High-strength and high-thermal-conductivity copper alloy for repairing crystallizer substrate and preparation method of high-strength and high-thermal-conductivity copper alloy
Through the gas atomization powdering and cold spraying process of Cu, Cr, and Zr combined with aging treatment, a copper alloy repair layer with high strength and high thermal conductivity is formed, which solves the thermal stress problem caused by high temperature in the existing technology and meets the crystallization requirements. The repair performance requirements of the device substrate.
Patent Information
- Application Number
- CN202410781971.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-18
AI Technical Summary
The existing copper alloy preparation method causes cracking, deformation, element segregation and grain coarsening due to thermal stress caused by high temperature when repairing the mold substrate. It is difficult to meet the requirements of high thermal conductivity, high strength and wear resistance, and may cause the shape of the substrate to change.
Using Cu, Cr, and Zr as raw materials, the copper alloy repair layer is prepared through aerosol powdering and cold spraying processes, and is subjected to aging treatment to form an FCC structure and nano-precipitated phases to improve strength and thermal conductivity, ensuring the relative strength of the repair layer. density and performance.
A copper alloy repair layer with high strength and high thermal conductivity is achieved, with a tensile strength higher than 430MPa and a thermal conductivity higher than 310W/(m·K). It avoids changes in the shape of the substrate and meets the performance requirements for mold repair.
Smart Images

Figure CN118726962A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of copper alloy materials and relates to a high-thermal-conductivity, high-strength copper alloy repair layer material and a preparation method thereof. Technical Background
[0002] High-strength and high-conductivity copper alloys have good mechanical and physical properties and are widely used in power, electronics, machinery and other industrial fields. The crystallizer is an important component in the continuous casting machine, and its substrate is usually made of copper-chromium alloy and copper-chromium-zirconium alloy. The upper and middle parts of the crystallizer copper plate are washed by high-temperature molten steel for a long time, while its back is cooled by 30-40°C water. The crystallizer copper plate is subject to the risk of high-temperature oxidation, hot and cold fatigue, thermal cracks and stress deformation. In the lower mouth area and vicinity of the crystallizer, the copper plate is subjected to severe high-temperature friction and wear damage during repeated billet drawing. Therefore, the crystallizer substrate needs to be repaired. The crystallizer repair layer needs to have good thermal conductivity, excellent wear resistance, corrosion resistance and thermal shock resistance. And during the repair and subsequent processing, the crystallizer substrate will not be deformed and the shape will not change.
[0003] Generally, the mainstream methods for preparing copper alloys are melting casting, selective laser melting, electron beam melting, etc. However, these methods have high temperatures, and thermal stress will cause the shape of the crystallizer substrate to change. In addition, although metal melting can ensure good bonding between interlayer metals, rapid solidification and high temperature also bring new problems, such as cracking, deformation, element segregation, grain coarsening, phase change, oxidation, etc. caused by thermal stress.
[0004] Cold spray technology is considered to be a solid-state additive technology that can prepare high-reflectivity, oxidation-sensitive or phase-change-sensitive materials. Due to the low temperature and no melting, oxidation and other solidification-related problems can be minimized. Cold spray has the advantages of high deposition efficiency, good raw material reusability, and environmental friendliness. By adjusting the process parameters, CuCrZr alloys with no phase change, no oxidation, and no thermal deformation can be obtained. It has industrial application scenarios in the repair of continuous casting machine slab crystallizer substrates. Summary of the invention
[0005] The present invention aims to provide a high-strength and high-thermal-conductivity copper alloy for a crystallizer substrate repair layer and a preparation method thereof. The invention uses Cu, Cr, and Zr as raw materials, prepares alloy powders by atomization powder making and cold spraying processes, and then combines aging treatment to obtain an alloy with high strength and high thermal conductivity, which meets the performance requirements of the crystallizer substrate repair layer.
