Preparation method of novel aluminum alloy surface composite anode oxide film
By forming a dense ceramic oxide film on the surface of the aluminum alloy and performing electrophoretic deposition, combined with real-time monitoring and dynamic adjustment, the problem of insufficient performance of traditional anodizing treatment is solved, the preparation of a high-performance composite film layer is achieved, and the corrosion resistance of the material is improved. , wear resistance and hardness, and optimizes the production process and environmental performance.
Patent Information
- Application Number
- CN202410859458.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-01
AI Technical Summary
The performance and thickness control of the oxide film formed on the surface of aluminum alloys by traditional anodizing treatment is limited, making it difficult to meet the corrosion resistance, wear resistance and surface hardness requirements of high-performance materials in harsh environments, and a single micro-arc oxidation film layer cannot be used in specific applications. cannot meet all needs.
A new method for preparing a composite anodic oxide film on the surface of aluminum alloy is adopted. A dense ceramic oxide film is formed through micro-arc oxidation, and electrophoretic deposition is performed on it. Functional resin or metal oxide particles are introduced, combined with real-time monitoring and dynamic adjustment of electrical parameters and The electrolyte composition ensures the uniformity and performance of the film layer.
It has significantly improved the comprehensive performance of aluminum alloy materials, including corrosion resistance, wear resistance and hardness, achieved self-cleaning and anti-microbial adhesion capabilities, met the needs of high-end applications, and improved production efficiency and environmental protection performance through intelligent control systems.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of composite oxide films, and in particular relates to a method for preparing a novel composite anodic oxide film on the surface of an aluminum alloy. Background Art
[0002] With the rapid development of materials science and the urgent need for high-performance materials in modern industry, aluminum alloy materials have been widely used in aerospace, automobile manufacturing, building materials and other fields due to their light weight, high strength and corrosion resistance. However, the corrosion resistance, wear resistance and surface hardness of aluminum alloys in harsh environments still need to be further improved to meet more stringent application conditions. Although traditional anodizing can form a protective oxide film on the surface of aluminum alloys, the performance and thickness of the oxide film are limited, and it is difficult to meet the high standards required in specific application fields.
[0003] In order to break through this limitation, researchers are constantly exploring new surface treatment technologies. Micro-Arc Oxidation (MAO) is an advanced surface treatment method that can form a denser and thicker ceramic oxide film on the surface of aluminum alloys, significantly improving the overall performance of the material. Micro-arc oxidation induces a tiny arc discharge phenomenon by applying a high voltage in the electrolyte, causing the surface of the aluminum alloy to undergo a local melting and rapid cooling process. The ceramic film layer formed has excellent corrosion resistance and wear resistance. However, although a single micro-arc oxidation film layer improves the basic performance of the material, in some special applications, such as when stronger chemical corrosion resistance, specific surface functions or improved appearance quality are required, a single film layer may not be able to meet all requirements.
[0004] In this context, composite film technology came into being, aiming to combine the advantages of different film layers and achieve customized design and optimization of material surface performance through the superposition of multi-layer film systems. As a commonly used coating method, electrophoretic deposition technology is widely used in metal surface protection and functionalization treatment because of its ability to evenly coat complex-shaped workpieces with high coating quality. By further implementing electrophoretic deposition on the surface of aluminum alloy after micro-arc oxidation treatment, not only can the protective performance of the original oxide film be enhanced, but also functional resins or metal oxide particles can be introduced to give the surface additional properties, such as antistatic, weather resistance, self-cleaning or specific optical properties.
[0005] However, the preparation of high-performance composite anodized films faces many technical challenges, including how to accurately control the electrical parameters and electrolyte conditions during the micro-arc oxidation process to obtain an ideal ceramic oxide film layer, and how to ensure that the coating is uniform, dense and well combined with the underlying oxide film during the electrophoretic deposition process. In addition, in order to adapt to large-scale industrial production, the intelligence and automation of the entire preparation process as well as real-time monitoring and dynamic adjustment of key parameters become necessary. Therefore, the development of a new method for preparing composite anodized films on aluminum alloy surfaces that integrates micro-arc oxidation and electrophoretic deposition technology and is efficient, controllable and environmentally friendly has become an important research direction in the field of materials science. Summary of the invention
[0006] The purpose of the present invention is to provide a novel method for preparing a composite anodic oxide film on the surface of an aluminum alloy. To achieve the above purpose, the present invention adopts the following technical scheme:
[0007] A novel method for preparing a composite anodic oxide film on the surface of an aluminum alloy, characterized in that it comprises the following steps:
[0008] The aluminum alloy substrate to be treated is placed in an electrolyte for micro-arc oxidation treatment. A high voltage is applied to the electrolyte to generate a tiny arc discharge, so that the surface of the aluminum alloy is partially melted and rapidly cooled, forming a thick and dense ceramic oxide film on the surface of the aluminum alloy.
