A Ti-6Al-4V titanium alloy and its heat treatment process

Through the solid solution aging heat treatment process, the heat treatment process of titanium alloy is simplified, and a two-state structure with an equiaxed primary α phase and a sheet α phase is formed, which solves the problems of complex process and high cost in the prior art, and improves the titanium alloy comprehensive mechanical properties.

CN118726879BActive Publication Date: 2024-11-15BAOJI BUM IND CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411232010.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-15
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The existing titanium alloy has complex heat treatment technology, cumbersome operation, high cutting force and high cost in subsequent processing, making it difficult to effectively regulate the microstructure of Ti-6Al-4V titanium alloy to improve the comprehensive mechanical properties.

Method used

The solid solution aging heat treatment process is adopted, including surface grinding and sealing treatment. The solid solution treatment temperature is between 850℃ and 950℃, and the aging treatment is carried out after water cooling. The aging temperature is 550℃ and the insulation time is 4 to 6 hours, forming an isometric Bistate structure of the primary α phase and the α phase of the sheet.

Benefits of technology

The heat treatment process is simplified, the mechanical cutting force of subsequent processing is reduced, the comprehensive mechanical properties of Ti-6Al-4V titanium alloy is improved, the production time is shortened and the cost is saved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726879B_ABST
    Figure CN118726879B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of titanium alloy heat processing, and specifically relates to a Ti‑6Al‑4V titanium alloy and a heat treatment process thereof, comprising the following steps: firstly, treating an oxide layer on the surface of a Ti‑6Al‑4V titanium alloy sample, then placing the treated titanium alloy sample into a heat treatment furnace, and heating it at a temperature lower than a β transformation temperature for solution treatment; taking out the sample after the solution treatment and then performing a hydrothermal treatment, then placing the sample after the water cooling treatment back into the heat treatment furnace for aging treatment, and then taking out the sample after the aging treatment and air cooling it to room temperature. The Ti‑6Al‑4V titanium alloy of the invention is heat treated, and after the heat treatment, the titanium alloy has better internal structure stability, higher hardness and mechanical properties, and better plasticity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of titanium alloy heat processing, and specifically relates to a Ti-6Al-4V titanium alloy and a heat treatment process thereof. Background Art

[0002] Titanium alloy is an alloy composed of titanium and other elements. Titanium alloy has been widely used in aerospace, chemical medicine, sports and leisure, medical industry and automobile industry due to its advantages of low density, high strength ratio, high corrosion resistance, good low temperature performance and high chemical activity. Titanium alloys are mainly divided into three categories: α titanium alloy, β titanium alloy and α+β titanium alloy, with alloy codes TA, TB and TC respectively. At present, the most commonly used titanium alloy in industrial production is TC4, i.e. Ti-6Al-4V, and most industrial products are developed around this alloy. TC4 is widely used in the manufacture of engine-related parts and various load-bearing beams and other components, so its performance requirements are higher. The performance of titanium alloy is closely related to the organization, so it is necessary to regulate the microstructure by heat treating Ti-6Al-4V titanium alloy to achieve this goal.

[0003] Common heat treatment methods for titanium alloys include solution aging, quenching, and annealing. Solution aging treatment is to heat the titanium alloy to a set solution temperature so that the solute in the titanium alloy can be completely dissolved in the titanium alloy matrix. In order to prevent the solute in the titanium alloy from re-precipitating, the titanium alloy needs to be cooled rapidly to form a solid solution strengthening effect. After that, the titanium alloy is aged at a set temperature and time to promote the improvement of the strength and hardness of the titanium alloy, and to maintain good plasticity and toughness. Quenching treatment includes three processes: heating, heat preservation, and cooling, which uses phase change to produce a strengthening effect. The strengthening effect of titanium alloy after quenching is related to factors such as the properties and concentration of alloying elements. These factors have a great relationship with the type, distribution, and quantity of phases obtained after quenching of titanium alloys. Annealing treatment is to heat the titanium alloy to a certain temperature and keep it warm, and then slowly cool it to room temperature. Annealing treatment is mainly to eliminate stress and defects, thereby improving the plasticity, toughness, processing performance and corrosion resistance of titanium alloys.