[0006] To achieve the above purpose, the technical solution provided by the present invention is:
[0007] The mass percentage of the elements in the copper alloy is: Cu 98.84-99.35%, Cr 0.53-0.85%, Zr 0.12-0.31%. According to the mass ratio requirements of the elements, the raw materials are weighed and then atomized and pulverized. After the obtained powder is dried and screened, a copper alloy repair layer blank is obtained by cold spraying process; the blank presents a morphology of flattened powder particles stacked in layers; in some of the particles, approximately equiaxed coarse crystals are clearly visible inside, and these parts undergo plastic deformation, or the plastic deformation is very small; while the grains at the boundaries of other particles present an elongated morphology, and these structures undergo severe plastic deformation; the relative density of the repair layer blank reaches more than 98.7%, and the average flattening rate of the powder particles is less than 0.458; then an aging treatment is carried out, and during the aging treatment, the boundaries of the particles with large deformations are preferentially recrystallized, so that the original particle interface forms a metallurgical bond, and the relative density of the repair layer after aging is maintained above 98.5%, and the strength and thermal conductivity are greatly improved.
[0008] The cold spraying process conditions are: gas preheating temperature of 540-560°C, gas pressure of 3.2-3.5MPa, powder feeding rate of 220-250SLM, and spray gun moving speed of 60-63mm / s. The aging treatment conditions are: heat preservation at 590-620°C for 1-2h, and then furnace cooling to room temperature. After cold spraying and aging treatment, the matrix of the obtained CuCrZr alloy is an FCC structure, with spherical and rod-shaped Cr nano-precipitates and spherical Zr-rich precipitates in the crystal. These dispersed precipitates play a strengthening role, and the strength of the obtained repair layer is higher than 430MPa, and the thermal conductivity is higher than 310W / (m·K).
[0009] A method for preparing a high-strength and high-thermal-conductivity copper alloy for a crystallizer substrate repair layer comprises the following steps:
[0010] (1) Raw material preparation: Prepare Cu, Cr, and Zr raw materials in the required proportions. CuCr and CuZr master alloys with known compositions may also be used.
[0011] (2) Gas atomization powder making: After the raw materials are weighed, gas atomization powder making is performed to obtain spherical solid solution alloy powder. Subsequently, air flow classification is performed to screen out spherical powder with a particle size range of -400 / +800 mesh, and the average particle size is 22 to 25 μm.
[0012] (3) Cold spraying: The screened powder is used to prepare a block using a cold spray system. The cold spray gas preheating temperature is 540-560°C, the gas pressure is 3.2-3.5MPa, the powder feeding rate is 220-250SLM, and the spray gun moving speed is 60-63mm / s. The powder is deposited on the repaired substrate, and the cold sprayed copper alloy repair layer blank is obtained after cold spraying. The blank presents a morphology of flattened powder particles stacked in layers; some of the particles have clearly visible approximately equiaxed coarse grains inside, and these parts have undergone plastic deformation, or the plastic deformation is very small; while the grains at the boundaries of other particles have an elongated morphology, and these structures have undergone severe plastic deformation; the relative density of the repair layer blank reaches 98.7%, and the average flattening rate of the powder particles is less than 0.458; the tensile strength is 170-190MPa, and the thermal conductivity is 140-160W / (m·K).
[0013] (4) Aging treatment: The cold-sprayed copper alloy repair layer blank is heated to 590-620°C in a protective atmosphere, kept at this temperature for 1-2 hours, and then cooled to room temperature in the furnace to obtain the copper alloy repair layer after aging treatment. During the aging treatment, the grain boundaries with large deformation preferentially recrystallize, so that the original grain interface forms a metallurgical bond. After aging, the relative density of the repair layer remains above 98.5%, and the strength and thermal conductivity are greatly improved; the tensile strength is higher than 430MPa, and the thermal conductivity is higher than 310W / (m·K).
[0014] After the cold spraying and aging treatment, the matrix of the obtained CuCrZr alloy is an FCC structure, and the FCC structured Cr nanophase and Zr-rich nanoalloy phase are dispersed and precipitated in the crystal. This structure enables the alloy to have high strength and excellent thermal conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 Cross-sectional metallographic photograph of Example 1
[0016] Figure 2 XRD diffraction patterns of CuCrZr alloys of Examples 1, 2, 3, 4, and 5
[0017] Figure 3 TEM image of Example 1
[0018] Figure 4 TEM image of Cr precipitation phase and corresponding Cr element distribution diagram of Example 1
[0019] Figure 5 TEM image of Zr-rich precipitate phase of Example 1 and corresponding Zr element distribution diagram DETAILED DESCRIPTION
[0020] Example 1
[0021] (1) Raw material preparation: Weigh 99.35% Cu, 0.53% Cr, and 0.12% Zr according to the mass ratio.