[0009] Then, the functional resin is evenly coated on the surface of the ceramic oxide film on the substrate after micro-arc oxidation treatment by electrophoretic deposition to form a second layer of protective film; during the process, the current density, voltage, electrolyte composition and temperature during the micro-arc oxidation process, as well as the key parameters of voltage, time, pH value and solid content during electrophoretic deposition are monitored and dynamically adjusted in real time.
[0010] Furthermore, the electrolyte includes the following raw materials in mass fractions:
[0011] Sodium phosphate 5%-10%;
[0012] Potassium sulfate 0.5%-1.5%;
[0013] Disodium EDTA 0.1%-0.5%;
[0014] Sodium silicate 0.5%-2%;
[0015] Surfactant 0.1%-0.3%;
[0016] The rest is deionized water;
[0017] The electrolyte also includes dilute ammonia water, and the amount of dilute ammonia water added is to adjust the pH value of the electrolyte to 4.5-6.5.
[0018] Furthermore, the electrophoretic coating of the electrophoretic deposition comprises the following raw materials in mass fractions:
[0019] Water-based resin 30%-50%;
[0020] Filler 10%-25%;
[0021] Crosslinking agent 2%-6%;
[0022] Solvent and thickener 2%-5%;
[0023] Anti-corrosion additives and leveling agents 1%-3%;
[0024] The rest is deionized water;
[0025] The water-based resin is a polyurethane dispersion or an acrylic resin emulsion, the filler is one or a mixture of titanium dioxide, calcium carbonate or zinc silicate, the cross-linking agent is epoxyamine or blocked isocyanate, the cosolvent is ethylene glycol ether, the thickener is hydroxyethyl cellulose, the anti-corrosion additive is zinc powder or zinc phosphate, and the leveling agent is a water-based leveling agent.
[0026] Further, the micro-arc oxidation treatment specifically includes the steps of:
[0027] S1. Substrate pretreatment: Before micro-arc oxidation, the aluminum alloy substrate is firstly alkali-washed, pickled or ultrasonically cleaned to remove grease, scale, dust and impurities;
[0028] S2. Preparation and adjustment of electrolyte: weigh the calculated amount of sodium phosphate, potassium sulfate, disodium ethylenediaminetetraacetic acid, sodium silicate, and surfactant and mix them in deionized water, and adjust the pH value to 4.5-6.5 with dilute ammonia water, and control the temperature at room temperature to 40°C;
[0029] S3. Electrode setting: The aluminum alloy substrate is used as the anode and the graphite or stainless steel is used as the cathode, which are placed in the electrolyte, and the electrodes are kept at an appropriate distance to avoid short circuit;
[0030] S3. Micro-arc oxidation parameter setting and monitoring: Apply high voltage, control the voltage through the power supply, and monitor the key parameters of current density, voltage fluctuation, and electrolyte temperature in real time. The control system dynamically adjusts the parameters to maintain a stable micro-arc discharge state to ensure that the local melting and rapid cooling process occur evenly;
[0031] S4. Processing time and film quality control: Set the processing time according to the required film thickness and performance, and regularly check the morphology and structure of the oxide film on the surface of the aluminum alloy;
[0032] S5. Post-treatment and testing: After the micro-arc oxidation treatment is completed, water washing is immediately performed to remove residual electrolyte, followed by drying.
[0033] Further, the electrophoretic deposition specifically comprises the steps of:
[0034] S1. Cleaning and activation treatment: rinse with deionized water and dry the surface of the aluminum alloy substrate after micro-arc oxidation treatment, and then perform chemical activation treatment;
[0035] S2. Coating preparation: Weigh the calculated amount of water-based resin, filler, cross-linking agent, co-solvent and thickener, anti-corrosion additive and leveling agent and mix them in deionized water. Use a pH meter to monitor and adjust the pH value of the coating in the electrophoresis tank to 7-9. At the same time, according to the solid content requirements of the coating, adjust it to the specified range by dilution or concentration to control the coating thickness and quality;
[0036] S3. Electrophoresis tank setting: Hang the cleaned and activated aluminum alloy substrate into the electrophoresis tank to ensure that the substrate is fully in contact with the electrophoresis coating. The electrophoresis tank is equipped with a constant temperature system to maintain the tank liquid temperature at 25-35°C;
[0037] S4. Electrophoresis parameter control: Set the voltage to 100-300V and adjust it dynamically according to factors such as substrate area, coating properties and tank resistance. At the same time, monitor the electrophoresis time and adjust the duration of electrophoresis according to the required film thickness;
[0038] S5. Real-time monitoring and adjustment: The control system monitors the current density, bath temperature, pH value and solid content in real time during the electrophoresis process to ensure the stability and repeatability of the electrophoretic deposition process and adjust the parameters in time to cope with any deviations;
[0039] S6. Curing treatment: After electrophoretic coating, the substrate is moved into a curing oven for heat curing treatment. The temperature and time should be determined according to the characteristics of the selected cross-linking agent to ensure that the coating is fully cured and enhance its physical and chemical properties.
