Ti / Ag / alpha-PbO2 / beta-PbO2 electrode as well as preparation method and application thereof
Through the Ti/Ag/α-PbO2/β-PbO2 electrode structure, the problems of insufficient brittleness and electrocatalytic capacity of Ti/PbO2 electrode are solved, and the long life and efficient electrocatalytic oxidation performance of the electrode are achieved, especially under acidic conditions. Stability and uniformity.
Patent Information
- Application Number
- CN202411396090.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-10-08
AI Technical Summary
In practical applications, Ti/PbO2 electrodes have problems such as brittleness, ease of inactivation, large internal stress in the electrode interface, peeling off the coating, and shortening of life. In addition, the dissolution of the Ag layer under acidic conditions leads to uneven coating and insufficient electrocatalytic capacity.
Using the Ti/Ag/α-PbO2/β-PbO2 electrode structure, the titanium matrix, the classic silver mirror reactive silver plating layer is etched by mixing acid, and the α-PbO2 and β-PbO2 layers are electrodeposited, combined with high-temperature heat treatment, a dense Ag layer is formed. The PbO2 layer with a quadrangular structure enhances the bonding force and conductivity of the electrodes, avoiding reactive oxygen penetration and dissolution of the Ag layer.
It significantly extends the service life of the electrode, improves the stability and electrocatalytic activity of the electrode, reduces the resistance of the electrode, and improves the degradation ability of organic pollutants.
Smart Images

Figure CN118993255A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrochemical technology, and in particular to a Ti / Ag / α-PbO2 / β-PbO2 electrode and a preparation method and application thereof. Background Art
[0002] Electrochemical catalytic oxidation technology is an important branch of the electrochemical technology field. It is an advanced oxidation technology that can effectively control environmental pollution. It has attracted widespread attention for its excellent characteristics such as simple operation, high efficiency, pollution-free and sustainability. It has been applied to the treatment of various types of wastewater such as dye wastewater and papermaking wastewater. Electrode materials are key components of electrochemical technology. PbO2 electrodes based on titanium have the advantages of low cost and high oxygen evolution potential and are widely used in the field of electrochemical technology. Active free radicals such as OH generated on the surface of the PbO2 active layer can directly react with organic pollutants, causing the organic pollutants to eventually decompose into H2O and CO2. However, in practical applications, Ti / PbO2 electrodes also have problems such as brittleness, easy deactivation, large internal stress at the electrode interface, easy coating shedding, and shortened life, which are greatly restricted in practical applications. In addition, when Ti / PbO2 electrodes are used for long-term electrocatalytic oxidation of organic pollutants, the electrolyte solution will corrode and dissolve the PbO2 active layer on the electrode surface, and finally the titanium substrate surface will be oxidized into weakly conductive TiO2, thereby accelerating the shedding of the PbO2 active layer, reducing the service life of the electrode, and reducing the electrocatalytic activity of the electrode. This has also greatly limited the practical application and promotion of Ti / PbO2 electrodes.
[0003] Adding a suitable intermediate layer can not only reduce the internal stress between the coatings, but also improve the corrosion resistance, chemical stability and service life of the electrode. The common tin antimony oxide intermediate layer and α-PbO2 intermediate layer can improve the service life of the electrode, but there are still problems such as insufficient electrocatalytic ability in practical applications. In addition, the metal oxide intermediate layer prepared by thermal decomposition has an irregular crack structure caused by alternating high temperature and room temperature, which is not conducive to the chemical stability and service life of the Ti / PbO2 electrode. When Ag is introduced as an intermediate layer into the titanium-based coated electrode under acidic conditions, due to E Θ Ag+ / Ag =0.7996 less than E Θ O2 / H2O =1.229, E Θ PbO2 / Pb 2+ =1.455. When PbO2 / β-PbO2 is directly electrodeposited on the surface of Ti / Ag electrode, the Ag layer on the surface of Ti / Ag electrode will dissolve and generate a large number of bubbles (O2), which will eventually lead to problems such as uneven and non-dense coating. Summary of the invention
[0004] The present invention provides a Ti / Ag / α-PbO2 / β-PbO2 electrode and a preparation method and application thereof, the purpose of which is to solve the above-mentioned problems existing in the background technology.