[0022] (2) Gas atomization powder making: After the raw materials are weighed, gas atomization powder making is performed to obtain spherical solid solution alloy powder. Then, air flow classification is performed, and then spherical powder with a suitable particle size range is screened and dried for use.
[0023] (3) Cold spraying: The screened powder is used to prepare a block using a cold spray system. The powder used is a spherical powder of -400 / +800 mesh with an average particle size of 22 μm. The cold spray gas preheating temperature is 540°C, the gas pressure is 3.5 MPa, the powder feeding rate is 220 SLM, and the spray gun moving speed is 60 mm / s. The powder is deposited on the substrate to be repaired, and the repair layer blank is obtained after cold spraying. Figure 1 The metallographic photograph of the repair layer blank shows a flattened powder particle layered stacking morphology; some of the particles have clearly visible approximately equiaxed coarse grains inside, and these parts have undergone plastic deformation, or the plastic deformation is very small; while the grains at the boundaries of other particles are slender, and these structures have undergone serious plastic deformation; the relative density of the repair layer blank reaches 98.7%, and the average flattening rate of the powder particles reaches 0.453; the tensile strength is 172MPa, and the thermal conductivity is 140W / (m·K)
[0024] (4) Aging treatment. The substrate in the cold sprayed block is removed by electric spark wire cutting, and the block is placed in a tubular furnace and heated to 590°C under argon protection, kept warm for 2 hours, and then cooled to room temperature with the furnace to obtain a copper alloy repair layer after aging treatment. During the aging treatment, the grain boundaries with large deformations preferentially recrystallize, so that the original grain interface forms a metallurgical bond. After aging, the relative density of the repair layer is 98.7%, and the strength and thermal conductivity are greatly improved. Its tensile strength is 430MPa and its thermal conductivity is 318W / (m·K).
[0025] The CuCrZr alloy prepared by the method is composed of an FCC matrix and a Cr nanophase and a Zr-rich nanophase with an FCC structure distributed inside the grains. Figure 2 The XRD spectrum of the alloy shows that the matrix is an FCC structure. Since the precipitated phase is small and dispersed, and the volume content is less than 5%, it is not observed in the XRD spectrum. Figure 3 The TEM image of the alloy shows the equiaxed grains of the alloy. Figure 4 The TEM image of the Cr phase of the alloy and the corresponding Cr element distribution diagram show that the Cr phase is distributed in nanometer-scale particles. Figure 5The TEM photo of the Zr-rich phase of the alloy and the corresponding Zr element distribution map show that the Zr-rich phase is also in the form of nano-scale particles. The interior of the crystal consists of dispersed nano-scale FCC structured Cr phase and Zr-rich nano-phase, which constitute the alloy reinforcement. The particles are deformed into a flat shape, and nano-scale precipitated phases are precipitated in the nano-scale grains at the particle boundaries and the internal equiaxed crystals of the particles. This special structure allows the alloy to have high strength while still having excellent thermal conductivity, with a tensile strength of 430MPa and a thermal conductivity of 318W / (m·K).
[0026] Example 2
[0027] (1) Raw material preparation: weigh 98.84% Cu, 0.85% Cr, and 0.31% Zr according to the mass ratio;
[0028] (2) Gas atomization powder making: After the raw materials are weighed, gas atomization powder making is performed to obtain spherical solid solution alloy powder. Then, air flow classification is performed, and then spherical powder with a suitable particle size range is screened and dried for use.
[0029] (3) Cold spraying: The sieved powder is used to prepare a block using a cold spray system. The powder used is a spherical powder of -400 / +800 mesh with an average particle size of 25μm. The cold spray gas preheating temperature is 560℃, the gas pressure is 3.2MPa, the powder feeding rate is 250SLM, and the spray gun moving speed is 63mm / s. The powder is deposited on the repaired substrate, and the cold spray repair layer blank is obtained after cold spraying. The blank presents a morphology of flattened powder particles stacked in layers; some of the particles have clearly visible approximately equiaxed coarse crystals inside, and these parts have undergone plastic deformation, or the plastic deformation is very small; while the grains at the boundaries of other particles have an elongated morphology, and these structures have undergone severe plastic deformation; the relative density of the repair layer blank reaches 98.9%, and the average flattening rate of the powder particles reaches 0.461; the tensile strength is 190MPa, and the thermal conductivity is 160W / (m·K)
[0030] (4) Aging treatment. The substrate in the cold sprayed block is removed by electric spark wire cutting, and the block is placed in a tubular furnace and heated to 620°C under argon protection, kept warm for 1 hour, and then cooled to room temperature with the furnace to obtain a copper alloy repair layer after aging treatment. During the aging treatment, the grain boundaries with large deformations preferentially recrystallize, so that the original grain interface forms a metallurgical bond. After aging, the relative density of the repair layer is 99.1%, and the strength and thermal conductivity are greatly improved. Its tensile strength is 441MPa and its thermal conductivity is 310W / (m·K).
