Alloy material surface ceramic galvanizing method

By using a ceramic zinc solution for electroplating treatment on the surface of the alloy material, a ceramic-like component is formed, which solves the problems of multiple washing times and poor welding performance in the existing electro-galvanizing process, and achieves higher environmental protection and corrosion resistance.

CN118727072AInactive Publication Date: 2024-10-01乐创机械科技无锡有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411061786.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing electro-galvanizing and hot-dip galvanizing processes require multiple water washings after degreasing, which results in the discharge of harmful chemical wastewater, affects the welding performance, and makes it difficult to effectively improve the corrosion resistance and weldability of alloy materials.

Method used

Ceramic zinc solution is used for electroplating treatment. Ceramic-like components are formed in the pores of the metal surface through ionization plating, changing the oxidation sequence, reducing the number of water washes, and improving corrosion resistance and weldability.

Benefits of technology

It reduces the number of water washings, improves environmental protection, extends the corrosion resistance of zinc by changing the oxidation sequence, and improves the corrosion resistance, impact resistance and welding performance of alloy materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727072A_ABST
    Figure CN118727072A_ABST
Patent Text Reader

Abstract

The invention discloses a method for ceramic zinc plating on the surface of an alloy material. The method comprises the following steps: (a) degreasing: degreasing an alloy part at 60-80 DEG C by adopting a degreasing solution; (b) acid pickling, wherein the degreased alloy part is sequentially subjected to acid pickling, water washing and neutralizing treatment; (c) electrolytic degreasing: carrying out electrolytic degreasing on the product obtained in the step (b) under the conditions of 65 A / dm < 2 >-85 A / dm < 2 > and 60-80 DEG C, and washing with water; (d) electrogalvanizing: placing the alloy part subjected to electrolytic degreasing in a ceramic zinc solution, carrying out electrogalvanizing treatment at the temperature of 20-25 DEG C, and washing with water; (e) activating, namely activating the product obtained in the step (d) in a solution containing trivalent chromate, washing with water, and drying; (f) post-treatment: carrying out passivation post-treatment on the product obtained in the step (e), and drying. And the corrosion resistance, the impact resistance and the weldability can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface treatment and relates to a galvanizing method, in particular to a method for ceramic galvanizing on the surface of an alloy material. Background Art

[0002] Surface treatment is the process of artificially creating a layer on the surface of a base material that has mechanical, physical, and chemical properties different from those of the base material. The purpose of surface treatment is to meet the product's requirements for corrosion resistance, wear resistance, decoration, or other special functions. For metal parts (such as alloys), the most commonly used surface treatment methods include mechanical grinding, chemical treatment, surface heat treatment, and surface spraying.

[0003] Chinese invention patent application number 202410532320.5 discloses a high-strength rivet nut processing method within the field of rivet nut production technology, comprising the following steps: step 1) wire drawing; step 2) cold heading; step 3) thread extrusion; step 4) high-frequency quenching and tempering: the product is heated on a high-frequency heating device, and is advanced while being heated by a track-type induction coil. It is then quenched in the quenching zone, where only the threaded area of ​​the rivet nut is quenched, and the rivet deformation area is not allowed to be quenched; the quenched rivet nut is tempered; step 5) surface treatment; and step 6) full optical inspection. The surface treatment in this application is electroplating zinc / zinc-nickel alloy on the product.

[0004] Chinese invention patent publication number CN102974519A discloses a corrosion protection process for fasteners in marine environments. The process follows the following process flow: workpiece degreasing → rust removal → phosphating or electrogalvanizing surface treatment → spraying → air drying → oven drying → heat preservation. This application utilizes a high-temperature manganese-based phosphating solution for phosphating or electrogalvanizing, and can be used to protect fasteners in marine environments. Chinese invention patent publication number CN116536582A discloses a high-plasticity alloyed hot-dip galvanized Q&P980 steel and its preparation method. The steel's composition, by weight, is as follows: C: 0.20% to 0.24%, Si: 0.6% to 1.8%, Al: 0.015% to 0.8%, Mn: 1.9% to 2.5%, Cr ≤ 0.5%, Mo ≤ 0.3%, P ≤ 0.05%, S ≤ 0.01%, Nb: 0 to 0.04%, Ti: 0 to 0.05%, with the balance being Fe and unavoidable impurities. The preparation method includes smelting, hot rolling, pickling, cold rolling, continuous annealing, and skin-passing. The hot-dip galvanized Q&P980 steel produced using this patent application has a tensile strength exceeding 980 MPa, a yield strength of 650 to 850 MPa, an elongation of 30% or greater, and a hole expansion ratio of 35% or greater. Whether hot-dip galvanizing or electro-galvanizing, multiple water washings are required after degreasing, which will discharge a large amount of wastewater containing harmful chemicals; more importantly, it will affect the welding performance of the product. Summary of the Invention

[0005] The purpose of the present invention is to provide a method for ceramic zinc plating on the surface of an alloy material in order to overcome the deficiencies of the prior art.