[0005] In order to achieve the above-mentioned purpose, the embodiment of the present invention provides a Ti / Ag / α-PbO2 / β-PbO2 electrode and its preparation method and application. The present invention has a simple production process, and the dense α-PbO2 layer can not only protect the Ag layer, but also effectively alleviate the penetration of active oxygen, greatly extending the service life of the electrode. β-PbO2 is a dense tetrahedral structure, which can also effectively prevent active oxygen from penetrating the electrode surface, protect the outer layer of the electrode from falling off, improve the electrode performance, extend the service life of the electrode, and provide abundant active sites for efficient electrocatalytic degradation of organic pollutants.
[0006] An embodiment of the present invention provides a method for preparing a Ti / Ag / α-PbO2 / β-PbO2 electrode, comprising the following steps:
[0007] S1: preparing a mixed acid solution and heating it, then placing the ultrasonically treated titanium substrate into the solution for etching to obtain a pretreated titanium substrate;
[0008] S2: Prepare a silver plating solution, suspend the pretreated titanium substrate in the silver plating solution for silver plating, take out the titanium substrate after the silver plating is completed, clean it with ultrapure water, and dry it naturally or in an oven; replace the silver plating solution, repeat the silver plating several times; and then perform high-temperature heat treatment to obtain a Ti / Ag electrode; wherein the silver layer is uniformly and densely attached to the surface of the titanium substrate and the silver layer maintains a morphology with moderate roughness. It should be noted that the silver layer prepared by the classic silver mirror reaction silver plating combined with high-temperature heat treatment has a structure with moderate roughness and a large specific surface area, which is conducive to the rapid electrodeposition of α-PbO2; secondly, the silver layer can react with the active oxygen that penetrates the α-PbO2 during the use of the electrode to generate conductive Ag2O, which effectively alleviates the problem of the coating being easy to fall off due to the formation of weakly conductive TiO2 on the surface of the titanium substrate;
[0009] S3: preparing an α-PbO2 electroplating solution and electro-depositing a Ti / Ag electrode in the α-PbO2 electroplating solution, and washing with deionized water to obtain a Ti / Ag / α-PbO2 electrode;
[0010] S4: Prepare a β-PbO2 electroplating solution and electro-deposit a Ti / Ag / α-PbO2 electrode in the β-PbO2 electroplating solution, and wash with deionized water to obtain a Ti / Ag / α-PbO2 / β-PbO2 electrode.
[0011] According to one aspect of the present invention, in step S1, the thickness of the titanium substrate is any one of 0.1 mm, 0.2 mm, and 0.3 mm; and the mixed acid solution includes sulfuric acid and tartaric acid.
[0012] According to one aspect of the present invention, in step S2, the silver plating solution includes silver salt, dilute ammonia water, strong base and reducing aldehyde.
[0013] According to one aspect of the present invention, the silver salt is silver nitrate with a concentration of 2.0 to 6.0 wt.%; the strong base is any one of sodium hydroxide and potassium hydroxide with a concentration of 1.0 to 4.0 wt.%; the reducing aldehyde is any one of glucose, formaldehyde, and acetaldehyde with a concentration of 3.0 to 7.0 wt.%; and the concentration of dilute ammonia water is 2.0 to 10.0 wt.%.
[0014] According to one aspect of the present invention, in step S2, the silver plating time is 20 min to 80 min; the number of silver plating is 1 to 5 times; the drying temperature is 30 to 50°C; and the heat treatment temperature is 350 to 500°C.
[0015] According to one aspect of the present invention, the specific process of electrodeposition in step S3 is: at 30-60°C and 2-7 mA / cm 2 Electrodeposition for 2 to 5 hours.
[0016] According to one aspect of the present invention, the specific process of electrodeposition in step S4 is: first, at 40-70°C, at 10 mA / cm 2 Electrodeposition for 10 to 30 minutes; then increase the current density by 5 mA / cm 2 Electrodeposition for 5 minutes, co-electrodeposition for 30 to 60 minutes.
[0017] Based on a general inventive concept, an embodiment of the present invention provides a Ti / Ag / α-PbO2 / β-PbO2 electrode obtained by the above-mentioned preparation method.
[0018] The embodiments of the present invention also provide the use of the Ti / Ag / α-PbO2 / β-PbO2 electrode obtained by the above-mentioned preparation method in electrochemical degradation of anthraquinone organic dye wastewater.