[0031] The CuCrZr alloy prepared by the method is composed of an FCC matrix and a Cr nanophase and a Zr-rich nanophase with an FCC structure distributed inside the grains. Figure 2The XRD pattern of the alloy is shown in Figure 2. This special structure makes the alloy have high strength and excellent thermal conductivity, with a tensile strength of 441 MPa and a thermal conductivity of 310 W / (m·K).
[0032] Example 3
[0033] (1) Raw material preparation: weigh 98.87% Cu, 0.85% Cr, and 0.28% Zr according to the mass ratio;
[0034] (2) Gas atomization powder making: After the raw materials are weighed, gas atomization powder making is performed to obtain spherical solid solution alloy powder. Then, air flow classification is performed, and then spherical powder with a suitable particle size range is screened and dried for use.
[0035] (3) Cold spraying: The sieved powder is used to prepare a block using a cold spray system. The powder used is a spherical powder of -400 / +800 mesh with an average particle size of 23μm. The cold spray gas preheating temperature is 550℃, the gas pressure is 3.4MPa, the powder feeding rate is 240SLM, and the spray gun moving speed is 61mm / s. The powder is deposited on the repaired substrate, and the cold spray repair layer blank is obtained after cold spraying. The blank presents a morphology of flattened powder particles stacked in layers; some of the particles have clearly visible approximately equiaxed coarse crystals inside, and these parts have undergone plastic deformation, or the plastic deformation is very small; while the grains at the boundaries of other particles have an elongated morphology, and these structures have undergone severe plastic deformation; the relative density of the repair layer blank reaches 98.8%, and the average flattening rate of the powder particles reaches 0.455; the tensile strength is 176MPa, and the thermal conductivity is 147W / (m·K)
[0036] (4) Aging treatment. The substrate in the cold sprayed block is removed by electric spark wire cutting, and the block is placed in a tubular furnace, heated to 600°C under argon protection, kept warm for 1.5 hours, and then cooled to room temperature with the furnace to obtain a copper alloy repair layer after aging treatment. During the aging treatment, the grain boundaries with large deformations preferentially recrystallize, so that the original grain interfaces form a metallurgical bond. After aging, the relative density of the repair layer is 98.7%, and the strength and thermal conductivity are greatly improved. Its tensile strength is 439MPa and its thermal conductivity is 311W / (m·K). The CuCrZr alloy prepared by the above method consists of an FCC matrix and Cr nanophases and Zr-rich nanophases with FCC structure distributed inside the grains. Figure 2 The XRD pattern of the alloy is shown in Figure 2. This special structure makes the alloy have high strength and excellent thermal conductivity, with a tensile strength of 439 MPa and a thermal conductivity of 311 W / (m·K).
[0037] Example 4
[0038] (1) Raw material preparation: weigh 99.29% Cu, 0.53% Cr, and 0.18% Zr according to the mass ratio;
[0039] (2) Gas atomization powder making: After the raw materials are weighed, gas atomization powder making is performed to obtain spherical solid solution alloy powder. Then, air flow classification is performed, and then spherical powder with a suitable particle size range is screened and dried for use.
