Rare earth light conversion core-shell nano material with multi-wavelength excitation or pulse width regulation and control functions as well as preparation method and application of rare earth light conversion core-shell nano material

Through multi-wavelength excitation and pulse width control, the rare earth photoconversion core-shell nanomaterial NaYF4:Yb3+/Tm3+@NaYF4:Er3+/Ho3+ is realized to emit red, green and blue primary colors of rare earth nanomaterials, solving the problem of photons in the existing technology. The limitations of emission control provide more flexible optical performance adjustment and application potential.

CN118725866AActive Publication Date: 2024-10-01Yongkang Hardware Technician College +1

Patent Information

Application Number
CN202410790753.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-01
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

Existing rare earth-doped upconversion nanocrystals have limitations in regulating photon emission. In particular, it is difficult to achieve red, green, and blue primary color emission on a single nanoparticle, and high excitation power density leads to local heating and luminescence color changes, and large Most reports only show orthogonal emission characteristics of dual colors.

Method used

Using multi-wavelength excitation or pulse width control, the rare earth photoconversion core-shell nanomaterial NaYF4:Yb3+/Tm3+@NaYF4:Er3+/Ho3+ is used to produce red light through continuous excitation at 1532nm, blue light through 980nm excitation, and green light under short pulse excitation at 1532nm. For light emission, adjust the excitation pulse time to control the luminescence color.

Benefits of technology

It achieves the emission of red, green and blue primary colors of rare earth light conversion materials under low-cost and simple preparation processes, and significantly adjusts the optical properties by adjusting excitation conditions. It is suitable for fields such as biomedical imaging, three-dimensional display and super-resolution nanomicroscopes. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725866A_ABST
    Figure CN118725866A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of rare earth light conversion materials, and discloses a rare earth light conversion core-shell nano material with multi-wavelength excitation or pulse width regulation and control functions as well as a preparation method and application of the rare earth light conversion core-shell nano material. The material is a rare earth light conversion material NaYF4: Yb < 3 + > / Tm < 3 + > / NaYF4: Er < 3 + > / Ho < 3 + > / NaYF4 doped in different shell layers based on different sensitizers (Yb < 3 + > and Er < 3 + >) and activators (Tm < 3 + > and Ho < 3 + >), and is prepared by adopting a thermal decomposition method. Under continuous excitation of 1532 nm, the rare earth light conversion material emits bright red light. Under continuous excitation of 980 nm, the material emits blue light. Under the excitation of 1532nm short pulse, the material emits green light. By adjusting the 1532nm excitation pulse time, the regulation and control of three primary colors of red, green and blue of the rare earth light conversion material can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of rare earth light conversion materials, and relates to a rare earth light conversion core-shell nanomaterial with multi-wavelength excitation or pulse width regulation, and a preparation method and application thereof, and in particular to a method for producing a rare earth light conversion core-shell nanomaterial that can emit red, green and blue primary colors through multi-wavelength excitation or pulse width regulation. Background Art

[0002] As one of the most promising luminescent nanomaterials, rare earth-doped upconversion nanocrystals have attracted great attention due to their unique anti-Stokes shift. Based on 4f electronic transitions and near-infrared excitation, the upconversion luminescence of rare earth ions has unique photophysical properties, including narrow-band emission, long fluorescence lifetime, high photochemical stability, and low background interference. In addition, rare earth upconversion nanocrystals with finely tunable multicolor emission are more attractive than quantum dots and organic dyes because the energy transfer process, emission color, and surface effects can be flexibly controlled at the nanoscale. In recent years, regulating the photon emission of rare earth-doped upconversion nanocrystals has become a hot topic of research due to their great potential in a wide range of applications, including biomedicine, three-dimensional display, super-resolution nanoscopy, and information security. In general, designing upconversion nanocrystals with specific emission characteristics to meet their target applications is one of the most critical requirements. Although a lot of work has been devoted to designing upconversion nanocrystals with luminescence regulation, current strategies still have great limitations, such as severe local heating caused by the use of high excitation power density and changes in luminescence color that vary with excitation power density. In addition, most reported upconversion nanocrystals only show dual-color based orthogonal emission characteristics. As an indispensable component of full-color emission, red, green and blue primary color upconversion luminescence usually plays a key role in many applications. However, the three-primary color emission on a single nanoparticle is less studied. Therefore, in order to overcome these limitations, it is urgent to develop a new type of upconversion nanocrystal that can generate red, green and blue primary color emission under selective near-infrared excitation. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the prior art, provide a rare earth light conversion core-shell nanomaterial with simple preparation process and low production cost, and realize red, green and blue primary color luminescence.

