Fluorine-containing wafer surface treatment liquid

By adding fluoride, silane coupling agent and organic solvent to the high aspect ratio wafer surface treatment liquid, the problem of gate collapse caused by traditional cleaning liquid is solved, and the effect of no adhesion during the drying process is achieved, ensuring that Wafer stability.

CN118726004APending Publication Date: 2024-10-01SHANGHAI SINYANG SEMICONDUCTOR MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310338374.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

After traditional cleaning fluids are used to process high aspect ratio wafers, the gate electrodes may collapse during the spin-drying process, and the cleaning fluids are difficult to completely remove, leaving contaminant residues and affecting device performance.

Method used

Use a fluoride-containing wafer surface treatment solution, which includes 0.005%-1% fluoride, 0.1%-20% silane coupling agent and organic solvent. By adjusting the component ratio and selecting the appropriate organic solvent, the IPA can be improved Contact angle to avoid adhesion.

Benefits of technology

After treatment, the IPA contact angle increased significantly, and the surface changed from hydrophilic to hydrophobic, avoiding adhesion and collapse between gate electrodes and ensuring the stability of the drying process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004157270150000051
    Figure BDA0004157270150000051
  • Figure BDA0004157270150000061
    Figure BDA0004157270150000061
  • Figure BDA0004157270150000071
    Figure BDA0004157270150000071
Patent Text Reader

Abstract

The invention discloses a fluoride-containing wafer surface treatment liquid. The wafer surface treatment liquid is prepared from the following raw materials in percentage by mass: 0.005 to 1 percent of fluoride, 0.1 to 20 percent of silane coupling agent and organic solvent, the sum of the mass fractions of all the components is 100%. The organic solvent is used for complementing the balance. After the wafer is treated by the wafer surface treatment liquid, the IPA contact angle is obviously increased, and the grids are not adhered in the drying process, so that the collapse of the grids is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a fluoride-containing wafer surface treatment liquid. Background Art

[0002] With the continuous development of the semiconductor industry, integrated circuits are gradually developing towards high integration and ultra-fine line widths. Therefore, more and more high aspect ratio structures are involved in the chip manufacturing process (in the semiconductor industry, structures with a depth / height and width ratio greater than or equal to 10 are generally defined as high aspect ratio). High aspect ratio structures not only face huge challenges during etching and deposition, but also have great problems in cleaning after etching. On the one hand, the current mainstream cleaning method is still wet cleaning based on water chemistry. For these micro-nano structures with small openings but large depths, it is difficult for liquids to enter the bottom of the grooves to achieve the purpose of cleaning; on the other hand, once the cleaning liquid enters the deep grooves, it is difficult to remove the liquid under the action of surface tension, resulting in residual contaminants, which become a potential threat to subsequent processes, and even cause device failure in severe cases. At the same time, the capillary force existing during the drying process of these high aspect ratio structures may also cause the collapse of these structures, resulting in device failure.

[0003] In the traditional IPA (isopropyl alcohol) spin-drying process, when the gate AR (aspect ratio) is greater than or equal to 10, a large force will be generated between the IPA and the gate (from the surface tension of IPA), and the gate will adhere to the gate during the spin-drying process, causing the gate to collapse during the drying process. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a fluoride-containing wafer surface treatment liquid in order to overcome the problem that the gate collapses during the spin-drying process after the wafer is treated with a conventional cleaning liquid. After the wafer is treated with the surface treatment liquid of the present invention, the IPA contact angle is significantly increased, and the gates will not adhere to each other during the drying process, thereby avoiding the occurrence of gate collapse.

[0005] The present invention mainly solves the above technical problems through the following technical solutions.

