the emission spectrum was tested under 455nm excitation.

[0064] The test results of thermal stability are as follows Figure 3 As shown in the figure, with the increase of temperature, the fluorescence emission intensity of the red phosphor in comparative example 1 which is not coated with stearic acid gradually decreases. When the temperature rises to 483K, the fluorescence emission intensity is only 20% of the initial fluorescence intensity; while the fluorescence emission intensity of the red phosphor coated with stearic acid remains basically unchanged, and is also maintained above 90% at 483K, which proves that the red phosphor coated with stearic acid has good fluorescence thermal stability.

[0065] The results of the water resistance test are as follows Figure 4 As shown, after immersion in water for 18 days, the emission intensity of the red phosphor coated with stearic acid still remains above 93% of the initial intensity, which is a significant improvement compared with the red phosphor of Comparative Example 1, indicating that the coating of hydrophobic organic stearic acid can significantly improve the water resistance of the red phosphor.

[0066] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A stearic acid coated red phosphor, It is characterized in that The red phosphor is Mn 4+ Doped fluoride, the typical representative formula is K 2 SiF 6 :Mn 4+ ; The outer layer of the red phosphor is coated with hydrophobic stearic acid, and the stearic acid and K 2 Mn 6 The molar ratio is (0.242-0.605):0.

3.

2. The stearic acid-coated red phosphor according to claim 1, It is characterized in that The stearic acid and K 2 Mn 6 The molar ratio is (0.242-0.605):0.

3.

3. The stearic acid-coated red phosphor according to claim 1, It is characterized in that The red phosphor has an excitation band range of 320-500 nm and can be excited by ultraviolet light, violet light or blue light.

4. The stearic acid-coated red phosphor according to claim 1, It is characterized in that The emission band of the red phosphor is in the range of 580-680 nm, and the emission center is at 632 nm.

5. A method for preparing the stearic acid-coated red phosphor according to any one of claims 1 to 4, It is characterized in that The following steps are involved: S1: KHF 2 and KMnO 4 Dissolve in HF solution and continue stirring, then add H 2 O 2 Until the solid is precipitated, the precursor K can be obtained after washing and drying. 2 Mn 6 ; S2: The precursor K obtained in S1 2 Mn 6 In the fluosilicic acid solution, KF is then added until dissolved; S3: Add stearic acid ethanol solution to the mixed solution in S2, continue stirring until the reaction is complete, and obtain the stearic acid-coated red phosphor after washing and drying.

6. The method for preparing a stearic acid-coated red phosphor according to claim 5, It is characterized in that In step S1, the KHF 2 and KMnO 4 The mass ratio is 20:

1.

7. The method for preparing a stearic acid-coated red phosphor according to claim 5, It is characterized in that In step S1, the stirring time is 1-2h, and the stirring speed is 400-600rpm; The drying temperature is 50-70° C. and the drying time is 8-12 hours.

8. The method for preparing a stearic acid-coated red phosphor according to claim 5, It is characterized in that In step S2, the KF and the precursor K 2 Mn 6 The molar ratio is 100:

3.

9. The method for preparing a stearic acid-coated red phosphor according to claim 5, It is characterized in that In step S3, the stirring speed is 500-900 rpm, and the stirring time is 15-60 min.

10. Use of the stearic acid-coated red phosphor according to any one of claims 1 to 4, It is characterized in that The red phosphor is used to prepare warm white light LED.

Citation Information

Patent Citations

  • Surface modification method of Mn&lt;4+&gt; doped fluoride red fluorescent powder material

    CN107142102A

  • Coated manganese-activated complex fluoride phosphors

    US20170275529A1