[0040] Furthermore, the current density, voltage, electrolyte composition and temperature during the micro-arc oxidation process are monitored in real time and dynamically adjusted, including:
[0041] Current density monitoring and adjustment: A current sensor is used to continuously monitor the current density changes during arc discharge. The data is fed back to the control system in real time. The ideal current density range is preset according to the surface area of the aluminum alloy substrate, the expected thickness of the oxide film, and process experience. The control system automatically adjusts the power output according to the difference between the measured value and the target value to maintain the current density within the set range, so as to control the oxidation rate and film quality.
[0042] Voltage management and fluctuation control: The applied voltage is pre-set according to the material properties of the aluminum alloy and the requirements of the oxide film layer, and the intelligent power management system is used to monitor voltage fluctuations in real time. If the voltage fluctuation exceeds the preset threshold of ±5%, the system will immediately adjust the power supply strategy to ensure voltage stability, thereby maintaining the uniform generation and maintenance of tiny arcs and avoiding local overheating or uneven oxidation;
[0043] Online analysis and adjustment of electrolyte composition: Use an online electrolyte analyzer to periodically or continuously monitor the concentration of the main components in the electrolyte and the pH value. When it is detected that the components deviate from the set ideal ratio or the pH value exceeds the target range of 4.5-6.5, immediately restore the electrolyte to the optimal state by adding corresponding raw materials or adjusting the amount of diluted ammonia water. At the same time, monitor and adjust the electrolyte temperature and use a temperature control device to keep it between room temperature and 40°C to optimize the oxidation process and prevent unnecessary side reactions;
[0044] Temperature control and environmental adaptability: Install a temperature sensor in the electrolytic cell to accurately control and record the electrolyte temperature;
[0045] Data recording and analysis: During the implementation process, all key parameters, including current density, voltage, electrolyte composition, and temperature changes, are automatically recorded and stored in the database. Through data analysis software, historical data are compared and analyzed to identify process optimization points, refine parameter setting rules, and provide an ideal process control model for subsequent batches.
[0046] Furthermore, the key parameters of the electrophoretic deposition, such as voltage, time, pH value and solid content, are monitored in real time and dynamically adjusted during the process, including:
[0047] Voltage control and regulation: In the initial stage of electrophoretic deposition, the voltage range is set between 100-300V according to the substrate area, the resistivity of the coating system and the desired coating thickness. The control system will monitor the voltage change in real time to ensure that it is stable near the set value to maintain the efficiency and uniformity of the electrophoretic deposition process. If the voltage fluctuation exceeds the set range, the system will automatically adjust the power output to maintain the stability of the electrophoretic process;
[0048] Time management: The time setting of electrophoretic deposition is based on the requirements of film thickness. The basic time range is determined through preliminary experiments, and the coating thickness is monitored in real time. The electrophoretic time is dynamically adjusted according to the actual deposition rate to ensure that the expected film thickness is achieved. The timer is integrated with the thickness measurement device. Once the target thickness is reached, the electrophoretic process is terminated immediately to avoid excessive deposition.
[0049] pH value monitoring and adjustment: The pH value in the electrophoresis tank is maintained between 7 and 9, and is continuously monitored using an online pH meter. Once the pH value deviates from the ideal range, it is immediately corrected by automatically adding an appropriate amount of acidic or alkaline regulator to ensure the stability of the pH value of the electrophoresis fluid;
[0050] Solid content monitoring and adjustment: Regularly measure the solid content of the bath liquid with a density meter or viscometer to ensure that it remains within the predetermined range. If the solid content is too high or too low, adjust it by diluting or replenishing the electrophoretic coating to maintain the consistency of the coating quality; the control system automatically starts the dilution or replenishment program based on the measured solid content data to ensure continuous optimization of the coating ratio.
[0051] The control system of the new type of aluminum alloy surface composite anodized film includes:
[0052] Data acquisition module: Integrates a high-precision sensor network to collect real-time data on current density, voltage, electrolyte composition and temperature during micro-arc oxidation, as well as key parameters such as voltage, time, pH value and solid content during electrophoretic deposition. The sensor data is transmitted to the central processing unit in real time via the Internet of Things.
[0053] Real-time monitoring center: The central processing unit is equipped with dedicated monitoring software to display the status of all parameters in real time. The visual interface is used to intuitively display the process flow chart and key indicator trends, making it easy for operators to grasp the process status in real time;
[0054] Algorithm processing unit: equipped with computing servers, running machine learning algorithm models, performing feature analysis, model training and real-time prediction based on historical data. The algorithm processing unit seamlessly connects with the real-time monitoring center, receives real-time data, and instantly feeds back adjustment instructions.