[0006] The present invention provides a wafer surface treatment liquid, the raw materials of which include the following components in mass fraction: 0.005%-1% fluoride, 0.1%-20% silane coupling agent and organic solvent; the sum of the mass fractions of the components is 100%; the organic solvent makes up the balance;

[0007] The silane coupling agent is Among them, R 1 , R 2 and R 3 are independently H, alkyl, alkoxy, -OH, -NH2, -COOH or -NHC(O)NHR 4; said R 1 , R 2 and R 3 At least one is an alkoxy group;

[0008] The R 4 is hydrogen or C1-C6 alkyl;

[0009] The organic solvent is selected from one or more of isopropyl alcohol (IPA), propylene glycol methyl ether acetate (PGMEA), N,N-dimethylformamide (DMF), n-hexane, cyclohexanone, tetrahydrofuran, dichloromethane, acetone and xylene.

[0010] In some embodiments, the R 4 is hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl or tert-butyl. Preferably, the R 4 It is hydrogen or methyl.

[0011] In some embodiments, the fluoride-containing compound is selected from one or more of hydrogen fluoride, ammonium fluoride, ammonium bifluoride, tetramethylammonium fluoride, fluorosulfonic acid, trihydroxyethylammonium fluoride, perfluorooctylethylene, perfluorodecene, perfluorohexylethylene, perfluorooctene, perfluorobutylethylene and 1H,1H,2H-perfluoro-1-hexene; preferably, the fluoride-containing compound is selected from one or both of hydrogen fluoride and fluorosulfonic acid.

[0012] In some embodiments, the mass fraction of the fluoride is 0.01%-0.08%, preferably, the mass fraction of the fluoride is 0.01%-0.05%.

[0013] In some embodiments, the R 1 , R 2 and R 3 are independently C1-C6 alkoxy, -NH2 or -COOH, said R 1 , R 2 and R 3 At least one is an alkoxy group; preferably, the C1-C6 alkoxy group is independently methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy or tert-butoxy, such as methoxy.

[0014] In some embodiments, the mass fraction of the silane coupling agent is 5%-20%, preferably, the mass fraction of the silane coupling agent is 5%-15%, and more preferably, the mass fraction of the silane coupling agent is 5% or 10%.

[0015] In some embodiments, the silane coupling agent is

[0016] In some embodiments, the organic solvent is selected from one or more of isopropyl alcohol, N,N-dimethylformamide and propylene glycol methyl ether acetate.

[0017] In some embodiments, when the organic solvent is a mixed solution of isopropyl alcohol and propylene glycol methyl ether acetate, the mass ratio of the isopropyl alcohol to the propylene glycol methyl ether acetate is 1:(1-2).

[0018] In some embodiments, the pH value of the wafer surface treatment solution is 7-12.

[0019] In some embodiments, the wafer is a high aspect ratio wafer.

[0020] In some embodiments, the ratio of the depth to width of the wafer is greater than or equal to 10, preferably 10-100, more preferably 10-50, and further preferably 10-15.

[0021] In some schemes, the raw materials of the wafer surface treatment liquid include the following components by mass fraction: 0.01%-0.05% fluoride, 5%-10% silane coupling agent and organic solvent; the sum of the mass fractions of each component is 100%; the organic solvent makes up the balance;

[0022] The fluoride-containing compound is selected from one or both of hydrogen fluoride and fluorosulfonic acid;

[0023] The silane coupling agent is

[0024] The organic solvent is selected from one or more of isopropyl alcohol, N,N-dimethylformamide and propylene glycol methyl ether acetate.

[0025] In some embodiments, the wafer surface treatment solution comprises raw materials comprising any of the following components in mass fractions:

[0026] Solution 1: 0.01% hydrogen fluoride, 5% and isopropyl alcohol, the isopropyl alcohol making up the balance;

[0027] Solution 2: 0.01% hydrogen fluoride, 5% and isopropyl alcohol, the isopropyl alcohol making up the balance;

[0028] Solution 3: 0.05% hydrogen fluoride, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance;

[0029] Solution 4: 0.05% hydrogen fluoride, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance;

[0030] Solution 5: 0.01% hydrogen fluoride, 5% and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance;

[0031] Solution 6: 0.01% hydrogen fluoride, 5% and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance;

[0032] Solution 7: 0.05% hydrogen fluoride, 10% and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance;

[0033] Solution 8: 0.05% hydrogen fluoride, 10% and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance;

[0034] Solution 9: 0.01% fluorosulfonic acid, 5% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance;

[0035] Solution 10: 0.01% fluorosulfonic acid, 5% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance;

[0036] Solution 11: 0.05% fluorosulfonic acid, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance;

[0037] Solution 12: 0.05% fluorosulfonic acid, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance;

[0038] Preferably, the raw materials of the wafer surface treatment liquid are composed of any of the above schemes.

