Efficient normalizing control method and production method of high-magnetic-induction oriented silicon steel

By improving the normalization process and controlling temperature and time during the normalization process of low-temperature and high-magnetic oriented silicon steel, the problem of insufficient solid solution of nitrides was solved, and high-efficiency production of high-magnetic oriented silicon steel was achieved, with the maximum magnetic induction reaching 1.920~ 1.925T, and improve production efficiency.

CN118726741AActive Publication Date: 2024-10-01武汉钢铁有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410757480.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

In the existing technology, during the normalization process of low-temperature high magnetic induction oriented silicon steel, the control of temperature and time is insufficient, resulting in insufficient nitride solid solution, reduced magnetic induction and low production efficiency, and cannot be widely used in the production of high magnetic induction oriented silicon steel. .

Method used

By improving the normalization process, when the dew point of the atmosphere in the furnace is fixed, the normalization temperature is above 1130°C, and the nitride solid solution time is reduced. The first normalization time is reduced to less than 70s, and the second normalization time is reduced to 30s. Below, the third stage normalizing temperature is 930~940°C, and the precipitation time of ALN is reduced to less than 75 seconds, which controls the uniformity of grains on the surface of the hot-rolled plate, shortens the normalizing time, and improves production efficiency.

Benefits of technology

The stable performance of high magnetic induction oriented silicon steel is achieved, with the maximum magnetic induction reaching 1.920~1.925T, shortening the normalization time and improving production efficiency and capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004889923520000061
    Figure BDA0004889923520000061
  • Figure BDA0004889923520000071
    Figure BDA0004889923520000071
  • Figure BDA0004889923520000081
    Figure BDA0004889923520000081
Patent Text Reader

Abstract

The invention discloses an efficient normalizing control method and a production method of high-magnetic-induction oriented silicon steel. A hot-rolled coil is subjected to normalizing annealing at different temperature stages, specifically, the normalizing temperature of the first stage is 1135-1140 DEG C, and the normalizing time is 55-70 s; the second-stage normalizing temperature is 1130-1135 DEG C, the dew point is controlled to be a positive dew point, and the normalizing time is 20-30 s; the third-stage normalizing temperature is 930-940 DEG C, the dew point is controlled to be a positive dew point, and the normalizing time is 55-75 s; and the fourth-stage cooling temperature is 860-870 DEG C, and the cooling time is 8-15 s. By means of the improved normalizing process, under the condition that the dew point of the atmosphere in the furnace is fixed, nitrides are subjected to solid solution more sufficiently at the temperature of 1130 DEG C or above, meanwhile, the solid solution time of the nitrides is shortened, the first-stage normalizing time is shortened to 70 s or below, the lowest time can reach 55 s, and the second-stage normalizing time is shortened to 30 s or below; under the condition that fine ALN is separated out more uniformly in the cooling process of about 930-940 DEG C, the time for separating out the ALN after the temperature of 930-940 DEG C is shortened to 75 seconds or below, and the lowest time can reach 55 seconds. By controlling the surface grain uniformity of the normalized hot-rolled plate, the normalizing time is greatly shortened, the normalizing production efficiency is improved, and the productivity is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of steel, and in particular relates to a normalization control method and a production method of high magnetic induction oriented silicon steel with high production efficiency. Background Art

[0002] Since the finished grains of oriented silicon steel have the characteristics of sharp Gaussian texture and preferential orientation, they are very easy to magnetize in the rolling direction and can obtain a higher saturation magnetic induction intensity. Taking advantage of this characteristic of oriented silicon steel, it is widely used in the production and manufacturing of transformer cores in industry. The higher the saturation magnetic induction intensity that oriented silicon steel can obtain, the lower its iron loss under specific magnetic induction conditions. The transformer core loss made of oriented silicon steel with excellent magnetic properties is also low, which is of great significance to reducing the energy loss of transformer equipment working engineering and improving the quality, volume and manufacturing cost of transformer equipment.

[0003] From the perspective of product magnetic properties, magnetic induction (B 800 ) Oriented silicon steel with a magnetic induction of more than 1.88T is called high magnetic induction oriented silicon steel. From the production process characteristics, oriented silicon steel is prepared by low-temperature slab heating method (referred to as "low-temperature oriented silicon steel", hot-rolled slab heating temperature is below 1200℃).