[0019] According to one aspect of the present invention, the anthraquinone organic dye is Alizarin Red S.
[0020] Reaction mechanism:
[0021] The present invention selects the metal Ag single substance with the best conductivity as the middle layer, and plates the Ag layer through the classic silver mirror reaction, so that the Ag layer is uniformly and completely attached to the titanium substrate with moderate surface roughness and uniform distribution. The Ag layer is further heat-treated at high temperature to improve the bonding force between the titanium substrate and the Ag layer, and the Ag layer after heat treatment still maintains the basic morphology with moderate surface roughness, increasing the coating coverage area; the Ag layer is used as the middle layer, not only does Ag have high conductivity, but Ag can also react with the active oxygen penetrating the surface of the active layer, and can also generate conductive Ag2O, effectively preventing active oxygen molecules or active oxygen atoms from diffusing to the surface of the titanium substrate, avoiding the generation of weakly conductive TiO2 on the surface of the titanium substrate, causing the coating to fall off, thereby improving the stability of the electrode. Selecting Ag single substance as the middle layer can not only significantly increase the bonding force between the titanium substrate and the PbO2 layer, but also increase the conductivity of the electrode, reduce the electrode resistance, improve the electrode stability, and enhance the service life of the electrode, and has great application potential in the field of electrochemical technology. Moreover, under alkaline conditions, depositing an α-PbO2 layer first and then a β-PbO2 layer on the surface of the Ti / Ag electrode can effectively avoid the dissolution of Ag on the surface of the Ti / Ag electrode to produce a large number of bubbles (O2), thereby causing problems such as uneven and non-dense coating.
[0022] The above scheme of the present invention has the following beneficial effects:
[0023] (1) The present invention performs mixed acid etching on the titanium substrate to obtain a titanium substrate with moderate surface roughness and uniform distribution, thereby increasing the contact area with the silver single layer; and then adopts the classic silver mirror reaction Ag plating method to effectively avoid CN in the process of Ag electrodeposition. - The Ag-plated titanium substrate is further sintered at high temperature to increase the bonding force between the titanium substrate and the Ag layer. After heat treatment, the Ag layer still maintains a moderate surface roughness and a large surface area, which is conducive to the rapid electrodeposition of the α-PbO2 layer, making the β-PbO2 layer more firmly bonded to the titanium substrate; the irregular crack structure unique to the intermediate layer prepared by thermal decomposition is avoided.
[0024] (2) The present invention first deposits an α-PbO2 layer on the surface of the Ti / Ag electrode under alkaline conditions, and then deposits a β-PbO2 layer, thereby effectively avoiding the key problem of direct electrodeposition of PbO2 / β-PbO2 layers on the surface of the Ti / Ag electrode, which would lead to the dissolution of the Ag layer. The highly conductive Ag is successfully introduced into the titanium-based coated electrode, which significantly increases the bonding force between the titanium substrate and the β-PbO2 active layer, improves the electrode conductivity, enhances the electrode stability, and increases the service life of the electrode.
[0025] (3) The principle of the design of the Ti / Ag / α-PbO2 / β-PbO2 electrode preparation process of the present invention is scientific and reliable, the preparation process is simple, no complicated equipment is required, the electrode has excellent electrocatalytic oxidation performance, and the difficulty of preparing complex titanium-based coating electrodes is greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 The AC impedance spectra of electrodes prepared in Example 1 and Comparative Example 1 of the present invention;
[0028] Figure 2 It is a graph showing accelerated life test of electrodes prepared in Example 1 of the present invention and Comparative Example 1;
[0029] Figure 3 This is a SEM image of the Ti / Ag electrode after silver plating heat treatment in Example 1 of the present invention;
[0030] Figure 4 This is the EDS image of the Ti / Ag electrode after silver plating heat treatment in Example 1 of the present invention;
[0031] Figure 5 This is a SEM image of the Ti / Ag / α-PbO2 electrode prepared in Example 1 of the present invention;
[0032] Figure 6 This is an EDS image of the Ti / Ag / α-PbO2 electrode prepared in Example 1 of the present invention;
[0033] Figure 7 This is an EDS image of the Ti / Ag / α-PbO2 electrode prepared in Example 1 of the present invention after the α-PbO2 layer is scraped off;
[0034] Figure 8 This is a SEM image of the Ti / Ag / α-PbO2 / β-PbO2 electrode prepared in Example 1 of the present invention;
[0035] Fig. 9 XRD patterns of Ti / Ag / α-PbO2 and Ti / Ag / α-PbO2 / β-PbO2 electrodes prepared in Example 1 of the present invention;
[0036] Fig.10 This is a graph showing the degradation rate of Alizarin Red S of electrodes prepared in the embodiments of the present invention and the comparative examples. DETAILED DESCRIPTION
[0037] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.