[0006] To achieve the above object, the technical solution adopted by the present invention is: a method for ceramic zinc plating on the surface of an alloy material, which comprises the following steps:

[0007] (a) Degreasing: Degreasing the alloy parts with degreasing solution at 60-80℃;

[0008] (b) pickling: the degreased alloy part is sequentially pickled, washed with water and neutralized;

[0009] (c) Electrolytic degreasing: The product obtained in step (b) was heated at 65A / dm 2 ~85A / dm 2 , electrolytic degreasing and water washing at 60-80℃;

[0010] (d) electrogalvanizing: placing the alloy part after electrolytic degreasing in a ceramic zinc solution at a temperature of 20 to 25° C. for electrogalvanizing treatment and then washing with water;

[0011] (e) Activation: The product obtained in step (d) is placed in a solution containing trivalent chromate for activation treatment, washed with water, and dried;

[0012] The ceramic zinc solution comprises the following components in percentage by mass:

[0013]

[0014] The conductive salt is a mixture of sodium citrate, sodium sulfate and o-chlorobenzaldehyde, the main salt is a mixture of sodium benzoate, sodium metabisulfite, acidic acid, chromium sulfate, sodium silicate, sodium nitrate and potassium hydroxide, the anode solvent is a mixture of cobalt nitrate and chromium nitrate, and the acid additive is a mixture of ammonium bifluoride and a brightener.

[0015] Optimally, in step (d), the current density of the electrogalvanizing is 5A / dm 2 ~10A / dm 2 .

[0016] Furthermore, in step (d), the ceramic zinc solution is prepared by mixing water and additives in a mass ratio of 3:7.

[0017] Optimally, in step (d), the buffer is caustic soda.

[0018] Optimally, in step (d), the conductive salt is a mixture of sodium citrate, sodium sulfate and o-chlorobenzaldehyde in a mass ratio of 1:1.5 to 1.6:1.

[0019] Optimally, in step (d), the main salt is a mixture of sodium benzoate, sodium metabisulfite, quercetin, chromium sulfate, sodium silicate, sodium nitrate and potassium hydroxide in a mass ratio of 15-20:10-12:22-25:80-85:220-230:30-35:1.

[0020] Optimally, in step (d), the anode dissolving agent is a mixture of cobalt nitrate and chromium nitrate in a mass ratio of 1:3.3 to 3.6.

[0021] Optimally, in step (d), the acid additive is a mixture of ammonium bifluoride and brightener in a mass ratio of 1:4.0 to 4.2.

[0022] The method of ceramic zinc plating on the surface of alloy materials of the present invention is to electroplate the product in a special ceramic zinc solution after electrolytic degreasing. It can not only reduce the number of water washings and improve environmental protection, but also its principle is to ionize the plated metal to form a ceramic-like component in the pores of the metal surface, which is beneficial to improve corrosion resistance, impact resistance and weldability. This is because the shape The ceramic composition changes the oxidation order of the alloy material: first silicon is oxidized (forming black spots), then zinc is oxidized (forming White rust), and finally iron oxidation (forming red rust), which prolongs the time for zinc to be oxidized . BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The products in Example 1 and Comparative Example 1 were subjected to salt spray tests for different lengths of time;

[0024] Figure 2 The figure is a comparison chart of the product performance in Example 1 and Comparative Examples 1-2. DETAILED DESCRIPTION

[0025] The method for ceramic zinc plating on the surface of an alloy material of the present invention comprises the following steps: (a) degreasing: degreasing the alloy part with a degreasing solution at 60-80°C; (b) pickling: sequentially pickling, water washing and neutralizing the degreased alloy part; (c) electrolytic degreasing: subjecting the product obtained in step (b) to a 65A / dm 2 ~85A / dm 2and electrolytically degreasing at 60-80° C. and washing with water; (d) electrogalvanizing: placing the alloy part after electrolytic degreasing in a ceramic zinc solution at a temperature of 20-25° C. for electrogalvanizing treatment and washing with water; (e) activation: placing the product obtained in step (d) into a solution containing trivalent chromate for activation treatment, washing with water, and drying; the ceramic zinc solution comprises the following components in percentage by weight: 28-30% water; 3.6-4.2% conductive salt; and 37.5-42.5% main salt; The buffer is 1.6-2.4%; the anode dissolver is 12.0-13.0%; the acid additive is 3.0-4.0%; and the zinc solution is 8.5-9.0%. The conductive salt is a mixture of sodium citrate, sodium sulfate, and o-chlorobenzaldehyde; the main salt is a mixture of sodium benzoate, sodium metabisulfite, acidic acid, chromium sulfate, sodium silicate, sodium nitrate, and potassium hydroxide; the anode dissolver is a mixture of cobalt nitrate and chromium nitrate; and the acid additive is a mixture of ammonium bifluoride and a brightener. By electrolytically degreasing the product and then electroplating it in a specially designed ceramic zinc solution, not only does it reduce the number of water washes and improve environmental friendliness, but it also utilizes the principle of ionizing the plated metal to form a ceramic-like component in the pores of the metal surface, which helps improve corrosion resistance, impact resistance, and weldability.