[0004] In order to achieve the purpose of heating the hot-rolled low-temperature slab, the low-temperature high-magnetic induction oriented silicon steel preparation process uses AlN with a low solid solution temperature as the main inhibitor. Through appropriate composition design, the heating temperature of the ingot can be reduced to below 1200°C. The low-temperature slab reheating technology includes the "inherent inhibitor method" and the "acquired inhibitor method". The "inherent inhibitor method" forms the inhibitor required for secondary recrystallization before cold rolling. In addition to the main AlN, Cu is also added. 2Precipitated phases such as S and MnSe and segregation elements such as Sn and Sb are used as auxiliary inhibitors to replace MnS with a higher solid solution temperature. The unstable secondary particle phase is dissolved back by short-term heating and heat preservation at a high temperature of 1100℃ to 1150℃. The more γ phases there are in the steel strip, the more nitrides have a solid solubility in the γ phase that is 10 times greater than in the α phase. The subsequent slow cooling to 900℃ achieves the precipitation of a large number of fine and uniformly dispersed inhibitors, so that there are enough fine and dispersed second phases to inhibit the normal growth of grains before secondary recrystallization occurs. The "acquisition inhibitor method" is a method for obtaining the inhibitors required for the production of high magnetic induction oriented silicon steel after decarburization annealing of the steel strip and before high-temperature annealing and secondary recrystallization. It includes coating a nitride promoter or a nitriding agent containing CrN, MnN, etc. before entering the high-temperature annealing furnace to achieve nitridation during the high-temperature annealing heating process, but it is not widely used because the obtained nitrides are not uniform and the performance of the finished product is not stable. The most widely used process measure is still to add a gas nitriding treatment section after the decarburization furnace, using a mixture of N2 and H2 to complete the nitriding treatment, forming (Al, Si) N on the surface of the steel strip to ensure the inhibitory amount of abnormal growth of secondary recrystallization.

[0005] In the preparation process of low-temperature high-magnetic induction oriented silicon steel, different primary crystallizations are related to the state of the inhibitor of the precipitated phase. The uniformity of the primary crystallization formation leads to different abilities of abnormal growth of secondary recrystallization, in order to achieve more uniform primary grains. The hot-rolled plate must go through the normalization stage to make the hot-rolled plate structure more uniform, increase the crystal grains on the upper and lower surfaces after normalization, and at the same time make the grains grow and the ALN solid solution coarsen, and strengthen the crystal phase of the organization. Generally, normalization at 1100℃ for more than 70S can gradually dissolve the inhibitor nitride. During the solid solution process, the atmosphere in the furnace is kept humid. The stronger the decarburization ability, the thicker the ferrite thickness on the surface of the steel strip, the more γ phase in the steel strip, and the solid solubility of nitride in the γ phase is 10 times greater than that in the α phase. Under the condition of a certain ferrite thickness, the normalization holding time can be shortened and the normalization production efficiency can be improved.

[0006] However, if the temperature and time are not well controlled during the normalizing process: for example, if the temperature of the steel strip does not reach the temperature of ALN solid solution, the ALN nitride solid solution is insufficient, and secondary recrystallization cannot occur afterwards; or if the steel strip temperature exceeds the temperature of ALN solid solution for too short a time, the nitride solid solution is less and the normalized grains are too small, and then other non-Gaussian orientation grains also grow to a certain extent and are difficult to be completely swallowed up, resulting in the overall texture orientation of the final product being poor and the magnetic induction being reduced. In order to control the matching relationship between the heating rate, normalizing temperature and time to obtain the best performance, various manufacturers have taken relevant measures and improvements in the normalizing process, but there are still shortcomings.

[0007] In actual production, the usual practice is to use a longer holding time (more than 70 seconds) to ensure the solid solution time of ALN during the heating process to reach the normalizing temperature of 1100°C; at the same time, coarse ALN is precipitated after 900°C (more than 70 seconds), resulting in low normalizing efficiency.

[0008] For example, Chinese patent application CN105177444A discloses a normalization control method for producing low-temperature high-magnetic induction oriented silicon steel. After conventional hot rolling, a two-stage normalization process is performed: the temperature T of the first normalized steel plate is controlled according to the Als content in the hot-rolled coil, and the temperature is kept for 20 to 30 seconds: then the temperature of the steel plate is lowered to 890 to 910°C to start the second normalization process, and the temperature is kept for 100 to 120 seconds to obtain good magnetic properties. This method has a low temperature of the steel plate before the start of the second normalization process, resulting in uneven precipitation of nitrides during the normalization process, and the maximum magnetic induction B cannot be obtained. 8 (T)>1.920 high magnetic induction oriented silicon steel, and low production efficiency, resulting in energy consumption.