[0038] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0039] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0040] The existing tin antimony oxide intermediate layer and α-PbO2 intermediate layer have problems such as insufficient electrocatalytic ability in practical applications. For example, the metal oxide intermediate layer prepared by thermal decomposition has an irregular crack structure caused by alternating high temperature and room temperature, which is not conducive to the chemical stability and service life of the Ti / PbO2 electrode. When Ag is introduced as an intermediate layer into the titanium-based coating electrode under acidic conditions, due to E Θ Ag+ / Ag =0.7996 less than E Θ O2 / H2O =1.229, E Θ PbO2 / Pb 2+ =1.455. When PbO2 / β-PbO2 is directly electrodeposited on the surface of Ti / Ag electrode, the Ag layer on the surface of Ti / Ag electrode will dissolve and generate a large number of bubbles (O2), which will eventually lead to problems such as uneven and non-dense coating.
[0041] The embodiments of the present invention provide a Ti / Ag / α-PbO2 / β-PbO2 electrode and a preparation method and application thereof.
[0042] The following will be described through specific examples and comparative examples.
[0043] Example 1
[0044] The present embodiment involves a method for preparing a Ti / Ag / α-PbO2 / β-PbO2 electrode, and the specific process includes three steps: mixed acid etching of a titanium substrate, preparation of an Ag layer, and electrodeposition of a PbO2 layer:
[0045] (1) Mixed acid etching of titanium substrate
[0046] First, the titanium substrate was cut into 2 cm × 4 cm × 0.2 mm, ultrasonically cleaned in acetone for 40 min, then taken out with tweezers and dried for later use;
[0047] Then, 100 mL of 20% sulfuric acid solution and 15% tartaric acid solution were prepared respectively, sealed for later use, and the sulfuric acid and tartaric acid solutions were mixed in a volume ratio of 2:1 to prepare a mixed acid;
[0048] Finally, the mixed acid solution was heated to 100°C and placed into a titanium substrate for etching. The etching time was 60 minutes, and the titanium substrate was turned over every 20 minutes. After the etching was completed, the titanium substrate was taken out with tweezers and washed several times with deionized water, placed on filter paper, dried at room temperature, and sealed for storage.
[0049] (2) Preparation of Ag layer
[0050] First, prepare 50 mL each of 4.0 wt. % AgNO 3 solution, 8.0 wt. % dilute ammonia solution, 2.0 wt. % NaOH solution and 5.0 wt. % glucose solution, and seal and store them at room temperature for later use.
[0051] Then, 8 mL of AgNO3 (4.0 wt.%) solution was added to a beaker (25 mL), and 8.0 wt.% of dilute ammonia (about 5 mL) was added dropwise until the solution was just dissolved and the solution became clear and transparent. Then, the same volume of dilute ammonia was added dropwise, and then 8 mL of 5 wt.% NaOH solution was added (the solution did not turn black); under the stirring condition of 500 rpm, 12 mL of 5 wt.% glucose solution was added, and after continuous high-speed stirring for 5 s, the stirring was stopped, and 4 titanium substrates (2 cm × 4 cm × 0.2 mm) were clamped and suspended with paper clips, and suspended vertically into the above solution, and allowed to stand for 40 minutes after the silver mirror reaction, the silver-plated titanium substrate was taken out, washed with ultrapure water several times, dried in an oven at 30-50 ° C or dried naturally to obtain a Ti / Ag electrode. The silver plating solution was replaced, and the silver plating was repeated three times, and the electrode was dried.
[0052] After the last silver plating, the electrode was placed in a vacuum tube furnace for heat treatment at 400°C for 60 minutes and naturally annealed for more than 5 hours. The titanium substrate was taken out to obtain a Ti / Ag electrode with a strong bonding force between the Ti substrate and the Ag layer.