[0004] If you want to improve the comprehensive mechanical properties of Ti-6Al-4V titanium alloy, the most critical issue is to regulate the microstructure of Ti-6Al-4V titanium alloy. However, the existing heat treatment process is complex and cumbersome to operate when regulating the microstructure of titanium alloy. The mechanical cutting force is large during subsequent processing, and the cost is high. Summary of the invention

[0005] In view of the deficiencies of the above-mentioned prior art, the object of the present invention is to provide a Ti-6Al-4V titanium alloy and a heat treatment process thereof. The Ti-6Al-4V titanium alloy of the present invention regulates the microstructure by a heat treatment method to ensure that the comprehensive mechanical properties are improved. The heat treatment process method is simple and easy to operate, which reduces the mechanical cutting force of the Ti-6Al-4V titanium alloy during subsequent processing, thereby reducing costs and saving time.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] A heat treatment process of Ti-6Al-4V titanium alloy comprises the following steps:

[0008] The surface of the Ti-6Al-4V titanium alloy sample was pre-treated by grinding to remove the oxide layer on the surface of the sample, and then sealed;

[0009] The polished Ti-6Al-4V sample was solution treated at a temperature of 850°C to 950°C and then water cooled.

[0010] The Ti-6Al-4V sample after solution water cooling was polished to remove the surface oxide layer, and then subjected to aging treatment. After the aging treatment, it was air-cooled to room temperature to obtain the heat-treated Ti-6Al-4V titanium alloy.

[0011] In a preferred embodiment of the present invention, the temperature during the solution treatment is 880°C and 950°C below the β phase transformation point, and 1000°C above the β phase transformation point. The holding time for the solution treatment is 1 h. When the Ti-6Al-4V titanium alloy is heat treated at the upper temperature of the α+β two-phase region, that is, at a temperature lower than the β phase transformation point, an equiaxed primary α phase and a lamellar α phase transformed from the β phase will be formed. Due to the formation of this microstructure, the comprehensive mechanical properties of the Ti-6Al-4V titanium alloy will be improved. It is further preferred that the solution treatment temperature is 950°C and the insulation is performed for 1 h.

[0012] In a preferred embodiment of the present invention, the solution treatment time is 60 min to 90 min.

[0013] In a preferred embodiment of the present invention, the aging treatment temperature is 550°C. The aging temperature plays a decisive role in the size of the secondary α phase. The volume fraction of the secondary α phase in the Ti-6Al-4V titanium alloy will have a great influence on the yield strength. Therefore, the aging treatment temperature is determined to be 550°C.

[0014] In a preferred embodiment of the present invention, the aging treatment time is 4 to 6 h. When the temperature during the aging treatment is 550°C, the holding time for the aging treatment is selected to be 4 h and 6 h, respectively. If the aging time in the Ti-6Al-4V titanium alloy is too long, the ω phase formed will provide nucleation points for the primary α phase, increasing the volume fraction of the primary α phase, and the lamellar α phase will also be affected by the excessively long aging time, resulting in an increase in volume fraction, an increase in aspect ratio, and coarsening of grains. Due to the influence of these factors, the mechanical properties of the Ti-6Al-4V titanium alloy are reduced, and it is further preferred that the holding time for the aging treatment is 4 h.

[0015] In a preferred embodiment of the present invention, the water cooling temperature is 20° C. and the water cooling time is 30 s.

[0016] In a preferred embodiment of the present invention, the tensile strength of the heat-treated Ti-6Al-4V titanium alloy is 1089 MPa-1171 MPa, the yield strength is 1005 MPa-1151 MPa, and the elongation is 5.3%-10%.

[0017] In a preferred embodiment of the present invention, the method for treating the surface of the Ti-6Al-4V titanium alloy sample is as follows: take a Ti-6Al-4V with a size of 10*10*10 mm, remove the surface oxide layer with sandpaper, and then seal and store it.

[0018] When the selected solution temperature is lower than the β phase transformation point of 995℃, the strength of the titanium alloy will increase with the increase of the solution temperature. When the selected solution temperature is higher than the β phase transformation point, the strength of the titanium alloy will show a downward trend with the increase of the solution temperature. And the plasticity of Ti-6Al-4V titanium alloy also shows a downward trend with the increase of the temperature during solution treatment. When the solution temperature of the alloy is higher than the β phase transformation point, the reason for the decrease in strength and plasticity is that the microstructure of Ti-6Al-4V titanium alloy is transformed into lamellar Widmanstatten. The aging temperature has little effect on the primary α phase in the microstructure of Ti-6Al-4V titanium alloy, but has a crucial influence on the size of the secondary α phase, that is, the lamellar α phase. In particular, the dynamic tensile strength of Ti-6Al-4V titanium alloy with dual-state structure will decrease with the increase of the width of the lamellar α phase, and the volume fraction of the lamellar α phase will have a great influence on the yield strength of Ti-6Al-4V titanium alloy.