[0009] There is also a Chinese patent application CN103074476A that discloses a method for producing high magnetic induction oriented silicon steel strip by three-stage normalization, which is carried out by normalization and tempering in three stages: the temperature of the first stage is controlled at 1050-1150°C, the temperature of the second stage is controlled at 1050-950°C, and the temperature of the third stage is controlled at 950-800°C to obtain high magnetic induction oriented silicon steel. Due to the lower temperature in the second stage, the normalized surface grains are not fully grown, and the maximum magnetic induction B cannot be obtained. 8 (T)>1.920 high magnetic induction oriented silicon steel. And the production efficiency is low, resulting in energy consumption. Summary of the invention

[0010] The technical problem to be solved by the present invention is to provide a normalization control method and production method for high magnetic induction oriented silicon steel in view of the deficiencies in the above-mentioned prior art. The present invention improves the normalization process, and under the condition that the dew point of the atmosphere in the furnace is fixed, the nitride solid solution is more fully achieved at normalization above 1130°C, and the nitride solid solution time is reduced: the first normalization time is reduced to below 70s and the minimum time can reach 55s, and the second normalization time is reduced to below 30s. In the cooling process of about 930-940°C, the precipitation of fine ALN is more uniform, and at the same time, the precipitation time of ALN after 930-940°C is reduced to below 75s, and the minimum time can reach 55s. By controlling the uniformity of the surface grains of the normalized hot-rolled plate, the normalization time is greatly shortened, the normalization production efficiency is improved, and the production capacity is increased.

[0011] The technical solution adopted by the present invention to solve the above-mentioned problems is:

[0012] An efficient production method for high magnetic induction oriented silicon steel, the steps of which are sequentially:

[0013] 1) After smelting and continuous casting into billets, heating is performed, and the billet heating temperature is controlled at 1160-1180°C;

[0014] 2) cooling and coiling after conventional hot rolling;

[0015] 3) Normalizing annealing of hot rolled coils at different temperature stages:

[0016] The first stage normalization temperature is 1135-1140℃, and the normalization time is 55-70s;

[0017] The second stage normalization temperature is 1130-1135℃, the dew point is controlled as positive dew point, and the normalization time is 20-30s;

[0018] The third stage normalization temperature is 930-940℃, the dew point is controlled to be positive dew point, and the normalization time is 55-75ss;

[0019] The cooling temperature of the fourth stage is 860-870°C, and the cooling time is 8-15s.

[0020] 4) cold rolling in a rolling mill to a thickness ranging from 0.2 to 0.3 mm, generally not exceeding 0.282 mm;

[0021] 5) Decarburization annealing after alkali washing: The decarburization annealing atmosphere is a moisture dew point of 40-55°, N 2 :H 2 =1:1 (volume ratio) mixed gas, decarburization temperature is 830-845°C, decarburization annealing time is 90-140s, and the carbon content at the end of decarburization annealing is controlled not to be higher than 0.0010%;

[0022] 6) Perform nitriding annealing: The nitriding annealing atmosphere is a moisture dew point of 30-40°, N 2 :H 2 =1:3 (volume ratio) mixed gas, nitriding temperature is 830-890°C, nitriding time is 20-50s, and the nitrogen content of the steel strip after nitriding is controlled to be 0.020-0.025wt% higher than the nitrogen content of the ingot;

[0023] 7) Perform high temperature annealing with changing atmosphere at different temperature stages:

[0024] a. Raise the temperature to 700-730℃ and keep it for 2-2.5h to remove the bound water in the MgO layer on the surface of the steel strip;

[0025] b. Heating: According to the determined secondary recrystallization temperature of 1080-1090°C, during the heating process before 1080-1090°C, the heating rate of the steel strip is controlled at 30-35°C / h, and pure N is used during the heating process. 2 atmosphere;

[0026] c. When the temperature reaches the secondary recrystallization temperature of 1080-1090°C, the high temperature annealing atmosphere is changed from pure nitrogen to N 2 :H 2 =1:(2.8~3) (volume ratio) mixed gas, and keep it at this temperature for 1.8~2.5h; continue heating and still in N 2 :H 2 =1:(2.8-3) (volume ratio) mixed gas atmosphere at a rate of 10-25°C / h to 1160-1250°C;

[0027] 8) After high temperature annealing, stretching and flattening annealing and insulation coating are carried out to obtain finished oriented silicon steel.

[0028] The method for producing high magnetic induction oriented silicon steel by controlling the normalizing temperature of the present invention is applicable to the steel components and their weight percentage contents: C 0.05%-0.065%, Si 3.1-3.4%, Als 0.022-0.032%, Mn0.08-0.09%, N 0.0060-0.0090%, S 0.0040-0.0070%, Sn 0.030-0.045%, Cr0.020-0.120%, and the rest is Fe and unavoidable impurities.