[0004] A rare earth photoconversion core-shell nanomaterial with multi-wavelength excitation or pulse width regulation, the chemical formula is: NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4The rare earth light conversion core-shell nanomaterial emits bright red light under continuous excitation at 1532nm; emits blue light under continuous excitation at 980nm; emits green light under short pulse excitation at 1532nm; and the luminescent color of the rare earth light conversion material can be controlled by adjusting the pulse time of 1532nm excitation.

[0005] A method for preparing a rare earth light conversion core-shell nanomaterial with multi-wavelength excitation or pulse width regulation comprises the following steps:

[0006] (1) Weigh Na(CF) in proportion 3 CO 2 ) 3 , Y(CF 3 CO 2 ) 3 , Yb(CF 3 CO 2 ) 3 , Tm(CF 3 CO 2 ) 3 , then add oleic acid, oleylamine and octadecene mixed solvent, place the solution in a three-necked flask, heat it to 120-180°C and react for 0.1-2h to form a rare earth-oleic acid complex;

[0007] (2) The rare earth-oleic acid complex obtained in step (1) is reacted at 270-320° C. for 0.5-3 h. After the reaction is completed, the three-necked flask is cooled to room temperature, ethanol is added, centrifuged, and washed with cyclohexane and ethanol to obtain NaYF 4 :Yb 3+ / Tm 3+ , dissolved in cyclohexane;

[0008] (3) Weigh Na(CF 3 CO 2 ) 3 , Y(CF 3 CO 2 ) 3 , Er(CF 3 CO 2 ) 3 , Ho(CF 3 CO 2 ) 3 , then add oleic acid, oleylamine and octadecene mixed solvent, place the solution in a three-necked flask, heat it to 120-180°C and react for 0.1-2h to form a precursor solution, i.e., a rare earth-oleic acid complex;

[0009] (4) The precursor solution in step (3) is cooled to room temperature, and the product NaYF 4 :Yb3+ / Tm 3+ Pour the mixture into the three-necked flask in step (3), heat the solution to 80-120°C for reaction for 0.1-1h, and then cool the solution to room temperature;

[0010] (5) The product obtained in step (4) was then reacted at 270-310° C. for 0.5-3 h. After the reaction was completed, the three-necked flask was cooled to room temperature, ethanol was added, centrifuged, and washed with cyclohexane and ethanol to obtain NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ , dissolved in cyclohexane;

[0011] (6) Weigh Na(CF) in proportion 3 CO 2 ) 3 and Y(CF 3 CO 2 ) 3 , then add oleic acid, oleylamine and octadecene mixed solvent, place the solution in a three-necked flask, heat it to 120-180°C and react for 0.1-2h to form a precursor solution, i.e., a rare earth-oleic acid complex;

[0012] (7) The precursor solution in step (6) is cooled to room temperature, the product in step (5) is poured into the three-necked flask in step (6), the solution is heated to 80-120° C. and reacted for 0.1-1 h, and then the solution is cooled to room temperature;

[0013] (8) The product obtained in step (7) was then reacted at 270-310° C. for 0.5-3 h. After the reaction was completed, the three-necked flask was cooled to room temperature, ethanol was added, centrifuged, and washed with cyclohexane and ethanol to obtain NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 , dissolved in cyclohexane.