[0053] (3) The electrodeposition of the PbO2 layer includes firstly electrodepositing an α-PbO2 layer and then electrodepositing a β-PbO2 layer.
[0054] First, prepare 50 mL of α-PbO2 electroplating solution containing 0.1 mol / L PbO and 3.5 mol / L NaOH, and prepare 50 mL of β-PbO2 electroplating solution containing 0.5 mol / L Pb(NO3)2, 0.04 mol / L NaF, and 0.1 mol / L HNO3;
[0055] Then, the α-PbO2 layer was electrodeposited by low current density, with a Ti / Ag electrode (1 cm × 1 cm × 0.2 mm) after high temperature heat treatment as the anode and a platinum electrode of the same size as the cathode in a 40°C electroplating solution at 3 mA / cm 2 The electrode was electroplated at a low current density for 4 h; the electrode was taken out and washed with deionized water to obtain a Ti / Ag / α-PbO2 electrode.
[0056] Finally, the β-PbO2 active layer was prepared by step-by-step electrodeposition. The Ti / Ag / α-PbO2 electrode was used as the anode and the platinum electrode of the same size was used as the cathode. The β-PbO2 active layer was prepared by step-by-step electrodeposition. The Ti / Ag / α-PbO2 electrode was used as the anode and the platinum electrode of the same size was used as the cathode. 2 Electrodeposition was performed at a current density of 15, 20, 25, 30, 35, 40, 45, and 50 mA / cm 2 The current density was set to 0.50 and the electrode was electroplated for 5 min. The electrode was taken out and washed with deionized water to obtain a Ti / Ag / α-PbO2 / β-PbO2 electrode.
[0057] In the preparation process of the Ag intermediate layer involved in this embodiment, the classic silver mirror reaction Ag plating method is adopted to effectively avoid CN - The Ag-plated titanium substrate is further sintered at high temperature to increase the bonding force between the titanium substrate and the Ag layer. In addition, the Ti / Ag electrode still maintains a moderate surface roughness and a large surface area after heat treatment. On the one hand, the Ag layer structure is conducive to the rapid electrodeposition of a dense α-PbO2 layer to protect the Ti / Ag electrode; on the other hand, it makes the α-PbO2 more firmly bonded to the titanium substrate and rapidly electrodeposited to generate a stacked, dense tetrahedral structure of β-PbO2. Ag, as a highly conductive metal, can also react with active oxygen that penetrates the surface of the active layer to generate conductive Ag2O, effectively preventing oxygen molecules or oxygen atoms from diffusing to the surface of the titanium substrate, greatly alleviating the generation of weakly conductive TiO2 on the surface of the titanium substrate, and avoiding the shedding of the coating, thereby further improving the stability of the electrode. Under alkaline conditions, using a low current density to first deposit an α-PbO2 layer on the surface of the Ti / Ag electrode can effectively avoid the dissolution of Ag on the surface of the Ti / Ag electrode to produce a large number of bubbles (O2), thereby causing problems such as uneven and non-dense coating. Selecting an Ag layer as the intermediate layer of the Ti / PbO2 electrode can not only significantly increase the bonding force between the titanium substrate and the PbO2 layer, but also increase the conductivity of the electrode, reduce the electrode resistance, improve the electrode stability, and enhance the service life of the electrode. In addition, the β-PbO2 prepared by the present invention is a dense tetrahedral structure, which can effectively prevent oxygen molecules or oxygen atoms from diffusing to the surface of the titanium substrate, and increase the surface area of the active layer and the electrocatalytic oxidation active sites, and has great application potential in the field of electrochemical technology.
[0058] Comparative Example 1
[0059] The preparation process of a Ti / β-PbO2 electrode involved in this comparative example includes two steps: mixed acid etching of the titanium substrate and electrodeposition of the β-PbO2 layer:
[0060] (1) Mixed acid etching of titanium substrate
[0061] First, the titanium substrate was cut into 2 cm × 4 cm × 0.2 mm, ultrasonically cleaned in acetone for 40 min, then taken out with tweezers and dried for later use;
[0062] Then, 100 mL of 20% sulfuric acid solution and 15% tartaric acid solution were prepared respectively, sealed for later use, and the sulfuric acid and tartaric acid solutions were mixed in a volume ratio of 2:1 to prepare a mixed acid;
[0063] Finally, the mixed acid solution was heated to 100°C and placed into a titanium substrate for etching for 60 min. After etching, the titanium substrate was taken out with tweezers and washed several times with deionized water, placed on filter paper, dried at room temperature, and sealed for storage.