[0029] The high magnetic induction oriented silicon steel prepared by the above method of the present invention has a finished product thickness not exceeding 0.3 mm and a maximum magnetic induction B 8 (T) reaches between 1.920 and 1.925, with the minimum iron loss P 17 (W / kg) reaches between 0.825 and 0.97.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] The present invention uses an improved normalizing process to make the nitride solid solution more complete at normalizing above 1130°C under the condition that the dew point of the furnace atmosphere is fixed, and at the same time reduce the nitride solid solution time: the first normalizing time is reduced to below 70s and the minimum time can reach 55s, and the second normalizing time is reduced to below 30s. In the cooling process of about 930-940°C, the precipitation of fine ALN is more uniform, and at the same time, the precipitation time of ALN after 930-940°C is reduced to below 75s and the minimum time can reach 55s. By controlling the uniformity of the surface grains of the normalized hot-rolled plate, the normalizing time is greatly shortened, the normalizing production efficiency is improved, and the production capacity is increased. The high magnetic induction oriented silicon steel produced by the present invention has stable performance and can be increased to above 1.920T. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is a microstructure photograph of the high magnetic induction oriented silicon steel produced by the present invention. DETAILED DESCRIPTION

[0033] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the present invention is not limited to the following embodiments.

[0034] The steel components applicable to the present invention and their weight percentage contents are: C 0.05%-0.065%, Si 3.1-3.4%, Als 0.022-0.032%, Mn 0.08-0.09%, N 0.0060-0.0090%, S 0.0040-0.0070%, Sn0.030-0.045%, Cr 0.020-0.120%, and the rest are Fe and unavoidable impurities.

[0035] The present invention provides an efficient production method of high magnetic induction oriented silicon steel, the steps of which are:

[0036] 1) After smelting and continuous casting into billets, heating is performed, and the billet heating temperature is controlled at 1160-1180°C;

[0037] 2) cooling and coiling after conventional hot rolling;

[0038] 3) Normalizing annealing of hot rolled coils at different temperature stages:

[0039] The first stage normalization temperature is 1135-1140℃, and the normalization time is 55-70s;

[0040] The second stage normalization temperature is 1130-1135℃, the dew point is controlled as positive dew point, and the normalization time is 20-30s;

[0041] The third stage normalization temperature is 930-940℃, the dew point is controlled to be positive dew point, and the normalization time is 55-75s;

[0042] The cooling temperature of the fourth stage is 860-870°C, and the cooling time is 8-15s.

[0043] 4) cold rolling in a rolling mill to a thickness ranging from 0.2 to 0.3 mm, generally not exceeding 0.282 mm;

[0044] 5) Decarburization annealing after alkali washing: The decarburization annealing atmosphere is a moisture dew point of 40-55°, N 2 :H 2 =1:1 mixed gas, the decarburization temperature is 830-845℃, the decarburization annealing time is 90-140s, and the carbon content at the end of the decarburization annealing is controlled not to be higher than 0.0010%;

[0045] 6) Perform nitriding annealing: The nitriding annealing atmosphere is a moisture dew point of 30-40°, N 2 :H2 =1:3 mixed gas, nitriding temperature is 830-890℃, nitriding time is 20-50s, and the nitrogen content of the steel strip after nitriding is controlled to be 0.020-0.025wt% higher than the nitrogen content of the ingot;

[0046] 7) Perform high temperature annealing with changing atmosphere at different temperature stages:

[0047] a. Raise the temperature to 700℃~730℃ and keep it at this temperature for 2~2.5h to remove the bound water in the MgO layer on the surface of the steel strip;

[0048] b. Heating: According to the determined secondary recrystallization temperature of 1080-1090°C, during the heating process before 1080-1090°C, the heating rate of the steel strip is controlled at 30-35°C / h, and pure N is used during the heating process. 2 atmosphere;

[0049] c. When the temperature reaches the secondary recrystallization temperature of 1080-1090°C, the high temperature annealing atmosphere is changed from pure nitrogen to N 2 :

[0050] H 2 =1:(2.8~3) mixed gas, and keep it at this temperature for 1.8~2.5h; continue heating and still in N 2 :

[0051] H 2 =1: (2.8-3) mixed gas atmosphere conditions at a rate of 10-25°C / h to 1160-1250°C;

[0052] 8) After high temperature annealing, stretching and flattening annealing and insulation coating are carried out to obtain finished oriented silicon steel.