[0014] In step (1), Na(CF 3 CO 2 ) 3 , Y(CF 3 CO 2 ) 3 , Yb(CF 3 CO 2 ) 3 , Tm(CF 3 CO2 ) 3 The feed ratio is Na: (Y + Yb + Tm) in a molar ratio of 2.5:1, wherein the molar ratio of Y: Yb: Tm is a: b: c; the total molar amount of a, b and c is 100%, and the molar ratio of b and c is (0.01-0.9): (0.002-0.02);

[0015] In step (3), Na(CF 3 CO 2 ) 3 , Y(CF 3 CO 2 ) 3 , Er(CF 3 CO 2 ) 3 , Ho(CF 3 CO 2 ) 3 The feed ratio is Na: (Y + Er + Ho) with a molar ratio of 2.5:1, wherein the molar ratio of Y: Er: Ho is d: e: f; the total molar amount of d, e and f is 100%, wherein the molar ratio of e and f is (0.002-0.1): (0.002-0.02);

[0016] In step (5), NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ Medium,NaYF 4 :Yb 3+ / Tm 3+ and NaYF 4 :Er 3+ / Ho 3 + ) in a molar ratio of 1:1.

[0017] In step (6), Na(CF 3 CO 2 ) 3 and Y(CF 3 CO 2 ) 3 The feed ratio is the molar ratio of Na:Y 2.5:1;

[0018] In step (8), NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4Medium,NaYF 4 :Yb 3+ / Tm 3+ ,NaYF 4 :Er 3 + / Ho 3+ and NaYF 4 The molar ratio is 1:1:1.

[0019] In steps (1), (3) and (6), in the mixed solvent of oleic acid, oleylamine and octadecene, the volume ratio of oleic acid, oleylamine and octadecene is 3:1:1.

[0020] The multi-wavelength excitation or pulse width controlled rare earth light conversion core-shell nanomaterial of the present invention is used for biomedical imaging, three-dimensional display, super-resolution nano-microscopy or anti-counterfeiting coding.

[0021] The beneficial effects of the present invention are:

[0022] (1) Using a 1532 nm continuous near-infrared laser to excite NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 The Edinburgh FLS980 fluorescence steady-state transient fluorescence spectrometer was used to measure the NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 The light conversion material was tested for fluorescence spectrum. Under 1532 nm excitation, the rare earth light conversion material NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 Emits bright red light.

[0023] (2) Using a 980 nm near-infrared laser to excite NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 The Edinburgh FLS980 fluorescence steady-state transient fluorescence spectrometer was used to measure the NaYF4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 The light conversion material was tested for fluorescence spectrum. Under 980 nanometer excitation, the rare earth light conversion material NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 Emits blue light.

[0024] (3) Use a 1532 nm short pulse near-infrared laser to excite NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 The Edinburgh FLS980 fluorescence steady-state transient fluorescence spectrometer was used to measure the NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 Fluorescence spectrum test of light conversion materials. Under 1532nm short pulse excitation, the rare earth light conversion material NaYF 4 :Yb 3 + / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 Green light is emitted. By adjusting the pulse time of 1532nm excitation, the luminescent color of the rare earth light conversion material can be adjusted.

[0025] (4) The universally applicable design strategy of the present invention provides more options for the construction of rare earth light conversion materials and can significantly adjust their optical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is the XRD diffraction pattern of the rare earth light conversion material of Example 1 of the present invention.

[0027] Figure 2 This is the TEM spectrum of the rare earth light conversion material of Example 1 of the present invention.

[0028] Figure 3 In the figure, a, b, and c are the emission spectra of the rare earth light conversion material under 1532 nm and 980 nm continuous light excitation and 1532 nm short pulse excitation, respectively, of Example 1 of the present invention.