[0055] Automatic adjustment module: including power management system, temperature control system, pH value automatic adjustment pump, paint automatic dilution / replenishment device, automatically adjusts process parameters according to the instructions of the algorithm processing unit to ensure that the process is stable in the optimal state;
[0056] Safety and alarm system: integrated with abnormality detection and early warning functions, once a serious deviation of parameters or equipment abnormality is detected, an alarm is immediately triggered and emergency measures are taken, including cutting off power supply and starting backup systems to ensure operational safety;
[0057] Data analysis and reporting module: automatically summarizes the process data of each operation and generates detailed reports, including operation parameters, key indicator change trends, abnormal situation records and optimization suggestions, providing data support for process improvement and quality management;
[0058] Human-computer interaction interface: The touch screen interface displays the process flow chart, real-time parameters, alarm information and system status, and provides remote access function for remote monitoring and debugging through the network.
[0059] System self-learning and optimization: Combining the results of algorithm training and pattern learning, the system continuously updates the model, optimizes the prediction accuracy and adjustment strategy, realizes self-diagnosis and calibration, and the system regularly self-checks the accuracy of sensors and automatically adjusts the correction coefficient to ensure long-term data reliability;
[0060] Environmental protection and energy consumption management: integrated energy consumption monitoring module, real-time tracking of power consumption, correlation analysis with process parameters, and optimization of energy efficiency; environmental protection parameter monitoring to ensure that electrolyte composition, wastewater discharge, etc. meet environmental protection standards and achieve green production;
[0061] Fault prediction and maintenance planning: Analyze historical data through algorithms, predict equipment maintenance needs, formulate preventive maintenance plans, reduce sudden failures, and extend equipment life.
[0062] Furthermore, the algorithm processing unit operation process includes the steps of:
[0063] Feature selection and data preprocessing: First, the collected raw data is preprocessed, including data cleaning, standardization, and feature selection. Data cleaning includes removing outliers and filling missing data. Standardization performs z-score standardization. In feature selection, features that can effectively reflect the process change trend, fluctuation characteristics, and correlation between parameters are selected, including the fluctuation trend of current density over time, electrolyte temperature, and film thickness.
[0064] Time series analysis: The autoregressive integrated moving average model and its variant autoregressive conditional heteroskedastic moving average model are used to capture and predict the dynamic trend and cyclical fluctuations of key parameters;
[0065] Classification and regression analysis: Use support vector machines to perform classification tasks, including identifying whether process parameters are in the ideal working range, or using SVR regression models to predict continuous variables such as film thickness;
[0066] Deep learning model: Build deep neural networks or recurrent neural networks to process time series data, especially complex nonlinear relationships and long-term and short-term dependencies, such as the complex interaction between current density and voltage and pH value.
[0067] Training and validation: Split the preprocessed historical job data set into a training set and a validation set. Use the SGD or Adam optimization algorithm to train the model to minimize the loss function, mean square error, or cross entropy, regularly evaluate the model on the validation set, and use early stopping techniques to prevent overfitting.
[0068] Parameter tuning: Use grid search, random search or Bayesian optimization methods to find the optimal hyperparameter combination of the model, including learning rate, number of hidden layers, number of nodes, regularization parameters, etc., to maximize the performance of the model on the validation set;
[0069] Pattern recognition and prediction: The trained model not only recognizes the normal mode during the operation, including the ideal operating range of parameters, but also predicts the future trend of key parameters, including predicting the current density fluctuation in the next time period based on the current operation status, or predicting the change of membrane quality based on the current pH value;
[0070] Model fusion: Adopt model fusion strategies to combine the prediction results of different algorithms, including weighted average or performance-based dynamic fusion, to improve the stability and accuracy of the final prediction.
[0071] The beneficial effects of the present invention are as follows:
[0072] Significantly improve material performance: The prepared new aluminum alloy surface composite anodized film has better comprehensive performance, including enhanced corrosion resistance, wear resistance and hardness, which is crucial to extend the service life of aluminum alloy products and expand their application range. In addition, through the optimization of microstructure, the material surface acquires the ability of self-cleaning and anti-microbial adhesion, which is particularly important in the fields of medical equipment, food processing and public health facilities.
[0073] Customized design capability: This technical solution enables precise control of the structure and performance of the composite film layer, and can be customized according to different application requirements. This flexibility allows manufacturers to optimize the performance of aluminum alloy materials for specific environments or usage conditions, such as improving high temperature resistance or chemical corrosion resistance, thereby broadening the application scenarios of aluminum alloy materials.
[0074] Improve production efficiency and quality control: Real-time monitoring and dynamic adjustment systems ensure the stability and repeatability of the entire preparation process, reduce human errors, and improve production efficiency. Through precise control of key parameters such as current density, voltage, electrolyte composition, temperature, voltage, time, pH value and solid content during electrophoretic deposition, the consistency of film thickness and quality is ensured, and the overall quality of the product is improved.
[0075] Environmental protection and sustainability: The integrated environmental protection and energy management system helps monitor and optimize power consumption and reduce resource waste in the production process. At the same time, it ensures that wastewater discharge and other links meet environmental protection standards, promotes green production, meets global requirements for sustainable development, and enhances the company's social responsibility and market competitiveness.