[0053] Example 1

[0054] The components and weight percentages of the high magnetic induction oriented silicon steel smelted in this embodiment are: C 0.056%, Si 3.25%, Als 0.030%, Mn 0.087%, N 0.0072%, S 0.006%, Sn 0.035%, Cr 0.120%, and the rest are Fe and unavoidable impurities. The production steps are as follows:

[0055] 1) After smelting and continuous casting into billets, heating is performed, and the billet heating temperature is controlled at 1160-1180°C;

[0056] 2) cooling and coiling after conventional hot rolling;

[0057] 3) Normalizing annealing of hot rolled coils at different temperature stages:

[0058] The first stage normalization temperature is 1135℃ and the normalization time is 70s;

[0059] The second stage normalization temperature is 1130℃, the dew point is controlled as positive dew point, and the normalization time is 30s;

[0060] The third stage normalization temperature is 930℃, the dew point is controlled as positive dew point, and the normalization time is 70s;

[0061] The fourth stage cooling temperature is 860°C and the cooling time is 15s;

[0062] 4) cold rolling with a rolling mill to a thickness of 0.282 mm;

[0063] 5) Decarburization annealing after alkali washing: The decarburization annealing atmosphere is a moisture dew point of 48°, N 2 :H 2 =1:1 mixed gas, decarburization temperature is 830℃, decarburization annealing time is 95~100s, and the carbon content at the end point of decarburization annealing is controlled not to be higher than 0.0010%;

[0064] 6) Perform nitriding annealing: The nitriding annealing atmosphere is a moisture dew point of 34°, N 2 :H 2 =1:3 mixed gas, nitriding temperature at 835℃, nitriding time 25-30s, control the nitrogen content of the steel plate after nitriding to increase the nitrogen content of the ingot by 0.020-0.025wt%;

[0065] 7) Perform high temperature annealing with changing atmosphere at different temperature stages:

[0066] a. Raise the temperature to 730°C and keep it for 2 hours to remove the bound water in the MgO layer on the surface of the strip;

[0067] b. Heating: According to the determined secondary recrystallization temperature of 1080°C, during the heating process before 1080°C, the heating rate of the steel strip is controlled at 30°C / h, and pure N is used during the heating process. 2 atmosphere;

[0068] c. When the temperature reaches the secondary recrystallization temperature of 1080°C, the high temperature annealing atmosphere is changed from pure nitrogen to N 2 :H 2 =1:

[0069] (2.8~3) mixed gas, and keep it at this temperature for 2.0h; continue heating and still in N 2 :H 2 =1:

[0070] (2.8-3) in a mixed gas atmosphere at a rate of 16°C / h to 1195-1200°C;

[0071] 8) After the high temperature annealing is completed, stretching and flattening annealing and insulating layer coating are performed to obtain the finished oriented silicon steel with a thickness of about 0.3 mm.

[0072] Comparative Example 1: The four-stage normalization temperature is fixed, but the holding time (i.e., the normalization time of the first to third stages and the cooling time of the fourth stage) is different from that of Example 1, and the other steps are the same. 8 and minimum iron loss P 17 As shown in Table 1.

[0073] Table 1

[0074]

[0075] Example 2

[0076] The components and weight percentages of the high magnetic induction oriented silicon steel smelted in this embodiment are: C 0.056%, Si 3.25%, Als 0.030%, Mn 0.087%, N 0.0072%, S 0.006%, Sn 0.035%, Cr 0.120%, and the rest are Fe and unavoidable impurities. The production steps are as follows:

[0077] 1) After smelting and continuous casting into billets, heating is performed, and the billet heating temperature is controlled at 1160-1180°C;

[0078] 2) cooling and coiling after conventional hot rolling;

[0079] 3) Normalizing annealing of hot rolled coils at different temperature stages:

[0080] The first stage normalization temperature is 1135℃ and the normalization time is 65s;

[0081] The second stage normalization temperature is 1130℃, the dew point is controlled as positive dew point, and the normalization time is 28s;

[0082] The third stage normalization temperature is 930℃, the dew point is controlled as positive dew point, and the normalization time is 65s;

[0083] The cooling temperature of the fourth stage is 860°C and the cooling time is 13s;

[0084] 4) cold rolling with a rolling mill to a thickness of about 0.215 mm;

[0085] 5) Decarburization annealing after alkali washing: The decarburization annealing atmosphere is a moisture dew point of 48°, N 2 :H 2 =1:1 mixed gas, decarburization temperature is 830℃, decarburization annealing time is 95~100s, and the carbon content at the end point of decarburization annealing is controlled not to be higher than 0.0010%;

[0086] 6) Perform nitriding annealing: The nitriding annealing atmosphere is a moisture dew point of 34°, N 2 :H 2 =1:3 mixed gas, nitriding temperature at 835℃, nitriding time 25-30s, control the nitrogen content of the steel plate after nitriding to increase the nitrogen content of the ingot by 0.020-0.025wt%;

[0087] 7) Perform high temperature annealing with changing atmosphere at different temperature stages:

[0088] a. Raise the temperature to 730°C and keep it for 2 hours to remove the bound water in the MgO layer on the surface of the strip;