[0019] Another object of the present invention is to provide a Ti-6Al-4V titanium alloy obtained by the heat treatment process described in any one of the above, wherein the Ti-6Al-4V titanium alloy consists of an α phase and a small amount of β phase.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The present invention targets Ti-6Al-4V, and in order to obtain a better microstructure and better performance, the Ti-6Al-4V is subjected to a solution treatment and an aging treatment. In order to obtain a dual-state structure with a lamellar α phase, the Ti-6Al-4V titanium alloy is subjected to a solution treatment at a higher temperature in the α+β two-phase region, and the solution treatment temperature is 850°C to 950°C. During the cooling and aging process, the content of the equiaxed α phase will decrease, and the secondary α phase, i.e., the lamellar α phase, is generated by the decomposition of the β phase. In order to obtain a large amount of lamellar α phase, heat treatment is required below the β phase transformation point. The content of the equiaxed α phase is very sensitive to the heat treatment temperature. Therefore, at a temperature lower than the β phase transformation point, the content and size of the equiaxed primary α phase will decrease, and the content and size of the precipitated lamellar α phase will increase. In order to obtain a lamellar α phase with appropriate size and content, the aging time should not be too long during the aging process, and the aging treatment time is 4 h to 6 h. h. If the aging time is too long, the content of lamellar α phase will increase to a certain extent, which will lead to a decrease in the plasticity of Ti-6Al-4V titanium alloy. If the size of lamellar α phase increases to a certain extent, the hardness of Ti-6Al-4V titanium alloy will decrease.

[0022] The heat treatment process of the Ti-6Al-4V titanium alloy of the present invention is simple and easy to operate, which reduces the mechanical cutting force of the Ti-6Al-4V titanium alloy during subsequent processing, thereby shortening the production time and saving costs.

[0023] 3. The present invention adopts a solution aging method in view of the characteristics and properties of Ti-6Al-4V titanium alloy. This method can achieve a dual-state structure of lamellar α phase with appropriate size and content in the Ti-6Al-4V titanium alloy after solution aging treatment, thereby improving the comprehensive mechanical properties of the Ti-6Al-4V titanium alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a SEM microstructure image of the Ti-6Al-4V titanium alloy after heat treatment in Example 1 of the present invention.

[0025] Figure 2 This is a SEM microstructure image of the Ti-6Al-4V titanium alloy after heat treatment in Example 2 of the present invention.

[0026] Figure 3 This is a SEM microstructure image of the Ti-6Al-4V titanium alloy after heat treatment in Example 3 of the present invention.

[0027] Figure 4 This is a SEM microstructure image of the Ti-6Al-4V titanium alloy after heat treatment in Example 4 of the present invention.

[0028] Figure 5This is a SEM microstructure picture of the Ti-6Al-4V titanium alloy after heat treatment in Comparative Example 1 of the present invention.

[0029] Figure 6 This is a SEM microstructure picture of the Ti-6Al-4V titanium alloy after heat treatment in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0030] The following is a detailed description of the technical solutions in the embodiments of the present invention in combination with the preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] It should be noted that all professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.

[0032] Example 1

[0033] A heat treatment process of Ti-6Al-4V titanium alloy comprises the following steps:

[0034] (1) Take a Ti-6Al-4V titanium alloy substrate with a size of 10 mm*10 mm*10 mm, and use sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to polish and remove the oxide layer on the surface of the Ti-6Al-4V substrate.

[0035] (2) The Ti-6Al-4V matrix obtained in step (1) is placed in a heat treatment furnace and heated to 880°C. The solution holding time is 1 h. After the holding time is reached, the Ti-6Al-4V titanium alloy is taken out and water-cooled at 20°C for 30 s.

[0036] (3) The samples after water cooling treatment were polished again with sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to remove the oxide layer on the surface of the Ti-6Al-4V matrix, and then placed in the heat treatment furnace again and heated to 550°C for aging and holding time of 4 h. After being taken out and air-cooled to room temperature, the heat-treated Ti-6Al-4V titanium alloy was obtained.