[0026] In step (d), the current density of the electrogalvanizing is 5A / dm 2 ~10A / dm 2 In step (d), the ceramic zinc solution is formed by mixing water and additives in a mass ratio of 3:7. In step (d), the buffering agent is caustic soda. In step (d), the conductive salt is a mixture of sodium citrate, sodium sulfate, and o-chlorobenzaldehyde in a mass ratio of 1:1.5 to 1.6:1. In step (d), the main salt is a mixture of sodium benzoate, sodium metabisulfite, quercetin, chromium sulfate, sodium silicate, sodium nitrate, and potassium hydroxide in a mass ratio of 15-20:10-12:22-25:80-85:220-230:30-35:1. In step (d), the anode dissolving agent is a mixture of cobalt nitrate and chromium nitrate in a mass ratio of 1:3.3 to 3.6. In step (d), the acid additive is a mixture of ammonium bifluoride and brightener in a mass ratio of 1:4.0 to 4.2.

[0027] The preferred embodiments of the present invention will be described in detail below.

[0028] Example 1

[0029] This embodiment provides a method for ceramic galvanizing the surface of an alloy material, wherein the alloy material may be a pipe joint, a communication bracket, a subway platform bracket, etc. (a pipe joint is used as an example in this embodiment, and is about 20 cm long), comprising the following steps:

[0030] (a) Degreasing: Degrease the alloy parts using a degreasing solution (alkaline degreasing agent FKES-2302) at 70°C for 10 minutes (good degreasing can be achieved in the temperature range of 60-80°C, and the treatment time can be 10-30 minutes, which has little effect on product performance);

[0031] (b) Pickling: The degreased alloy parts are sequentially pickled (using conventional pickling solution, with the following formula: 350 ml / L hydrochloric acid, 3 g / L hexamethylenetetramine, 1.5 g / L sodium benzoate, pickling temperature 40°C), rinsed (rinsed with running water at 25°C), and neutralized (using 100 mg / L sodium hydroxide solution at 25°C).

[0032] (c) Electrolytic degreasing: The product obtained in step (b) was subjected to electrolytic degreasing at 70A / dm 2 、70℃ condition (65A / dm 2 ~85A / dm 2 , 60-80 ℃ conditions can achieve good electrolytic degreasing) (electrolytic degreasing can be carried out in an existing conventional electrolytic degreasing solution, the electrolytic degreasing solution specifically comprises: 10g silicate (dry Sheng), 15g caustic soda, 2g sodium metasilicate pentahydrate, 8g sodium gluconate and 90g deionized water), water washing (rinsing with running water, the rinsing water temperature is 25 ℃);

[0033] (d) Electrogalvanizing: The alloy parts after electrolytic degreasing were placed in a ceramic zinc solution for electrogalvanizing at a temperature of 20-25°C (room temperature was used in this embodiment) for 30 minutes, followed by washing with running water at 25°C. The ceramic zinc solution was prepared as follows (the following percentages are by mass; 1 L of the solution can be used):

[0034] Add 30% water; add conductive salts to the water: 1.1% sodium citrate, 1.7% sodium sulfate, 1.1% o-chlorobenzaldehyde, and stir at room temperature for 5 minutes in a blender; add main salts: 1.7% sodium benzoate, 1.1% sodium metabisulfite, 2.3% quercetin, 8.4% chromium sulfate, 22% sodium silicate solution (Xinwang, commercially available), 3.4% sodium nitrate, 0.1% potassium hydroxide, and stir at room temperature for 15 minutes in a blender; add buffer: 2.0% caustic soda; add anode solvent: 2.8% cobalt nitrate, 9.8% chromium nitrate, and stir at room temperature for 8 minutes in a blender; add acid additives: 0.7% ammonium bifluoride, 2.8% brightener (EH-158), and stir at room temperature for 5 minutes in a blender; replenish water: 8.6% zinc solution (cyanide-free zinc plating solution, Beijing Luhang), 0.4% ethylene glycol, and stir at room temperature for 10 minutes in a blender, and control the pH value at 6.8;

[0035] (e) Activation: The product obtained in step (d) was placed in a solution containing trivalent chromate (TN-300) for activation treatment (room temperature, 25 seconds), washed with running water (rinsing water temperature was 25°C), and dried in an oven (80°C).