[0089] b. Heating: According to the determined secondary recrystallization temperature of 1080°C, during the heating process before 1080°C, the heating rate of the steel strip is controlled at 30°C / h, and pure N is used during the heating process. 2 atmosphere;

[0090] c. When the temperature reaches the secondary recrystallization temperature of 1080°C, the high temperature annealing atmosphere is changed from pure nitrogen to N 2 :H 2 =1:

[0091] (2.8~3) mixed gas, and keep it at this temperature for 2.0h; continue heating and still in N 2 :H 2 =1:

[0092] (2.8-3) in a mixed gas atmosphere at a rate of 16°C / h to 1195-1200°C;

[0093] 8) After the high temperature annealing is completed, stretching and flattening annealing and insulating layer coating are performed to obtain the finished oriented silicon steel with a thickness of 0.23 mm.

[0094] Comparative Example 2: The four-stage normalization temperature is fixed, but the holding time is different from that of Example 2, and the other steps are the same. 8 and minimum iron loss P 17 As shown in Table 2.

[0095] Table 2

[0096]

[0097] Example 3

[0098] The components and weight percentages of the high magnetic induction oriented silicon steel smelted in this embodiment are: C 0.056%, Si 3.25%, Als 0.030%, Mn 0.087%, N 0.0072%, S 0.006%, Sn 0.035%, Cr 0.120%, and the rest are Fe and unavoidable impurities. The production steps are as follows:

[0099] 1) After smelting and continuous casting into billets, heating is performed, and the billet heating temperature is controlled at 1160-1180°C;

[0100] 2) cooling and coiling after conventional hot rolling;

[0101] 3) Normalizing annealing of hot rolled coils at different temperature stages:

[0102] The first stage normalization temperature is 1135℃ and the normalization time is 60s;

[0103] The second stage normalization temperature is 1130℃, the dew point is controlled as positive dew point, and the normalization time is 25s;

[0104] The third stage normalization temperature is 930℃, the dew point is controlled as positive dew point, and the normalization time is 60s;

[0105] The fourth stage cooling temperature is 860°C and the cooling time is 10s;

[0106] 4) cold rolling with a rolling mill to a thickness of about 0.215 mm;

[0107] 5) Decarburization annealing after alkali washing: The decarburization annealing atmosphere is a moisture dew point of 48°, N 2 :H 2 =1:1 mixed gas, decarburization temperature is 830℃, decarburization annealing time is 95~100s, and the carbon content at the end point of decarburization annealing is controlled not to be higher than 0.0010%;

[0108] 6) Perform nitriding annealing: The nitriding annealing atmosphere is a moisture dew point of 34°, N 2 :H 2 =1:3 mixed gas, nitriding temperature at 835℃, nitriding time 25-30s, control the nitrogen content of the steel plate after nitriding to increase the nitrogen content of the ingot by 0.020-0.025wt%;

[0109] 7) Perform high temperature annealing with changing atmosphere at different temperature stages:

[0110] a. Raise the temperature to 730°C and keep it for 2 hours to remove the bound water in the MgO layer on the surface of the strip;

[0111] b. Heating: According to the determined secondary recrystallization temperature of 1080°C, during the heating process before 1080°C, the heating rate of the steel strip is controlled at 30°C / h, and pure N is used during the heating process. 2 atmosphere;

[0112] c. When the temperature reaches the secondary recrystallization temperature of 1080°C, the high temperature annealing atmosphere is changed from pure nitrogen to N 2 :H 2 =1:

[0113] (2.8~3) mixed gas, and keep it at this temperature for 2.0h; continue heating and still in N 2 :H 2 =1:

[0114] (2.8-3) in a mixed gas atmosphere at a rate of 16°C / h to 1195-1200°C;

[0115] 8) After the high temperature annealing is completed, stretching and flattening annealing and insulating layer coating are performed to obtain the finished oriented silicon steel with a thickness of about 0.23 mm.

[0116] Comparative Example 3: The four-stage normalization temperature is fixed, but the holding time is different from that of Example 3, and the other steps are the same. 8 and minimum iron loss P 17 As shown in Table 3.