[0029] Figure 4 The emission spectra (a) and luminescent photographs (b) of the rare earth light conversion material under excitation of different pulse widths at 1532 nm according to Example 1 of the present invention are shown. DETAILED DESCRIPTION

[0030] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific examples.

[0031] Example 1

[0032] The rare earth light conversion core-shell structure NaYF of the present invention realizes red, green and blue primary color luminescence through multi-wavelength excitation and pulse width regulation 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 (Yb mole percentage 20% / Tm mole percentage 0.5% / Er mole percentage 20% / Ho mole percentage 0.5%), the preparation method comprises the following steps:

[0033] Raw materials: 1mmol Na(CF 3 CO 2 ) 3 , 0.358mmol Y(CF 3 CO 2 ) 3 , 0.04mmol Yb(CF 3 CO 2 ) 3 , 0.002mmol Tm(CF 3 CO 2 ) 3 .

[0034] (1) Weigh 1 mmol Na(CF 3 CO 2 ) 3 , 0.358mmol Y(CH 3 CO 2 ) 3 , 0.04mmol Yb(CH 3 CO 2 ) 3, 0.002mmol Tm(CH 3 CO 2 ) 3 , 6 mL of oleic acid, 2 mL of oleylamine and 2 mL of octadecene were added to a three-necked flask, and the solution was heated to 120°C for 0.5 h to form a rare earth-oleic acid complex;

[0035] Then the reaction was continued at 320°C for 1 hour. After the reaction was completed, the three-necked flask was cooled to room temperature, ethanol was added, centrifuged, and washed with cyclohexane and ethanol. The product NaYF 4 :Yb 3+ / Tm 3+ Soluble in cyclohexane.

[0036] (2) Weigh 1 mmol Na(CF 3 CO 2 ) 3 , 0.358mmol Y(CH 3 CO 2 ) 3 , 0.04mmol Er(CH 3 CO 2 ) 3 , 0.002mmol Ho(CH 3 CO 2 ) 3 , 6 mL of oleic acid, 2 mL of oleylamine and 2 mL of octadecene were added to a three-necked flask, and the solution was heated to 120°C for 0.5 h to form a rare earth-oleic acid complex;

[0037] The precursor solution was cooled to room temperature, the product in step (1) was poured into a three-necked flask, the solution was heated to 100°C for reaction for 0.5h, and then the solution was cooled to room temperature;

[0038] Then the reaction was continued at 320°C for 1 hour. After the reaction was completed, the three-necked flask was cooled to room temperature, ethanol was added, centrifuged, and washed with cyclohexane and ethanol. The product NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ Soluble in cyclohexane.

[0039] (3) Weigh 1 mmol Na(CF 3 CO 2 ) 3 , 0.4mmol Y(CH 3 CO 2 ) 3, 6 mL of oleic acid, 2 mL of oleylamine and 2 mL of octadecene were added to a three-necked flask, and the solution was heated to 120°C for 0.5 h to form a rare earth-oleic acid complex;

[0040] The precursor solution was cooled to room temperature, the product in step (2) was poured into a three-necked flask, the solution was heated to 100°C for reaction for 0.5h, and then the solution was cooled to room temperature;

[0041] Then the reaction was continued at 320°C for 1 hour. After the reaction was completed, the three-necked flask was cooled to room temperature, ethanol was added, centrifuged, and washed with cyclohexane and ethanol. The product NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 Soluble in cyclohexane.

[0042] The XRD diffraction patterns and TEM patterns of the obtained products are shown in Figure 1 , 2, prove that the present invention synthesized pure NaYF 4 The matrix has a uniform morphology.