[0036] Comparative Example 1

[0037] This example provides a method for ceramic galvanizing of an alloy material surface, which is basically the same as that in Example 1, except that step (d) is hot-dip galvanizing: the galvanizing temperature is 450°C and the galvanizing time is 30 seconds (the aluminum content of the zinc solution is 0.02 wt%).

[0038] Comparative Example 2

[0039] This example provides a method for ceramic zinc plating on the surface of an alloy material, which is basically the same as that in Example 1, except that step (d) is electrogalvanizing: refer to step 3 in Example 1 in publication number CN 114214676A.

[0040] Comparative Example 3

[0041] This example provides a method for ceramic zinc plating on the surface of an alloy material, which is basically the same as that in Example 1, except that no main salts are added and a surface coating cannot be obtained.

[0042] The pipe joints in Example 1 and Comparative Example 1 were subjected to a salt spray test (SST). The results are shown in Table 1. Figure 1 (Test standard: ASTM B117, 35°C, 5% NaCl) The product in Example 1 developed slight black rust after 480 hours of SST treatment, but no white rust or red rust developed after 1000 hours. The product in Comparative Example 1 developed white rust and partially red rust after 480 hours of SST treatment.

[0043] The pipe joints in Example 1 and Comparative Examples 1-2 were also tested for performance, and the results are shown in Table 1. Figure 2 As shown, the specific test methods are as follows: corrosion resistance (i.e., the aforementioned salt spray test, SST) is based on ASTM B117; corrosion resistance CCT is based on JIS H8502; pencil hardness is tested according to ASTM D3363-05; adhesion is tested according to ASTM D3359-17; and weldability is tested using the Radiographic Test (RT).

[0044] The above embodiments are only for illustrating the technical concept and features of the present invention. Their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it accordingly. They are not intended to limit the scope of protection of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for ceramic zinc plating on the surface of an alloy material, comprising the following steps: (a) Degreasing: Degreasing the alloy parts with a degreasing solution at 60-80°C; (b) pickling: the degreased alloy part is pickled, washed with water and neutralized in sequence; (c) Electrolytic degreasing: The product obtained in step (b) was heated to 65A / dm 2 ~85A / dm 2 , electrolytic degreasing and water washing at 60-80℃; (d) electrogalvanizing: placing the alloy part after electrolytic degreasing in a ceramic zinc solution at a temperature of 20 to 25° C. for electrogalvanizing treatment and washing with water; (e) Activation: placing the product obtained in step (d) into a solution containing trivalent chromate for activation treatment, washing with water, and drying; Characterized in that the ceramic zinc solution comprises the following components in percentage by mass: The conductive salt is a mixture of sodium citrate, sodium sulfate and o-chlorobenzaldehyde, the main salt is a mixture of sodium benzoate, sodium pyrosulfite, ruticosic acid, chromium sulfate, sodium silicate, sodium nitrate and potassium hydroxide, the anode solvent is a mixture of cobalt nitrate and chromium nitrate, and the acid additive is a mixture of ammonium bifluoride and a brightener.

2. The method for ceramic zinc plating on the surface of an alloy material according to claim 1, characterized in that: In step (d), the current density of the electrogalvanizing is 5A / dm 2 ~10A / dm 2 .

3. The method for ceramic zinc plating on the surface of the alloy material according to claim 1 or 2, characterized in that: In step (d), the ceramic zinc solution is prepared by mixing water and an additive in a mass ratio of 3:

7.

4. The method for ceramic zinc plating on the surface of an alloy material according to claim 1, characterized in that: In step (d), the buffer is caustic soda.

5. The method for ceramic zinc plating on the surface of an alloy material according to claim 1, characterized in that: In step (d), the conductive salt is a mixture of sodium citrate, sodium sulfate and o-chlorobenzaldehyde in a mass ratio of 1:1.5 to 1.6:

1.

6. The method for ceramic zinc plating on the surface of an alloy material according to claim 1, characterized in that: In step (d), the main salt is a mixture of sodium benzoate, sodium metabisulfite, acid, chromium sulfate, sodium silicate, sodium nitrate and potassium hydroxide in a mass ratio of 15-20:10-12:22-25:80-85:220-230:30-35:

1.

7. The method for ceramic zinc plating on the surface of an alloy material according to claim 1, characterized in that: In step (d), the anode dissolving agent is a mixture of cobalt nitrate and chromium nitrate in a mass ratio of 1:3.3-3.

6.

8. The method for ceramic zinc plating on the surface of an alloy material according to claim 1, characterized in that: In step (d), the acid additive is a mixture of ammonium bifluoride and a brightener in a mass ratio of 1:4.0 to 4.2.