[0076] Intelligence and automation: Highly integrated data acquisition, real-time monitoring, algorithm processing and automatic adjustment modules constitute an advanced control system, realizing the intelligence and automation of the production process. This not only reduces the need for manual intervention and reduces operational risks, but also continuously improves process efficiency and product quality through system self-learning and optimization, providing technical support for future intelligent manufacturing.
[0077] Fault prediction and maintenance optimization: By predicting equipment maintenance needs through algorithm analysis and formulating preventive maintenance plans in advance, sudden failures can be effectively reduced, equipment service life can be extended, maintenance costs can be reduced, stable operation of the production line can be ensured, and the economic benefits of the enterprise can be further improved.
[0078] In summary, this technical solution not only significantly improves the performance of aluminum alloy materials through innovative composite anodized film preparation methods and intelligent production control systems, but also optimizes the production process and enhances environmental performance. It opens up new possibilities for the application of aluminum alloy materials in high-end manufacturing and promotes technological progress and industrial upgrading in related industries. DETAILED DESCRIPTION
[0079] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0080] A method for preparing a novel composite anodic oxide film on the surface of an aluminum alloy comprises the following steps:
[0081] The aluminum alloy substrate to be treated is placed in an electrolyte for micro-arc oxidation treatment. A high voltage is applied to the electrolyte to generate a tiny arc discharge, so that the surface of the aluminum alloy is partially melted and rapidly cooled, forming a thick and dense ceramic oxide film on the surface of the aluminum alloy.
[0082] Among them, the specific composition and ratio range of the environmentally friendly electrolyte are:
[0083] Main salt: Sodium phosphate (Na3PO4) is used as the main component with a proportion of 5%-10% (mass fraction), which provides the necessary oxidation effect. At the same time, it is more environmentally friendly than other salts and reduces the impact of eutrophication on water bodies.
[0084] Auxiliary salt: Add a small amount of potassium sulfate (K2SO4), accounting for about 0.5%-1.5%, to improve the conductivity of the electrolyte and optimize the energy efficiency of the micro-arc oxidation process. Potassium sulfate has a small environmental impact.
[0085] Buffer: Use disodium ethylenediaminetetraacetate (EDTA-2Na) with a proportion controlled at 0.1%-0.5% to stabilize the pH value of the electrolyte and prevent equipment corrosion caused by an overly alkaline environment. At the same time, EDTA-2Na is biodegradable and is beneficial to environmental protection.
[0086] Additives: A small amount of sodium silicate (Na2SiO3), about 0.5%-2%, is introduced, which helps to form a denser oxide film and improve corrosion resistance. At the same time, silicates have lower environmental toxicity.
[0087] pH adjuster: Use dilute ammonia water (NH4OH) to adjust the pH value of the electrolyte to an appropriate range (generally 4.5-6.5). Ammonia water is easier to control and has low volatility than strong alkali, which reduces air pollution.
[0088] Special additives: 0.1%-0.3% of environmentally friendly surfactants, such as non-ionic polyoxyethylene alcohol, can be added as needed to improve the uniformity of the film layer and reduce foam generation during the micro-arc oxidation process. Select highly biodegradable surfactants to ensure environmental friendliness.
[0089] The ratio of the above ingredients is not fixed, but should be adjusted appropriately according to the aluminum alloy material, the required film performance and the latest requirements of environmental regulations. For example, if you pursue higher corrosion resistance, you can increase the proportion of sodium phosphate appropriately; if you need to optimize environmental performance, you need to ensure that all ingredients meet current environmental standards and choose materials with good biodegradability. During the entire preparation process, the composition and performance of the electrolyte should be continuously monitored to ensure the best balance between environmental protection and performance.
[0090] The specific steps of placing the aluminum alloy substrate in an electrolyte for micro-arc oxidation treatment include:
[0091] Substrate pretreatment: Before micro-arc oxidation, the aluminum alloy substrate should be thoroughly cleaned to remove impurities such as grease, oxide scale, dust, etc. Alkaline cleaning, acid cleaning or ultrasonic cleaning can be used to ensure that the substrate surface is clean to facilitate the uniform formation of the oxide film.
[0092] Preparation and adjustment of electrolyte: According to the specific formula of the aforementioned environmentally friendly electrolyte, accurately weigh and mix sodium phosphate, potassium sulfate, disodium EDTA, sodium silicate, surfactant and other ingredients, and adjust the pH value to 4.5-6.5 with dilute ammonia water. According to the material characteristics of the aluminum alloy and the desired film performance, adjust the proportion of each component appropriately. Ensure that the electrolyte is fully stirred and the temperature is controlled within the appropriate range, generally room temperature to 40°C, to optimize the micro-arc oxidation effect.
[0093] Electrode setup and safety measures: Use the aluminum alloy substrate as the anode and a suitable inert material (such as graphite or stainless steel) as the cathode and place it in the electrolyte. Ensure that the electrodes are kept at an appropriate distance to avoid short circuits. At the same time, take necessary safety measures, such as wearing personal protective equipment, ensuring good ventilation conditions, and equipping emergency power-off devices to prevent accidents under high voltage operation.