[0043] A method for realizing rare earth light conversion core-shell structure of red, green and blue primary color luminescence through multi-wavelength excitation and pulse width control, the specific method is:

[0044] (1) Using a 1532 nm continuous near-infrared laser to excite the NaYF obtained in Example 1 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 The Edinburgh FLS980 fluorescence steady-state transient fluorescence spectrometer was used to measure the NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 The light conversion material is tested for fluorescence spectrum. Figure 3 As shown in a, under continuous excitation at 1532 nm, the rare earth photoconversion material NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 Emits bright red light.

[0045] (2) Using a 980 nm continuous near-infrared laser to excite the NaYF obtained in Example 1 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 The Edinburgh FLS980 fluorescence steady-state transient fluorescence spectrometer was used to measure the NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3 + / Ho 3+ @NaYF 4 The light conversion material is tested for fluorescence spectrum. Figure 3 As shown in b, under continuous excitation at 980 nm, the rare earth photoconversion material NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 Emits blue light.

[0046] (3) Use a 1532 nm short pulse near-infrared laser to excite NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 The Edinburgh FLS980 fluorescence steady-state transient fluorescence spectrometer was used to measure the NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 The light conversion material is tested for fluorescence spectrum. Figure 3 As shown in c, under 1532 nm short pulse excitation, the rare earth photoconversion material NaYF 4 :Yb 3+ / Tm 3+ @NaYF 4 :Er 3+ / Ho 3+ @NaYF 4 Emits green light.

[0047] like Figure 4 As shown, by adjusting the pulse time of 1532nm excitation, the luminescent color of the rare earth light conversion material can be controlled. 200μs~1ms is green light, 3~5ms is yellow light, and more than 7ms is red light.

[0048] Finally, it should be emphasized that the above examples are only used to illustrate the technical solution of the present invention, rather than to limit the protection scope of the present invention. Although we have described the preferred implementation in detail, professionals should understand that they can be modified or replaced by equivalents without departing from the core and scope of the technical solution of the present invention.

Claims

1. A rare earth light conversion core-shell nanomaterial with multi-wavelength excitation or pulse width regulation, characterized in that: The chemical formula is: NaYF4:Yb 3+ / Tm 3+ @NaYF4:Er 3+ / Ho 3+ @NaYF4, the rare earth photoconversion core-shell nanomaterial emits bright red light under continuous excitation at 1532nm; under continuous excitation at 980nm, the material emits blue light; under short pulse excitation at 1532nm, the material emits green light; by adjusting the pulse time of 1532nm excitation, the luminescent color of the rare earth photoconversion material can be controlled.

2. The method for preparing the rare earth light conversion core-shell nanomaterial with multi-wavelength excitation or pulse width modulation according to claim 1, characterized in that: (1) Weighing Na(CF3CO2)3, Y(CF3CO2)3, Yb(CF3CO2)3, and Tm(CF3CO2)3 in proportion, then adding them into a mixed solvent of oleic acid, oleylamine, and octadecene, placing the solution in a three-necked flask, heating it to 120-180°C, and reacting it for 0.1-2h to form a rare earth-oleic acid complex; (2) The rare earth-oleic acid complex obtained in step (1) is reacted at 270-320° C. for 0.5-3 h. After the reaction is completed, the three-necked flask is cooled to room temperature, ethanol is added, centrifuged, and washed with cyclohexane and ethanol to obtain NaYF4:Yb 3+ / Tm 3+ , dissolved in cyclohexane; (3) Weigh Na(CF3CO2)3, Y(CF3CO2)3, Er(CF3CO2)3, and Ho(CF3CO2)3 in proportion, add them to a mixed solvent of oleic acid, oleylamine, and octadecene, place the solution in a three-necked flask, heat it to 120-180°C, and react for 0.1-2h to form a precursor solution, i.e., a rare earth-oleic acid complex; (4) The precursor solution in step (3) is cooled to room temperature, and the product NaYF4:Yb 3+ / Tm 3+ Pour the mixture into the three-necked flask in step (3), heat the solution to 80-120°C for reaction for 0.1-1h, and then cool the solution to room temperature; (5) The product obtained in step (4) was then reacted at 270-310°C for 0.5-3h. After the reaction was completed, the three-necked flask was cooled to room temperature, ethanol was added, centrifuged, and washed with cyclohexane and ethanol to obtain NaYF4:Yb 3+ / Tm 3+ @NaYF4:Er 3+ / Ho 3+ , dissolved in cyclohexane; (6) weighing Na(CF3CO2)3 and Y(CF3CO2)3 in proportion, then adding them to a mixed solvent of oleic acid, oleylamine and octadecene, placing the solution in a three-necked flask, heating it to 120-180°C and reacting it for 0.1-2h to form a precursor solution, i.e., a rare earth-oleic acid complex; (7) The precursor solution in step (6) is cooled to room temperature, the product in step (5) is poured into the three-necked flask in step (6), the solution is heated to 80-120° C. and reacted for 0.1-1 h, and then the solution is cooled to room temperature; (8) The product obtained in step (7) was then reacted at 270-310° C. for 0.5-3 h. After the reaction was completed, the three-necked flask was cooled to room temperature, ethanol was added, centrifuged, and washed with cyclohexane and ethanol to obtain NaYF4:Yb 3+ / Tm 3+ @NaYF4:Er 3+ / Ho 3+ @NaYF4, dissolved in cyclohexane.