[0117] Table 3

[0118]

[0119] Example 4

[0120] The components and weight percentages of the high magnetic induction oriented silicon steel smelted in this embodiment are: C 0.056%, Si 3.25%, Als 0.030%, Mn 0.087%, N 0.0072%, S 0.006%, Sn 0.035%, Cr 0.120%, and the rest are Fe and unavoidable impurities. The production steps are as follows:

[0121] 1) After smelting and continuous casting into billets, heating is performed, and the billet heating temperature is controlled at 1160-1180°C;

[0122] 2) cooling and coiling after conventional hot rolling;

[0123] 3) Normalizing annealing of hot rolled coils at different temperature stages:

[0124] The first normalization temperature is 1135℃, 55s;

[0125] The second stage normalization temperature is 1135℃, the dew point is controlled as positive dew point, and the normalization time is 20s;

[0126] The third stage normalization temperature is 940℃, the dew point is controlled as positive dew point, and the normalization time is 55s;

[0127] The fourth stage cooling temperature is 870°C and the cooling time is 8s;

[0128] 4) cold rolling with a rolling mill to a thickness of 0.215 mm;

[0129] 5) Decarburization annealing after alkali washing: The decarburization annealing atmosphere is a moisture dew point of 48°, N 2 :H 2 =1:1 mixed gas, decarburization temperature is 830℃, decarburization annealing time is 95~100s, and the carbon content at the end point of decarburization annealing is controlled not to be higher than 0.0010%;

[0130] 6) Perform nitriding annealing: The nitriding annealing atmosphere is a moisture dew point of 34°, N 2 :H 2 =1:3 mixed gas, nitriding temperature at 835℃, nitriding time 25-30s, control the nitrogen content of the steel plate after nitriding to increase the nitrogen content of the ingot by 0.020-0.025wt%;

[0131] 7) Perform high temperature annealing with changing atmosphere at different temperature stages:

[0132] a. Raise the temperature to 730°C and keep it for 2 hours to remove the bound water in the MgO layer on the surface of the strip;

[0133] b. Heating: According to the determined secondary recrystallization temperature of 1080°C, during the heating process before 1080°C, the heating rate of the steel strip is controlled at 30°C / h, and pure N is used during the heating process. 2 atmosphere;

[0134] c. When the temperature reaches the secondary recrystallization temperature of 1080°C, the high temperature annealing atmosphere is changed from pure nitrogen to N 2 :H 2 =1: (2.8-3) mixed gas, and keep it at this temperature for 2.0h; continue heating and still in N 2 :H 2 =1: (2.8-3) mixed gas atmosphere conditions at a rate of 16°C / h to 1195-1200°C;

[0135] 8) After the high temperature annealing is completed, stretching and flattening annealing and insulating layer coating are performed to obtain the finished oriented silicon steel with a thickness of 0.23 mm.

[0136] Comparative Example 3: The four-stage normalization temperature is fixed, but the holding time is different from that of Example 4, and the other steps are the same. 8 and minimum iron loss P 17 As shown in Table 4.

[0137] Table 4

[0138]

[0139] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and changes without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A method for controlling normalization of high magnetic induction oriented silicon steel, characterized in that: Normalizing annealing is performed on the hot rolled coil at different temperature stages: The first stage normalizing temperature is 1135-1140℃, and the normalizing time is 55-70s; The second stage normalization temperature is 1130-1135℃, the dew point is controlled to be positive dew point, and the normalization time is 20-30s; The third stage normalization temperature is 930-940℃, the dew point is controlled to be positive dew point, and the normalization time is 55-75s; The cooling temperature of the fourth stage is 860-870°C, and the cooling time is 8-15s.

2. A method for producing high magnetic induction oriented silicon steel, comprising the steps of smelting, continuous casting into billets, slab heating, hot rolling and coiling, normalizing annealing, cold rolling, and annealing, characterized in that: Normalizing annealing is performed on the hot rolled coil at different temperature stages: The first stage normalizing temperature is 1135-1140℃, and the normalizing time is 55-70s; The second stage normalization temperature is 1130-1135℃, the dew point is controlled to be positive dew point, and the normalization time is 20-30s; The third stage normalization temperature is 930-940℃, the dew point is controlled to be positive dew point, and the normalization time is 55-75s; The cooling temperature of the fourth stage is 860-870°C, and the cooling time is 8-15s.

3. The method for producing high magnetic induction oriented silicon steel according to claim 2, wherein: Annealing includes decarburization annealing, nitriding annealing and high-temperature annealing in sequence; wherein, alkali washing is performed before decarburization annealing, the decarburization annealing atmosphere is a mixture of N2:H2=1:1 with a moisture dew point of 40-55°C, a decarburization temperature of 830-845°C, a decarburization annealing time of 90-140s, and the carbon content at the end point of decarburization annealing is controlled to be no higher than 0.0010%.

4. The method for producing high magnetic induction oriented silicon steel according to claim 3, wherein: The nitriding annealing atmosphere is a mixture of N2:H2=1:3 with a moisture dew point of 30-40°C, a nitriding temperature of 830-890°C, a nitriding time of 20-50s, and a nitrogen content in the steel strip after nitriding, the increase value △N compared to the nitrogen content of the ingot is controlled to be 0.020-0.025wt%.