[0037] Example 2

[0038] A heat treatment process of Ti-6Al-4V titanium alloy comprises the following steps:

[0039] (1) Take a Ti-6Al-4V titanium alloy substrate with a size of 10 mm*10 mm*10 mm, and use sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to polish and remove the oxide layer on the surface of the Ti-6Al-4V substrate.

[0040] (2) The Ti-6Al-4V matrix obtained in step (1) is placed in a heat treatment furnace and heated to 880°C. The solution holding time is 1 h. After the holding time is reached, the Ti-6Al-4V titanium alloy is taken out and water-cooled at 20°C for 30 s.

[0041] (3) The samples after water cooling treatment were polished again with sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to remove the oxide layer on the surface of the Ti-6Al-4V matrix, and then placed in the heat treatment furnace again and heated to 550°C for aging and holding time of 6 h. After being taken out and air-cooled to room temperature, the heat-treated Ti-6Al-4V titanium alloy was obtained.

[0042] Example 3

[0043] A heat treatment process of Ti-6Al-4V titanium alloy comprises the following steps:

[0044] (1) Take a Ti-6Al-4V titanium alloy substrate with a size of 10 mm*10 mm*10 mm, and use sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to polish and remove the oxide layer on the surface of the Ti-6Al-4V substrate.

[0045] (2) The Ti-6Al-4V matrix obtained in step (1) is placed in a heat treatment furnace and heated to 950°C. The solution holding time is 1 h. After the holding time is reached, the Ti-6Al-4V titanium alloy is taken out and water-cooled at 20°C for 30 s.

[0046] (3) The samples after water cooling treatment were polished again with sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to remove the oxide layer on the surface of the Ti-6Al-4V matrix, and then placed in the heat treatment furnace again and heated to 550°C for aging and holding time of 4 h. After being taken out and air-cooled to room temperature, the heat-treated Ti-6Al-4V titanium alloy was obtained.

[0047] Example 4

[0048] A heat treatment process of Ti-6Al-4V titanium alloy comprises the following steps:

[0049] (1) Take a Ti-6Al-4V titanium alloy substrate with a size of 10 mm*10 mm*10 mm, and use sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to polish and remove the oxide layer on the surface of the Ti-6Al-4V substrate.

[0050] (2) The Ti-6Al-4V matrix obtained in step (1) is placed in a heat treatment furnace and heated to 950°C. The solution holding time is 1 h. After the holding time is reached, the Ti-6Al-4V titanium alloy is taken out and water-cooled at 20°C for 30 s.

[0051] (3) The samples after water cooling treatment were polished again with sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to remove the oxide layer on the surface of the Ti-6Al-4V matrix, and then placed in the heat treatment furnace again and heated to 550°C for aging and holding time of 6 h. After being taken out and air-cooled to room temperature, the heat-treated Ti-6Al-4V titanium alloy was obtained.

[0052] Example 5

[0053] A heat treatment process of Ti-6Al-4V titanium alloy comprises the following steps:

[0054] (1) Take a Ti-6Al-4V titanium alloy substrate with a size of 10 mm*10 mm*10 mm, and use sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to polish and remove the oxide layer on the surface of the Ti-6Al-4V substrate.

[0055] (2) The Ti-6Al-4V matrix obtained in step (1) is placed in a heat treatment furnace and heated to 850°C. The solution holding time is 1 hour. After the holding time is reached, the Ti-6Al-4V titanium alloy is taken out and water-cooled at 20°C for 30 seconds.

[0056] (3) The samples after water cooling treatment were polished again with sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to remove the oxide layer on the surface of the Ti-6Al-4V matrix, and then placed in the heat treatment furnace again and heated to 550°C for aging and holding time of 4 h. After being taken out and air-cooled to room temperature, the heat-treated Ti-6Al-4V titanium alloy was obtained.

[0057] Example 6

[0058] A heat treatment process of Ti-6Al-4V titanium alloy comprises the following steps:

[0059] (1) Take a Ti-6Al-4V titanium alloy substrate with a size of 10 mm*10 mm*10 mm, and use sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to polish and remove the oxide layer on the surface of the Ti-6Al-4V substrate.

[0060] (2) The Ti-6Al-4V matrix obtained in step (1) is placed in a heat treatment furnace and heated to 950°C. The solution holding time is 1 hour. After the holding time is reached, the Ti-6Al-4V titanium alloy is taken out and water-cooled at 20°C for 30 seconds.