3. The preparation method according to claim 2, characterized in that: In step (1), the feed ratio of Na(CF3CO2)3, Y(CF3CO2)3, Yb(CF3CO2)3, and Tm(CF3CO2)3 is a molar ratio of Na:(Y+Yb+Tm) of 2.5:1, wherein the molar ratio of Y:Yb:Tm is a:b:c; the total molar amount of a, b and c is 100%, and the molar ratio of b and c is (0.01-0.9):(0.002-0.02).

4. The preparation method according to claim 2, characterized in that: In step (3), the feed ratio of Na(CF3CO2)3, Y(CF3CO2)3, Er(CF3CO2)3, and Ho(CF3CO2)3 is a molar ratio of Na:(Y+Er+Ho) of 2.5:1, wherein the molar ratio of Y:Er:Ho is d:e:f; the total molar amount of d, e, and f is 100%, wherein the molar ratio of e and f is (0.002-0.1):(0.002-0.02).

5. The preparation method according to claim 2, characterized in that: In step (5), NaYF4:Yb 3+ / Tm 3+ @NaYF4:Er 3+ / Ho 3+ In NaYF4:Yb 3+ / Tm 3+ and NaYF4:Er 3+ / Ho 3+ ) in a molar ratio of 1:

1.

6. The preparation method according to claim 2, characterized in that: In step (6), the feed ratio of Na(CF3CO2)3 and Y(CF3CO2)3 is a molar ratio of Na:Y of 2.5:

1.

7. The preparation method according to claim 2, characterized in that: In step (8), NaYF4:Yb 3+ / Tm 3+ @NaYF4:Er 3+ / Ho 3+ @NaYF4, the molar ratio of NaYF4:Yb 3+ / Tm 3+ , NaYF4:Er 3+ / Ho 3+ and NaYF4 is 1:1:

1.

8. The preparation method according to claim 2, characterized in that: In steps (1), (3) and (6), in the mixed solvent of oleic acid, oleylamine and octadecene, the volume ratio of oleic acid, oleylamine and octadecene is 3:1:

1.

9. Use of the multi-wavelength excited or pulse width modulated rare earth light conversion core-shell nanomaterial according to claim 1 for biomedical imaging, three-dimensional display, super-resolution nanomicroscopy or anti-counterfeiting coding.

Citation Information

Patent Citations

  • Method for preparing three-primary-color up-conversion luminescent material with orthogonal excitation-emission response

    CN111808604A

Cited By

  • Panchromatic upconversion single nanocrystal excited by single wavelength as well as preparation and application of panchromatic upconversion single nanocrystal

    CN120718652A