[0064] (2) Electrodeposition of β-PbO2 layer
[0065] First, prepare 100 mL of β-PbO2 electroplating solution containing 0.5 mol / L Pb(NO3)2, 0.04 mol / L NaF, and 0.1 mol / L HNO3;
[0066] Then, the β-PbO2 active layer was prepared by step-by-step electrodeposition. The titanium substrate (1 cm × 1 cm) was used as the anode and the platinum electrode of the same size was used as the cathode. The β-PbO2 active layer was prepared by step-by-step electrodeposition. The titanium substrate (1 cm × 1 cm) was used as the anode and the platinum electrode of the same size was used as the cathode. 2 Electrodeposition was performed at a current density of 15, 20, 25, 30, 35, 40, 45, and 50 mA / cm 2 Current density electrodeposition for 5 min;
[0067] Finally, the electrode was taken out and washed with deionized water to obtain a Ti / β-PbO2 electrode.
[0068] Comparative Example 2
[0069] The difference from Example 1 is that the heat treatment step after silver plating is omitted to prepare a Ti / Ag / α-PbO2 / β-PbO2 electrode.
[0070] Comparative Example 3
[0071] The difference from Example 1 is that the step of electrodepositing the α-PbO2 layer is omitted to prepare a Ti / Ag / β-PbO2 electrode.
[0072] Comparative Example 4
[0073] The difference from Example 1 is that the α-PbO2 layer is replaced by a tin antimony oxide intermediate layer to prepare a Ti / Ag / Zr-SnO2 / β-PbO2 electrode.
[0074] Comparative Example 5
[0075] The difference from Example 1 is that the electrodeposition of the β-PbO2 layer does not adopt step-by-step electrodeposition, and the electrodeposition temperature is 20 mA / cm 2 The Ti / Ag / α-PbO2 / β-PbO2 electrode was prepared by electroplating at a current density of 50 min.
[0076] Performance testing and result analysis:
[0077] The titanium-based coating electrodes prepared in the above examples and comparative examples were subjected to performance testing and analysis, including the following steps:
[0078] (1) Charge transfer resistance is an important parameter for evaluating the electrochemical performance of electrodes. In order to further study the electrochemical performance of electrodes, the electrochemical impedance spectroscopy (EIS) curves of Ti / β-PbO2 electrode (Comparative Example 1) and Ti / Ag / α-PbO2 / β-PbO2 electrode (Example 1) were measured in 0.1 mol / L Na2SO4 solution at an amplitude of 0.01 V and a frequency of 0.1-1 MHz. In the EIS curve, the diameter of the semicircular arc of the high-frequency part of the resistance is used to measure the charge transfer resistance between the substrate and the coated electrode, that is, the electrode resistance. The smaller the diameter, the smaller the electrode resistance; the larger the diameter, the greater the electrode resistance. Figure 1 As shown in Figure 2, through equivalent circuit fitting, it is found that the impedance of Ti / β-PbO2 and Ti / Ag / α-PbO2 / β-PbO2 electrodes are 11.20Ω·cm -2 、5.34Ω·cm -2 , indicating that the Ti / Ag / α-PbO2 / β-PbO2 electrode of the present invention has better conductivity.
[0079] (2) Accelerated life test can evaluate the stability of metal oxide electrodes. Generally speaking, the stability of the electrode is an important performance in practical applications, and is usually used to explore how fast the PbO2 active layer falls off from the titanium substrate. 2 The Ti / β-PbO2 electrode of Comparative Example 1 and the Ti / Ag / α-PbO2 / β-PbO2 electrode of Example 1 were subjected to an accelerated life test in a 15wt.% H2SO4 aqueous solution using a DC power supply. The voltage change was recorded to evaluate the stability and life of the electrode. The test was terminated when the battery voltage exceeded 10V. The results are as follows Figure 2 As shown in the figure, the voltage of the Ti / β-PbO2 electrode exceeded 10 V at 5 min, reaching 12.78 V, while the voltage of the Ti / Ag / α-PbO2 / β-PbO2 electrode exceeded 10 V at 62.183 h, reaching 15.98 V. This shows that the Ag layer can significantly improve the stability and service life of the electrode.