[0039] In some embodiments, the wafer surface treatment solution is used to clean wafers with a high aspect ratio.

[0040] The term "high aspect ratio" of the present invention; in the semiconductor industry, a structure having a ratio of depth to width greater than or equal to 10 is generally defined as having a high aspect ratio.

[0041] The "room temperature" of the present invention refers to 20°C to 30°C.

[0042] Without violating the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0043] The reagents and raw materials used in the present invention are commercially available.

[0044] The positive improvement effect of the present invention is that after the wafer is treated with the fluoride-containing wafer surface treatment liquid of the present invention, the IPA contact angle is significantly increased, the surface changes from hydrophilic to hydrophobic, and no adhesion occurs between the gates during the drying process, thereby avoiding the occurrence of gate collapse. DETAILED DESCRIPTION

[0045] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0046] Example 1

[0047] The surface treatment liquid was prepared according to the ingredients and proportions of each example in Table 1, and mixed evenly, specifically stirred at room temperature for 1 hour (without any order of addition).

[0048] Table 1

[0049]

[0050]

[0051] Note: “ / ” means does not exist.

[0052] This test uses TEOS (tetraethoxysilane) and SiN (silicon nitride) for testing. The test method is:

[0053] 1. Cut the wafer with aspect ratio of 10 into 30*30mm test pieces;

[0054] 2. Soak the test piece in IPA cleaning solution for 1 minute; take it out;

[0055] 3. Immerse the test pieces in the surface treatment solutions described in Table 1 for 1 minute, take them out and blow dry them with nitrogen;

[0056] 4. The contact angle test was performed using a contact angle tester (Attension Theta Lite), and the test solution was IPA. The surface roughness was tested at the same time, and the surface of the test piece was observed by electron microscopy. The results are shown in Table 2 below.

[0057] Table 2

[0058]

[0059]

[0060] It can be seen from the test results that after being immersed in the surface treatment liquid of the present application, the IPA contact angle is significantly increased, and no adhesion will occur between the gates during the drying process, thereby avoiding the occurrence of gate collapse.

Claims

1. A wafer surface treatment liquid, characterized in that: The raw materials include the following components in mass fraction: 0.005%-1% fluoride, 0.1%-20% silane coupling agent and organic solvent; the mass fraction of each component is 100%; the organic solvent makes up the balance; The silane coupling agent is Among them, R 1 , R 2 and R 3 are independently H, alkyl, alkoxy, -OH, -NH2, -COOH or -NHC(O)NHR 4 ; said R 1 , R 2 and R 3 At least one is an alkoxy group; The R 4 is hydrogen or C1-C6 alkyl; The organic solvent is selected from one or more of isopropanol, propylene glycol methyl ether acetate, N,N-dimethylformamide, n-hexane, cyclohexanone, tetrahydrofuran, dichloromethane, acetone and xylene.

2. The wafer surface treatment solution according to claim 1, characterized in that: The wafer surface treatment solution meets one or more of the following conditions: (1) The fluoride-containing compound is selected from one or more of hydrogen fluoride, ammonium fluoride, ammonium bifluoride, tetramethylammonium fluoride, fluorosulfonic acid, trihydroxyethylammonium fluoride, perfluorooctylethylene, perfluorodecene, perfluorohexylethylene, perfluorooctene, perfluorobutylethylene and 1H,1H,2H-perfluoro-1-hexene; (2) The mass fraction of the fluoride is 0.01%-0.08%; and (3) R 4 is hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl or tert-butyl.