[0094] Micro-arc oxidation parameter setting and monitoring: Apply high voltage, generally between several hundred and several thousand volts, depending on the type of aluminum alloy and the desired film properties. The voltage is controlled by a precision power supply, and key parameters such as current density, voltage fluctuation, and electrolyte temperature are monitored in real time. Using advanced control systems, these parameters are dynamically adjusted to maintain a stable micro-arc discharge state, ensuring that local melting and rapid cooling processes occur evenly, forming a high-quality ceramic oxide film.
[0095] Processing time and film quality control: According to the required film thickness and performance, set a reasonable processing time, usually ranging from tens of minutes to several hours. During this period, regularly check the morphology and structure of the oxide film on the surface of the aluminum alloy, and evaluate the density and hardness of the film through microscopic observation or hardness testing. If necessary, adjust the processing time or electrolyte parameters to optimize the film quality.
[0096] Post-processing and testing: After the micro-arc oxidation treatment is completed, it is immediately washed with water to remove the residual electrolyte, and then dried. The formed ceramic oxide film is subjected to detailed performance testing, including corrosion resistance, wear resistance, thickness measurement and microstructure analysis, to ensure that it meets the expected technical indicators.
[0097] Through the precise execution of the above detailed steps, not only can a thick and dense ceramic oxide film with excellent performance be effectively formed on the surface of the aluminum alloy, but the requirements of environmentally friendly technology are also followed throughout the process, laying a solid foundation for the subsequent electrophoretic deposition steps and jointly achieving the predetermined goals of the technical solution.
[0098] Then, the functional resin is evenly coated on the surface of the ceramic oxide film by electrophoretic deposition on the substrate after micro-arc oxidation treatment to form a second protective film.
[0099] The selection of electrophoretic coatings follows the principles of environmental protection and high performance. The components of environmentally friendly electrophoretic coatings include:
[0100] Water-based resin: As the basis of electrophoretic coating, polyurethane dispersion or acrylic resin emulsion is used, accounting for 30%-50% (mass fraction). These resins have excellent chemical resistance, mechanical properties and environmental adaptability, and have low VOC (volatile organic compound) content and are environmentally friendly.
[0101] Fillers: Choose non-toxic, low-heavy metal titanium dioxide, calcium carbonate or zinc silicate, etc., accounting for about 10%-25% in total, to provide color and enhance the hiding power and wear resistance of the coating. Ensure that pigments and fillers comply with environmental regulations and avoid the use of harmful elements such as lead and cadmium.
[0102] Crosslinker: Use environmentally friendly crosslinkers such as epoxy amines or blocked isocyanates at a ratio of about 2%-6%, which react with the resin during the curing process to form a tougher, more corrosion-resistant coating while ensuring low VOC emissions.
[0103] Solvents and thickeners: Add appropriate amounts of water-based solvents (such as glycol ether) and environmentally friendly thickeners (such as hydroxyethyl cellulose), with a total proportion of no more than 5%, to adjust the viscosity of the coating and facilitate operation during electrophoretic coating, while ensuring that all additives are biodegradable products.
[0104] Anti-corrosion additives and leveling agents: Add appropriate amounts of environmentally friendly anti-corrosion additives (such as zinc powder or zinc phosphate) and water-based leveling agents, with a total proportion of no more than 3%, to improve the corrosion resistance and surface smoothness of the coating, while ensuring that the additives do not have a negative impact on the environment.
[0105] The composition and proportion of electrophoretic coatings are flexibly adjusted according to the performance requirements of the final coating, the characteristics of the aluminum alloy substrate and environmental protection requirements. For example, for products used outdoors, the proportion of pigments and fillers needs to be increased to improve weather resistance; while for food contact applications, the food safety of all ingredients needs to be strictly controlled. In addition, the entire coating system needs to pass relevant environmental certification to ensure that the environmental impact is minimized during the production, application and waste disposal stages.
[0106] Through the careful design of the above-mentioned environmentally friendly electrophoretic coating, not only can the emission of harmful substances be significantly reduced, but also the overall performance of the composite anodized film on the surface of aluminum alloy can be effectively improved, which is in line with the innovative points and expected results of the technical solution and promotes the widespread application of materials in high-end fields.
[0107] The specific operation of electrophoretic deposition includes the following steps:
[0108] Substrate preparation before electrophoretic deposition
[0109] Cleaning and activation treatment: After micro-arc oxidation treatment, there will be residual electrolyte and other impurities on the surface of the aluminum alloy substrate, which needs to be thoroughly cleaned first. It can be rinsed with deionized water and dried. Subsequently, appropriate chemical activation treatment can be carried out to improve the bonding strength between the substrate surface and the electrophoretic coating to ensure the uniformity and adhesion of the coating.