[0080] (3) SEM and EDS can be used to analyze the microstructure. Scan the prepared electrode. Figure 3 As shown in the figure, Ag was plated three times and heat treated in air at 400℃ for 1h. The Ag layer basically covered the Ti substrate, providing protection for the Ti electrode and ensuring good conductivity. Figure 4 As shown in FIG. 1 , EDS analysis of the Ti / Ag electrode revealed that it was mainly composed of Ti (40.16 wt.%), Ag (53.34 wt.%), and O (6.50 wt.%) elements, indicating that the Ag layer was heat treated in an air atmosphere, Ag was not oxidized, and Ti was basically covered. Figure 5 As shown in Figure 2, the surface of Ti / Ag / α-PbO2 prepared by electrodeposition shows a dense structure, which can effectively prevent the penetration of active oxygen and improve the stability of the electrode. Figure 6 As shown in Figure 1, EDS analysis of the Ti / Ag / α-PbO2 electrode revealed that it was mainly composed of Pb (80.75 wt.%), O (19.12 wt.%), Ti (0.10 wt.%) and a small amount of Ag (0.03 wt.%), indicating that Ag was basically covered. The EDS spectrum of the Ti / Ag / α-PbO2 electrode after the α-PbO2 layer was scraped off is shown in Figure 1. Figure 7 As shown, it was found that it was mainly composed of Pb (4.26wt.%), O (22.30wt.%), Ti (72.72wt.%) and Ag (0.72wt.%) elements. Relatively speaking, the Ag content is relatively low. It may be that when the α-PbO2 layer is scraped off, the Ag layer attached to the Ti substrate is also scraped off; secondly, part of the Ag layer may also be dissolved under alkaline conditions during the electrodeposition process, and then deposited in the α-PbO2 layer in a co-deposition manner. In summary, EDS analysis shows that the Ag / α-PbO2 intermediate layer was successfully prepared. Figure 8 As shown in the figure, the β-PbO2 active layer is a dense tetrahedral pyramid structure and new β-PbO2 is derived outward from some of the vertices of the tetrahedral pyramids. This structure can effectively prevent active oxygen from penetrating the electrode surface and increase the surface area of the electrode, protecting the outer layer of the electrode from falling off, and providing abundant active sites for efficient electrocatalytic degradation of anthraquinone organic pollutants.
[0081] (4) XRD analysis of crystal structure. Fig. 9As shown in the figure, the crystal structure of the interface of Ti / Ag / α-PbO2 and Ti / Ag / α-PbO2 / β-PbO2 electrodes was tested and analyzed by XRD. The spectrum drawn by Ti / Ag / α-PbO2 electrode was compared with the standard card of α-PbO2. The Ti / Ag / α-PbO2 electrode showed characteristic diffraction peaks at 36.16°, 60.52°, and 76.97°, which corresponded to the (200), (132), and (400) crystal planes of the standard α-PbO2 (PDF#41-1416) material, respectively. Therefore, α-PbO2 was electrodeposited on the Ti / Ag surface, which further demonstrated that the Ti / Ag / α-PbO2 electrode was successfully prepared. The characteristic diffraction peaks of Ti / Ag / α-PbO2 / β-PbO2 electrode at 31.80°, 36.12°, 62.31°, and 76.79° correspond to the (101), (200), (301), and (211) crystal planes of standard β-PbO2 (PDF#41-1492) material, respectively. Therefore, β-PbO2 was electrodeposited on the surface of Ti / Ag / α-PbO2, further indicating that the Ti / Ag / α-PbO2 / β-PbO2 electrode was successfully prepared.
[0082] (5) With Alizarin Red S (ARS) solution as the target pollutant, the Ti / Ag / α-PbO2 / β-PbO2 electrode of Example 1 and the electrodes of Comparative Examples 1, 2, 3, 4, and 5 were used as anodes, and platinum electrodes of the same size were used as cathodes at 40 mA / cm 2 When the ARS solution with an initial concentration of 30.00 mg / L is degraded at a current density of Fig.10 As shown, the degradation rate of Example 1 is 96.49%, the degradation rate of Comparative Example 1 is 94.59%, the degradation rate of Comparative Example 2 is 71.88%, the degradation rate of Comparative Example 3 is 94.34%, the degradation rate of Comparative Example 4 is 54.62%, and the degradation rate of Comparative Example 5 is 81.44%. It shows that the Ti / Ag / α-PbO2 / β-PbO2 electrode has better electrocatalytic activity, indicating that the Ti / Ag / α-PbO2 / β-PbO2 electrode has great application potential in the degradation of anthraquinone organic dyes (especially Alizarin Red S) and other electrochemical technology fields.