3. The wafer surface treatment solution according to claim 2, characterized in that: The wafer surface treatment solution meets one or more of the following conditions: (1) The fluoride-containing compound is selected from one or both of hydrogen fluoride and fluorosulfonic acid; (2) The mass fraction of the fluoride is 0.01%-0.05%; and (3) R 4 It is hydrogen or methyl.

4. The wafer surface treatment solution according to claim 3, characterized in that: The wafer surface treatment solution meets one or more of the following conditions: (1) R 1 , R 2 and R 3 are independently C1-C6 alkoxy, -NH2 or -COOH, said R 1 , R 2 and R 3 At least one is an alkoxy group; (2) The mass fraction of the silane coupling agent is 5%-20%; (3) the organic solvent is selected from one or more of isopropyl alcohol, N,N-dimethylformamide and propylene glycol methyl ether acetate; and (4) The pH value of the wafer surface treatment solution is 7-12.

5. The wafer surface treatment liquid according to claim 4, characterized in that: The wafer surface treatment solution meets one or more of the following conditions: (1) R 1 , R 2 and R 3 In the above, C1-C6 alkoxy is independently methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy or tert-butoxy, for example methoxy; (2) The mass fraction of the silane coupling agent is 5%-15%; and (3) When the organic solvent is a mixed solution of isopropyl alcohol and propylene glycol methyl ether acetate, the mass ratio of the isopropyl alcohol to the propylene glycol methyl ether acetate is 1:(1-2).

6. The wafer surface treatment solution according to claim 5, characterized in that: The wafer surface treatment solution meets one or both of the following conditions: (1) The mass fraction of the silane coupling agent is 5% or 10%; and (2) The silane coupling agent is 7. The wafer surface treatment solution according to claim 1, characterized in that: The raw materials include the following components in mass fraction: 0.01%-0.05% fluoride, 5%-10% silane coupling agent and organic solvent; the sum of the mass fractions of each component is 100%; the organic solvent makes up the balance; The fluoride-containing compound is selected from one or both of hydrogen fluoride and fluorosulfonic acid; The silane coupling agent is The organic solvent is selected from one or more of isopropyl alcohol, N,N-dimethylformamide and propylene glycol methyl ether acetate.

8. The wafer surface treatment solution according to any one of claims 1 to 7, characterized in that: The wafer surface treatment liquid, its raw materials include any of the following components in mass fractions: Solution 1: 0.01% hydrogen fluoride, 5% and isopropyl alcohol, the isopropyl alcohol making up the balance; Solution 2: 0.01% hydrogen fluoride, 5% and isopropyl alcohol, the isopropyl alcohol making up the balance; Solution 3: 0.05% hydrogen fluoride, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance; Solution 4: 0.05% hydrogen fluoride, 10% and isopropyl alcohol, the isopropyl alcohol making up the balance; Solution 5: 0.01% hydrogen fluoride, 5% and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance; Solution 6: 0.01% hydrogen fluoride, 5% and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance; Solution 7: 0.05% hydrogen fluoride, 10% and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance; Solution 8: 0.05% hydrogen fluoride, 10% and N,N-dimethylformamide, with N,N-dimethylformamide making up the balance; Solution 9: 0.01% fluorosulfonic acid, 5% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance; Solution 10: 0.01% fluorosulfonic acid, 5% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance; Solution 11: 0.05% fluorosulfonic acid, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance; Solution 12: 0.05% fluorosulfonic acid, 10% and propylene glycol methyl ether acetate, propylene glycol methyl ether acetate making up the balance.

9. The wafer surface treatment solution according to claim 8, characterized in that: The raw materials of the wafer surface treatment liquid are composed of any one of the schemes in claim 8.

10. The wafer surface treatment solution according to claim 9, characterized in that: The wafer surface treatment liquid is used for cleaning wafers with a high aspect ratio.