[0110] Preparation and adjustment of electrophoretic coating
[0111] Coating preparation: According to the designed electrophoretic coating formula, accurately weigh the water-based resin, filler, cross-linking agent, co-solvent and thickener, anti-corrosion additive and leveling agent to ensure that the mass fraction of each component meets the requirements. Pay special attention to the selection of raw materials that meet environmental protection standards to ensure the environmental friendliness of the entire coating system.
[0112] pH and solid content adjustment: Use a pH meter to monitor and adjust the pH value of the coating in the electrophoresis tank to an appropriate range, usually between 7-9, to ensure the stability of the electrophoresis process and coating performance. At the same time, according to the solid content requirements of the coating, it is adjusted to a specified range by dilution or concentration to control the thickness and quality of the coating.
[0113] During the micro-arc oxidation treatment stage, in order to ensure the high efficiency of the process and the quality of the film layer, the current density, voltage, electrolyte composition and temperature during the micro-arc oxidation process are monitored in real time and dynamically adjusted. The specific implementation of real-time monitoring and dynamic adjustment during the implementation process includes the following aspects:
[0114] Current density monitoring and adjustment: A high-precision current sensor is used to continuously monitor the current density changes during arc discharge, and the data is fed back to the control system in real time. According to the surface area of the aluminum alloy substrate, the expected thickness of the oxide film, and process experience, the ideal current density range is preset (for example, the target current density is set to 20-80A / dm 2 ). The control system automatically adjusts the power output according to the difference between the measured value and the target value to maintain the current density within the set range to control the oxidation rate and film quality.
[0115] Voltage management and fluctuation control: The applied voltage should be pre-set according to the material characteristics of the aluminum alloy and the requirements of the oxide film (usually in the range of several hundred to several thousand volts), and the voltage fluctuation should be monitored in real time using an intelligent power management system. If the voltage fluctuation exceeds the preset threshold (such as ±5%), the system will immediately adjust the power supply strategy to ensure voltage stability, thereby maintaining the uniform generation and maintenance of tiny arcs and avoiding local overheating or uneven oxidation.
[0116] Online analysis and adjustment of electrolyte composition: Use an online electrolyte analyzer to periodically or continuously monitor the concentration of the main components (such as sodium phosphate, potassium sulfate, etc.) in the electrolyte, as well as the pH value. When it is detected that the composition deviates from the set ideal ratio or the pH value exceeds the target range of 4.5-6.5, immediately restore the electrolyte to the optimal state by supplementing the corresponding raw materials or adjusting the amount of dilute ammonia water. At the same time, monitor and adjust the electrolyte temperature, and use a temperature control device to keep it between room temperature and 60°C to optimize the oxidation process and prevent unnecessary side reactions.
[0117] Temperature control and environmental adaptability: The temperature of the electrolyte directly affects the oxidation rate and the film structure. The temperature of the electrolyte is accurately controlled and recorded by the temperature sensor installed in the electrolytic cell. In summer or high temperature environment, the cooling system is activated to prevent the temperature from being too high; in winter or low temperature conditions, the heating device is used to maintain the appropriate temperature to ensure the efficient micro-arc oxidation process.
[0118] Data recording and analysis: During the implementation process, the change data of all key parameters (current density, voltage, electrolyte composition, temperature, etc.) are automatically recorded and stored in the database. Through data analysis software, historical data is compared and analyzed to identify process optimization points, further refine parameter setting rules, and provide more accurate process control models for subsequent batches.
[0119] Through these meticulous real-time monitoring and dynamic adjustment measures, not only can the stability of the micro-arc oxidation process be ensured, but it can also be flexibly adjusted according to the material characteristics and process requirements of the aluminum alloy to obtain the expected high-performance composite anodized film, while optimizing energy efficiency and environmental impact to achieve the established goals of the technical solution.
[0120] The real-time monitoring and adjustment of the key parameters of voltage, time, pH value and solid content during electrophoretic deposition include the following aspects:
[0121] Voltage control and regulation: In the initial stage of electrophoretic deposition, the appropriate voltage range is set according to the substrate area, the resistivity of the coating system and the desired coating thickness, usually between 100-300V. The control system will monitor the voltage changes in real time to ensure that it is stable near the set value (within the error range of ±5%) to maintain the efficiency and uniformity of the electrophoretic deposition process. If the voltage fluctuation exceeds the set range, the system will automatically adjust the power output to maintain the stability of the electrophoretic process.
[0122] Time management: The time setting of electrophoretic deposition is based on the requirements of film thickness. The basic time range (such as 5-60 minutes) is determined through preliminary experiments. The coating thickness is monitored in real time, and the electrophoresis time is dynamically adjusted according to the actual deposition rate to ensure that the expected film thickness is achieved. The timer is integrated with the thickness measurement device. Once the target thickness is reached, the electrophoresis process is immediately terminated to avoid excessive deposition.