[0061] (3) The samples after water cooling treatment were polished again with sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to remove the oxide layer on the surface of the Ti-6Al-4V matrix, and then placed in the heat treatment furnace again and heated to 550°C for aging and holding time of 5 h. After being taken out and air-cooled to room temperature, the heat-treated Ti-6Al-4V titanium alloy was obtained.

[0062] Comparative Example 1

[0063] A heat treatment process of Ti-6Al-4V titanium alloy comprises the following steps:

[0064] (1) Take a Ti-6Al-4V titanium alloy substrate with a size of 10 mm*10 mm*10 mm, and use sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to polish and remove the oxide layer on the surface of the Ti-6Al-4V substrate.

[0065] (2) The Ti-6Al-4V matrix obtained in step (1) is placed in a heat treatment furnace and heated to 1000°C. The solution holding time is 1 hour. After the holding time is reached, the Ti-6Al-4V titanium alloy is taken out and water-cooled at 20°C for 30 seconds.

[0066] (3) The samples after water cooling treatment were polished again with sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to remove the oxide layer on the surface of the Ti-6Al-4V matrix, and then placed in the heat treatment furnace again and heated to 550°C for aging and holding time of 4 h. After being taken out and air-cooled to room temperature, the heat-treated Ti-6Al-4V titanium alloy was obtained.

[0067] Comparative Example 2

[0068] A heat treatment process of Ti-6Al-4V titanium alloy comprises the following steps:

[0069] (1) Take a Ti-6Al-4V titanium alloy substrate with a size of 10 mm*10 mm*10 mm, and use sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to polish and remove the oxide layer on the surface of the Ti-6Al-4V substrate.

[0070] (2) The Ti-6Al-4V matrix obtained in step (1) is placed in a heat treatment furnace and heated to 1000°C. The solution holding time is 1 hour. After the holding time is reached, the Ti-6Al-4V titanium alloy is taken out and water-cooled at 20°C for 30 seconds.

[0071] (3) The samples after water cooling treatment were polished again with sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to remove the oxide layer on the surface of the Ti-6Al-4V matrix, and then placed in the heat treatment furnace again and heated to 550°C for aging and holding time of 6 h. After being taken out and air-cooled to room temperature, the heat-treated Ti-6Al-4V titanium alloy was obtained.

[0072] Comparative Example 3

[0073] A heat treatment process of Ti-6Al-4V titanium alloy comprises the following steps:

[0074] (1) Take a Ti-6Al-4V titanium alloy substrate with a size of 10 mm*10 mm*10 mm, and use sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to polish and remove the oxide layer on the surface of the Ti-6Al-4V substrate.

[0075] (2) The Ti-6Al-4V matrix obtained in step (1) is placed in a heat treatment furnace and heated to 1050°C. The solution holding time is 1 hour. After the holding time is reached, the Ti-6Al-4V titanium alloy is taken out and water-cooled at 20°C for 30 seconds.

[0076] (3) The samples after water cooling treatment were polished again with sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to remove the oxide layer on the surface of the Ti-6Al-4V matrix, and then placed in the heat treatment furnace again and heated to 550°C for aging and holding time of 4 h. After being taken out and air-cooled to room temperature, the heat-treated Ti-6Al-4V titanium alloy was obtained.

[0077] Comparative Example 4

[0078] A heat treatment process of Ti-6Al-4V titanium alloy comprises the following steps:

[0079] (1) Take a Ti-6Al-4V titanium alloy substrate with a size of 10 mm*10 mm*10 mm, and use sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to polish and remove the oxide layer on the surface of the Ti-6Al-4V substrate.

[0080] (2) The Ti-6Al-4V matrix obtained in step (1) is placed in a heat treatment furnace and heated to 950°C. The solution holding time is 1 hour. After the holding time is reached, the Ti-6Al-4V titanium alloy is taken out and water-cooled at 20°C for 30 seconds.

[0081] (3) The samples after water cooling treatment were polished again with sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to remove the oxide layer on the surface of the Ti-6Al-4V matrix, and then placed in the heat treatment furnace again and heated to 550°C for aging and holding time of 3.5 h. After being taken out and air-cooled to room temperature, the heat-treated Ti-6Al-4V titanium alloy was obtained.