[0083] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A Ti / Ag / α-PbO 2 / β-PbO 2 Method for preparing the electrode, It is characterized in that The steps include: S1: preparing a mixed acid solution and heating it, then placing the ultrasonically treated titanium substrate into the solution for etching to obtain a pretreated titanium substrate; S2: prepare a silver plating solution, place the pretreated titanium substrate in the silver plating solution for silver plating, take out the titanium substrate after the silver plating is completed, clean it with ultrapure water, and dry it naturally or in an oven; replace the silver plating solution, repeat the silver plating several times; and then perform high-temperature heat treatment to obtain a Ti / Ag electrode; S3: Preparation of α-PbO 2 Plating solution and Ti / Ag electrode on α-PbO 2 Electrodeposition was performed in the plating solution and washed with deionized water to obtain Ti / Ag / α-PbO 2 electrode; S4: Preparation of β-PbO 2 The plating solution is Ti / Ag / α-PbO 2 Electrode in β-PbO 2 Electrodeposition was performed in the plating solution and washed with deionized water to obtain Ti / Ag / α-PbO 2 / β-PbO 2 electrode.
2. The Ti / Ag / α-PbO according to claim 1 2 / β-PbO 2 Method for preparing the electrode, It is characterized in that In step S1, the thickness of the titanium substrate is any one of 0.1 mm, 0.2 mm, and 0.3 mm; and the mixed acid solution includes sulfuric acid and tartaric acid.
3. The Ti / Ag / α-PbO according to claim 1 2 / β-PbO 2 Method for preparing the electrode, It is characterized in that In step S2, the silver plating solution includes silver salt, dilute ammonia water, strong base and reducing aldehyde.
4. The Ti / Ag / α-PbO according to claim 3 2 / β-PbO 2 Method for preparing the electrode, It is characterized in that The silver salt is silver nitrate with a concentration of 2.0-6.0 wt.%; the strong base is any one of sodium hydroxide and potassium hydroxide with a concentration of 1.0-4.0 wt.%; the reducing aldehyde is any one of glucose, formaldehyde and acetaldehyde with a concentration of 3.0-7.0 wt.%; the concentration of dilute ammonia water is 2.0-10.0 wt.%.
5. The Ti / Ag / α-PbO according to claim 1 2 / β-PbO 2 Method for preparing the electrode, It is characterized in that In step S2, the silver plating time is 20 min to 80 min; the number of silver plating is 1 to 5 times; the drying temperature is 30 to 50°C; and the heat treatment temperature is 350 to 500°C.
6. The Ti / Ag / α-PbO according to claim 1 2 / β-PbO 2 Method for preparing the electrode, It is characterized in that The specific process of electrodeposition in step S3 is: at 30-60°C and 2-7 mA / cm 2 Electrodeposition for 2 to 5 hours.
7. The Ti / Ag / α-PbO according to claim 1 2 / β-PbO 2 Method for preparing the electrode, It is characterized in that The specific process of electrodeposition in step S4 is as follows: first, at 40-70°C, at 10 mA / cm 2 Electrodeposition for 10 to 30 minutes; then increase the current density by 5 mA / cm 2 Electrodeposition for 5 minutes, co-electrodeposition for 30 to 60 minutes.
8. Ti / Ag / α-PbO obtained by the preparation method according to any one of claims 1 to 7 2 / β-PbO 2 electrode.
9. Ti / Ag / α-PbO obtained by the preparation method according to any one of claims 1 to 7 2 / β-PbO 2 Application of electrodes in electrochemical degradation of anthraquinone organic dye wastewater.
10. The use according to claim 9, It is characterized in that The anthraquinone organic dye is Alizarin Red S.
Citation Information
Patent Citations
Preparing method and application of silver-doped lead dioxide electrode
CN110066000A
Titanium-based lead dioxide electrode for degrading rhodamine B, and preparation method and application thereof
CN110980890A
Lead oxide-coated electrode for use in electrolysis and process for producing the same
US4822459A