5. The method for producing high magnetic induction oriented silicon steel according to claim 3, wherein: High temperature annealing uses high temperature annealing with atmosphere changed at different temperature stages. The specific process is as follows: a. Raise the temperature to 700-730℃ and keep it for 2-2.5 hours to remove the bound water in the MgO layer on the surface of the strip; b. Heating: According to the determined secondary recrystallization temperature of 1080-1090°C, during the heating process before 1080-1090°C, the heating rate of the steel strip is controlled at 30-35°C / h, and pure N2 atmosphere is used during the heating process; c. When the temperature reaches the secondary recrystallization temperature of 1080-1090°C, the high temperature annealing atmosphere is changed from pure nitrogen to a mixed gas of N2:H2=1:(2.8-3.2), and kept at this temperature for 1.8-2.5h; continue heating and still in N2: Under the mixed gas atmosphere of H2=1:(2.8-3.2), the temperature is raised to 1160-1250°C at a rate of 10-25°C / h.

6. The efficient production method of high magnetic induction oriented silicon steel according to claim 2, characterized in that: The steps include: 1) After smelting and continuous casting into billets, heating is carried out, and the billet heating temperature is controlled at 1160-1180°C; 2) After conventional hot rolling, cooling and coiling; 3) Normalizing annealing of hot rolled coils at different temperature stages: The first stage normalizing temperature is 1135-1140℃, and the normalizing time is 55-70s; The second stage normalization temperature is 1130-1135℃, the dew point is controlled to be positive dew point, and the normalization time is 20-30s; The third stage normalization temperature is 930-940℃, the dew point is controlled to be positive dew point, and the normalization time is 55-75s; The cooling temperature of the fourth stage is 860-870°C, and the cooling time is 8-15s. 4) cold rolling in a rolling mill to a thickness not exceeding 0.3 mm; 5) Decarburization annealing after alkali washing: the decarburization annealing atmosphere is a mixture of N2:H2=1:1 with a moisture dew point of 40-55°C, a decarburization temperature of 830-845°C, a decarburization annealing time of 90-140s, and the carbon content at the end of the decarburization annealing is controlled to be no higher than 0.0010%; 6) Performing nitriding annealing: The nitriding annealing atmosphere is a mixture of N2:H2=1:3 with a moisture dew point of 30-40°C, a nitriding temperature of 830-890°C, a nitriding time of 20-50s, and controlling the nitrogen content of the steel strip after nitriding to increase the nitrogen content of the ingot by ΔN by 0.020-0.025wt%; 7) Perform high temperature annealing with changing atmosphere at different temperature stages: a. Raise the temperature to 700-730℃ and keep it warm for 2-2.5h; b. Heating: According to the determined secondary recrystallization temperature of 1080-1090°C, during the heating process before 1080-1090°C, the heating rate of the steel strip is controlled at 30-35°C / h, and a pure N2 atmosphere is used during the heating process; c. When the temperature reaches the secondary recrystallization temperature of 1080-1090°C, the high temperature annealing atmosphere is changed from pure nitrogen to a mixed gas of N2:H2=1:(2.8-3), and kept at this temperature for 1.8-2.5h; the temperature is continued to be raised at a rate of 10-25°C / h to 1160-1250°C, still under the mixed gas atmosphere of N2:H2=1:(2.8-3); 8) After the high temperature annealing is completed, the post-finishing process is carried out to obtain the finished oriented silicon steel.

7. The normalization control method for high magnetic induction grain-oriented silicon steel according to claim 1 or the production method for high magnetic induction grain-oriented silicon steel according to any one of claims 2 to 6, characterized in that: The applicable steel components and their weight percentage contents are: C 0.05%-0.065%, Si 3.1-3.4%, Als 0.022-0.032%, Mn 0.08-0.09%, N 0.0060-0.0090%, S 0.0040-0.0070%, Sn 0.030-0.045%, Cr 0.020-0.120%, and the rest are Fe and unavoidable impurities.

8. High magnetic induction oriented silicon steel produced by the method according to any one of claims 2 to 6, characterized in that: The thickness of the finished product does not exceed 0.3mm, the maximum magnetic induction B8 reaches between 1.920 and 1.925T, and the minimum iron loss P 17 Reach 0.825~0.97W / kg.

Citation Information

Patent Citations

  • Method for producing high-magnetic-induction oriented silicon strips through three-stage normalizing

    CN103074476A

  • Production method for improving electromagnetic property of oriented silicon steel

    CN103834908A

  • High magnetic induction grain-oriented silicon steel with B800 being more than or equal to 1.94T and production method thereof

    CN104561795A

  • Production method of oriented silicon steel

    CN107779727A

  • Novel production method for normalizing and cooling high-magnetic-induction oriented silicon steel and product