[0082] Comparative Example 5

[0083] A heat treatment process of Ti-6Al-4V titanium alloy comprises the following steps:

[0084] (1) Take a Ti-6Al-4V titanium alloy substrate with a size of 10 mm*10 mm*10 mm, and use sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to polish and remove the oxide layer on the surface of the Ti-6Al-4V substrate.

[0085] (2) The Ti-6Al-4V matrix obtained in step (1) is placed in a heat treatment furnace and heated to 950°C. The solution holding time is 1 hour. After the holding time is reached, the Ti-6Al-4V titanium alloy is taken out and water-cooled at 20°C for 30 seconds.

[0086] (3) The samples after water cooling treatment were polished again with sandpaper with mesh sizes of 80#, 240#, 500#, 800#, 1000#, 1200#, 1500#, 2000#, and 3000# to remove the oxide layer on the surface of the Ti-6Al-4V matrix, and then placed in the heat treatment furnace again and heated to 550°C for aging and holding time of 6.5 h. After being taken out and air-cooled to room temperature, the heat-treated Ti-6Al-4V titanium alloy was obtained.

[0087] Performance Testing

[0088] By comparing Example 1 to Example 6 and Comparative Example 1 to Comparative Example 5, it can be found that by changing the solution temperature and aging time of the Ti-6Al-4V titanium alloy, the α phase content and size of the titanium alloy sample decrease with the increase of the solution temperature; and the content and size of the precipitated lamellar α phase will also continue to increase with the increase of the solution temperature, and the hardness of the Ti-6Al-4V titanium alloy will also be improved. The above embodiments illustrate that the parameters of the heat treatment of the Ti-6Al-4V titanium alloy can be adjusted in a wide range. According to the actual industrial production and life needs of the Ti-6Al-4V titanium alloy, the required comprehensive mechanical properties can be achieved by changing and matching the solution temperature and aging time of the Ti-6Al-4V titanium alloy solution aging.

[0089] Mechanical properties test: The mechanical properties of Examples 1 to 6 and Comparative Examples 1 to 5 were tested using a 5980 dual-column floor-standing universal testing machine. The results are shown in Table 1.

[0090] Table 1 Mechanical properties test results of Example 1 to Example 6 and Comparative Example 1 to Comparative Example 5

[0091]

[0092] Table 1 shows the mechanical property test results of the Ti-6Al-4V titanium alloy after heat treatment of Examples 1 to 6 of the present invention and Comparative Examples 1 to 5. The results show that when the solution treatment is carried out at a higher temperature in the dual-phase region in the embodiments, a large amount of α phase is transformed into β phase, which provides good organizational conditions for the later aging phase transformation of the titanium alloy, thereby improving the strength of the titanium alloy. After solution aging, part of the equiaxed primary α structure will be transformed into a lamellar structure of the β phase, and a uniformly distributed structure is obtained. The comprehensive mechanical properties of Example 3 are better. If the titanium alloy is treated at a temperature higher than the β phase transformation temperature, it will form Widmanstatten, resulting in increased brittleness and a significant reduction in plasticity, which will reduce the comprehensive mechanical properties of the titanium alloy.

[0093] Figure 1 This is the SEM microstructure picture of the Ti-6Al-4V titanium alloy after heat treatment in Example 1 of the present invention. It can be seen from the figure that under this heat treatment process, the structure is mainly composed of equiaxed α phase, and there is a partial lamellar α phase when water-cooled, and the β transformation structure in the structure is composed of lamellar α phase and β matrix.

[0094] Figure 2 This is the SEM microstructure picture of the Ti-6Al-4V titanium alloy after heat treatment in Example 2 of the present invention. It can be seen from the figure that as the solution temperature increases, the α grains will grow accordingly, and the β phase is distributed on the α equiaxed grain boundaries. At this time, the sample composition is uniform. As the aging time increases, the strength and hardness of the sample are correspondingly improved.

[0095] Figure 3 This is a SEM microstructure picture of the Ti-6Al-4V titanium alloy after heat treatment in Example 3 of the present invention. It can be seen from the figure that the content of the equiaxed α phase is reduced due to the transformation of the α phase to the β phase. The stable α phase and β phase are formed by the transformation of the secondary α phase and the β phase obtained from the β phase before.

[0096] Figure 4 This is the SEM microstructure picture of the Ti-6Al-4V titanium alloy after heat treatment in Example 4 of the present invention. It can be seen from the figure that when the temperature of the solid solution continues to rise to near the phase transformation point, the amount of precipitation of the lamellar α phase increases, and the size also increases, and the equiaxial α phase in the structure appears to be fused.