[0040] (3) Cold spraying: The screened powder is used to prepare a block using a cold spray system. The powder used is a spherical powder of -400 / +800 mesh with an average particle size of 24μm. The cold spray gas preheating temperature is 550℃, the gas pressure is 3.3MPa, the powder feeding rate is 230SLM, and the spray gun moving speed is 62mm / s. The powder is deposited on the repaired substrate, and the cold spray repair layer blank is obtained after cold spraying. The blank presents a morphology of flattened powder particles stacked in layers; some of the particles have clearly visible approximately equiaxed coarse crystals inside, and these parts have undergone plastic deformation, or the plastic deformation is very small; while the grains at the boundaries of other particles have an elongated morphology, and these structures have undergone severe plastic deformation; the relative density of the repair layer blank reaches 98.9%, and the average flattening rate of the powder particles reaches 0.454; the tensile strength is 179MPa, and the thermal conductivity is 152W / (m·K)
[0041] (4) Aging treatment. The substrate in the cold sprayed block is removed by electric spark wire cutting, and the block is placed in a tubular furnace and heated to 600°C under argon protection, kept warm for 2 hours, and then cooled to room temperature with the furnace to obtain a copper alloy repair layer after aging treatment. During the aging treatment, the grain boundaries with large deformations preferentially recrystallize, so that the original grain interface forms a metallurgical bond. After aging, the relative density of the repair layer is 99.1%, and the strength and thermal conductivity are greatly improved. Its tensile strength is 436MPa and its thermal conductivity is 313W / (m·K).
[0042] The CuCrZr alloy prepared by the method is composed of an FCC matrix and spherical and rod-shaped Cr nanophases and Zr-rich nanophases of an FCC structure distributed inside the grains. Figure 2 The XRD pattern of the alloy is shown in Figure 2. This special structure makes the alloy have high strength and excellent thermal conductivity, with a tensile strength of 436MPa and a thermal conductivity of 313W / (m·K).
[0043] Example 5
[0044] (1) Raw material preparation: weigh 99.14% Cu, 0.62% Cr, and 0.24% Zr according to the mass ratio;
[0045] (2) Gas atomization powder making: After the raw materials are weighed, gas atomization powder making is performed to obtain spherical solid solution alloy powder. Then, air flow classification is performed, and then spherical powder with a suitable particle size range is screened and dried for use.
[0046] (3) Cold spraying: The screened powder is used to prepare a block using a cold spray system. The powder used is a spherical powder of -400 / +800 mesh with an average particle size of 24μm. The cold spray gas preheating temperature is 560℃, the gas pressure is 3.3MPa, the powder feeding rate is 230SLM, and the spray gun moving speed is 62mm / s. The powder is deposited on the repaired substrate, and the cold spray repair layer blank is obtained after cold spraying. The blank presents a morphology of flattened powder particles stacked in layers; some of the particles have clearly visible approximately equiaxed coarse crystals inside, and these parts have undergone plastic deformation, or the plastic deformation is very small; while the grains at the boundaries of other particles have an elongated morphology, and these structures have undergone severe plastic deformation; the relative density of the repair layer blank reaches 98.9%, and the average flattening rate of the powder particles reaches 0.458; the tensile strength is 181MPa, and the thermal conductivity is 154W / (m·K)
[0047] (4) Aging treatment. The substrate in the cold sprayed block is removed by electric spark wire cutting, and the block is placed in a tubular furnace and heated to 610°C under argon protection. It is kept warm for 1.5 hours and then cooled to room temperature with the furnace to obtain the block after aging treatment. During the aging treatment, the grain boundaries with large deformations are preferentially recrystallized, so that the original grain interface forms a metallurgical bond. The relative density of the repair layer after aging is 99.2%, and the strength and thermal conductivity are greatly improved. Its tensile strength is 437MPa and its thermal conductivity is 315W / (m·K).
[0048] The CuCrZr alloy prepared by the method is composed of an FCC matrix and a Cr nanophase and a Zr-rich nanophase with an FCC structure distributed inside the grains. Figure 2 The XRD pattern of the alloy is shown in Figure 2. This special structure makes the alloy have high strength and excellent thermal conductivity, with a tensile strength of 437MPa and a thermal conductivity of 315W / (m·K).
Claims
1. A high-strength and high-thermal-conductivity copper alloy for a crystallizer substrate repair layer, characterized in that: The copper alloy has the following element mass percentages: Cu 98.84-99.35%, Cr 0.53-0.85%, and Zr 0.12-0.31%. According to the element mass ratio requirements, the raw materials are weighed and then atomized and pulverized. After the obtained powder is dried and screened, a copper alloy repair layer blank is obtained by a cold spraying process. The blank presents a morphology of flattened powder particles stacked in layers. Nearly equiaxed coarse grains are clearly visible inside a part of the particles, and these parts undergo plastic deformation or very little plastic deformation. The grains at the boundaries of other particles present an elongated morphology, and these structures undergo severe plastic deformation. The relative density of the repair layer blank reaches more than 98.7%, and the average flattening rate of the powder particles is less than 0.