[0097] Figure 5 This is a SEM microstructure picture of the Ti-6Al-4V titanium alloy after heat treatment in Comparative Example 1 of the present invention. It can be seen from the figure that when the temperature of the solid solution exceeds the phase transition point, the structure undergoes a phase transition, the content of the α phase decreases, and the content of the β phase increases. In addition, during the cooling process of the β phase, the needle-shaped α phase that is transformed will form α clusters.

[0098] Figure 6This is the SEM microstructure picture of the Ti-6Al-4V titanium alloy after heat treatment in Comparative Example 2 of the present invention. It can be seen from the figure that when heat treatment is carried out above the phase transformation point, the α phase transforms to the β phase more fully, and the β phase grain size increases, and the hardness is significantly improved. However, due to the transformation of the structure, the large amount of β phase causes the elongation to decrease significantly.

[0099] In summary, the present invention targets Ti-6Al-4V and performs a solid solution aging treatment on it in order to obtain a better microstructure and better performance. In order to obtain a dual-state structure with a lamellar α phase, the Ti-6Al-4V titanium alloy is subjected to a solid solution treatment at a higher temperature in the α+β two-phase region. During the cooling and aging process, the content of the equiaxed α phase will decrease, and the secondary α phase, i.e., the lamellar α phase, is generated by the decomposition of the β phase. In order to obtain a large amount of lamellar α phase, it is necessary to perform a heat treatment below the β phase transformation point. The content of the equiaxed α phase is reduced. The amount is very sensitive to the heat treatment temperature, so at a temperature lower than the β phase transformation point, the content and size of the equiaxed primary α phase will decrease, and the content and size of the precipitated lamellar α phase will increase. In order to obtain the lamellar α phase with appropriate size and content, the aging time should not be too long during the aging process. If the aging time is too long, the content of the lamellar α phase will increase to a certain extent, which will lead to a decrease in the plasticity of the Ti-6Al-4V titanium alloy. When the size of the lamellar α phase increases to a certain extent, the hardness of the Ti-6Al-4V titanium alloy will decrease.

[0100] It should be noted that when the present invention relates to a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundant description, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, once those skilled in the art know the basic creative concept, they can make other changes and modifications to these embodiments. Therefore, the attached protection scope is intended to be interpreted as including the preferred embodiment and all changes and modifications that fall within the scope of the present invention.

[0101] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the protection scope of the present invention and its equivalent technology, the present invention is also intended to include these changes and variations.

Claims

1. A heat treatment process of Ti-6Al-4V titanium alloy, characterized in that: The following steps are involved: The surface of Ti-6Al-4V titanium alloy is pre-treated by grinding; The polished Ti-6Al-4V titanium alloy sample is subjected to a solution treatment at a temperature of 950°C, followed by water cooling after the solution treatment; the solution treatment time is 60 to 90 minutes; The Ti-6Al-4V titanium alloy sample after solution water cooling was polished to remove the surface oxide layer, and then subjected to aging treatment. After the aging treatment, it was air-cooled to room temperature to obtain a heat-treated Ti-6Al-4V titanium alloy. The aging treatment temperature was 550°C, and the aging treatment time was 4h to 6h.

2. The heat treatment process of Ti-6Al-4V titanium alloy according to claim 1, characterized in that: The water cooling temperature is 20° C. and the water cooling time is 30 seconds.

3. The heat treatment process of Ti-6Al-4V titanium alloy according to claim 1, characterized in that: The specific pretreatment method is: using sandpaper with different mesh sizes to polish the surface of the Ti-6Al-4V titanium alloy successively to remove the surface oxide layer.

4. The heat treatment process of Ti-6Al-4V titanium alloy according to claim 1, characterized in that: The size of the Ti-6Al-4V titanium alloy is 10 mm×10 mm×10 mm.

5. A Ti-6Al-4V titanium alloy obtained by the heat treatment process according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Titanium alloy strong toughening treatment method based on pulse current

    CN110592509A

  • Quadruple heat treatment process for improving comprehensive mechanical properties of (alpha + beta) type titanium alloy

    CN116162876A

  • Heat treatment method for improving tensile property of TC4 titanium alloy

    CN116441565A

  • TC4 titanium alloy heat treatment method and application thereof

    CN117165884A

  • Manufacturing method for improving welding seam strength of titanium alloy welding part

    CN117888047A