458. Then, an aging treatment is performed, and during the aging treatment, the boundaries of the particles with large deformation are preferentially recrystallized, so that the original particle interfaces form metallurgical bonds. After aging, the relative density of the repair layer is maintained at more than 98.5%, and the strength and thermal conductivity are greatly improved.
2. The high-strength and high-thermal-conductivity copper alloy for a crystallizer substrate repair layer according to claim 1, characterized in that: The conditions of the cold spraying process are as follows: the gas preheating temperature is 540-560° C., the gas pressure is 3.2-3.5 MPa, the powder feeding rate is 220-250 SLM, and the spray gun moving speed is 60-63 mm / s.
3. The high-strength and high-thermal-conductivity copper alloy for a crystallizer substrate repair layer according to claim 1, characterized in that: The aging treatment conditions are as follows: the aging temperature is 590-620° C., the temperature is kept for 1-2 hours, and then the furnace is cooled to room temperature; after cold spraying and aging treatment, the matrix of the high-strength and high-thermal-conductivity copper alloy of the obtained repair layer is an FCC structure, and there are spherical and rod-shaped Cr nano-precipitates and spherical Zr-rich precipitation phases in the crystal, and these dispersed precipitation phases play a strengthening role, and the strength of the obtained repair layer is higher than 430MPa, and the thermal conductivity is higher than 310W / (m·K).
4. The method for preparing a high-strength and high-thermal-conductivity copper alloy for a crystallizer substrate repair layer according to claim 1, characterized in that: The following steps are included (1) Raw material preparation: Prepare Cu, Cr, and Zr raw materials in the required proportions. CuCr and CuZr master alloys with known compositions may also be used. (2) Gas atomization powder making: After the raw materials are weighed, gas atomization powder making is performed to obtain spherical solid solution alloy powder; then air flow classification is performed to screen out spherical powder with a particle size range of -400 / +800 mesh, and the average particle size is 22 to 25 μm; (3) Cold spraying: The screened powder is used to prepare a block by a cold spraying system; the cold spraying gas preheating temperature is 540-560°C, the gas pressure is 3.2-3.5 MPa, the powder feeding rate is 220-250 SLM, and the spray gun moving speed is 60-63 mm / s; the powder is deposited on the substrate, and after cold spraying, a cold sprayed copper alloy repair layer blank is obtained; the blank presents a morphology of flattened powder particles stacked in layers; in some of the particles, approximately equiaxed coarse grains are clearly visible inside, and these parts undergo plastic deformation, or the plastic deformation is very small; while the grains at the boundaries of other particles present an elongated morphology, and these structures undergo severe plastic deformation; the relative density of the repair layer blank reaches 98.7%, and the average flattening rate of the powder particles is less than 0.458; the tensile strength is 170-190 MPa, and the thermal conductivity is 140-160 W / (m·K); (4) Aging treatment: The cold-sprayed copper alloy repair layer blank is heated to 590-620°C in a protective atmosphere, kept at this temperature for 1-2 hours, and then cooled to room temperature in the furnace to obtain the copper alloy repair layer after aging treatment; during the aging treatment, the grain boundaries with large deformation are preferentially recrystallized, so that the original grain interface forms a metallurgical bond, and the relative density of the repair layer after aging is maintained above 98.5%, and the strength and thermal conductivity are greatly improved; the tensile strength is higher than 430 MPa, and the thermal conductivity is higher than 310 W / (m·K); After the cold spraying and aging treatment, the obtained CuCrZr alloy has a matrix of FCC structure, and FCC structured Cr nanophase and Zr-rich nanoalloy phase are dispersed and precipitated in the crystal; this structure enables the alloy to have high strength and excellent thermal conductivity.
Citation Information
Patent Citations
Crystallizer cold spraying integral repairing method and special clamping device for corner processing
CN104372332A
Crystallizer surface repairing method and device
CN116716602A
Mold for continuous casting and method for manufacturing and repairing the same
JP2004306120A
Cited By
Method for recycling and reusing 3D printing substrate at low cost
CN120828136A