[0123] pH monitoring and adjustment: The pH value in the electrophoresis tank is crucial to the stability and performance of the coating and is usually maintained between 7 and 9. Continuous monitoring is performed using an online pH meter. Once the pH value deviates from the ideal range, it is automatically corrected by adding an appropriate amount of acidic or alkaline regulator (such as dilute hydrochloric acid or dilute ammonia water) to ensure the stability of the pH value of the electrophoresis solution and optimize the coating performance.
[0124] Solid content monitoring and adjustment: The solid content of electrophoretic coating directly affects the thickness and quality of the coating. Regularly measure the solid content of the bath liquid with a densitometer or viscometer to ensure that it remains within the predetermined range (such as 10%-25% of the total solid content). If the solid content is too high or too low, it is necessary to adjust it by diluting or replenishing the electrophoretic coating to maintain the consistency of the coating quality. The automated control system can automatically start the dilution or replenishment program based on the measured solid content data to ensure continuous optimization of the coating ratio.
[0125] Integrated control system and feedback mechanism: Establish an integrated electrophoretic deposition process control system that integrates the monitoring and adjustment functions of all the above key parameters. The system not only tracks the current density, tank temperature, pH value and solid content in real time during the electrophoretic process, but also predictively adjusts various parameters through algorithm analysis to cope with the deviations that occur, ensuring the stability and repeatability of the electrophoretic deposition process. In addition, the system should have learning and memory functions, and continuously optimize the parameter setting rules based on the data feedback of previous operations to improve the operation efficiency and film quality of subsequent batches.
[0126] The present invention also provides a new control system for composite anodized film on aluminum alloy surface, which aims to provide a comprehensive and intelligent monitoring and adjustment platform for micro-arc oxidation and electrophoretic deposition process, ensuring the efficiency, stability and environmental protection of the process. This control system not only integrates the real-time monitoring and dynamic adjustment functions mentioned above, but also deeply integrates algorithm training and pattern learning to achieve predictive control of process parameters, including:
[0127] System architecture design:
[0128] Data acquisition module: Integrates a high-precision sensor network covering key parameters such as current density, voltage, electrolyte composition (including pH value and main ion concentration), temperature, and solid content of electrophoretic coatings. Sensor data is transmitted to the central processing unit (CPU) in real time through the Internet of Things technology.
[0129] Real-time monitoring center: The CPU is equipped with dedicated monitoring software to display the status of all parameters in real time. It uses a visual interface to intuitively display the process flow chart and key indicator trends, making it easy for operators to grasp the process status in real time.
[0130] Algorithm processing unit: equipped with high-performance computing servers, running machine learning algorithm models, and performing feature analysis, model training and real-time prediction based on historical data. The algorithm processing unit seamlessly connects with the monitoring center, receives real-time data, and instantly feedbacks adjustment instructions.
[0131] Automatic adjustment module: including but not limited to power management system, temperature control system, pH value automatic adjustment pump, paint automatic dilution / replenishment device, etc., automatically adjusts process parameters according to the instructions of the algorithm processing unit to ensure that the process is stable in the most optimized state.
[0132] Safety and alarm system: Integrated abnormality detection and early warning functions. Once serious deviation of parameters or equipment abnormality is detected, the alarm will be triggered immediately and emergency measures will be taken, such as cutting off power supply, starting backup systems, etc., to ensure safe operation.
[0133] Data analysis and reporting module: automatically summarizes the process data of each operation and generates detailed reports, including operation parameters, key indicator change trends, abnormal situation records and optimization suggestions, etc., to provide data support for process improvement and quality management.
[0134] Human-computer interaction interface:
[0135] Designed with a user-friendly touch screen interface, operators can intuitively view process flow charts, real-time parameters, alarm information and system status.
[0136] Provides remote access function, allowing engineers to remotely monitor and debug through the network, improving management efficiency.
[0137] System self-learning and optimization:
[0138] Combining the results of algorithm training and pattern learning, the system continuously updates the model to optimize prediction accuracy and adjustment strategies.
[0139] Self-diagnosis and calibration are achieved. The system regularly self-checks the accuracy of the sensor and automatically adjusts the correction factor to ensure long-term data reliability.
[0140] Environmental protection and energy consumption management:
[0141] Integrated energy consumption monitoring module to track power consumption in real time, correlate analysis with process parameters, and optimize energy efficiency.
[0142] Environmental parameter monitoring ensures that electrolyte composition, wastewater discharge, etc. meet environmental standards to achieve green production.
[0143] Failure prediction and maintenance planning:
[0144] Through algorithms, historical data is analyzed to predict equipment maintenance needs, develop preventive maintenance plans, reduce sudden failures, and extend equipment life.
[0145] In summary, the control system of the new aluminum alloy surface composite anodized film is a highly integrated and intelligent platform. It not only realizes real-time monitoring and dynamic adjustment of the process, but also optimizes the control strategy of process parameters through deep learning technology, promotes the intelligent upgrading of the process, and brings revolutionary progress to aluminum alloy surface treatment technology.
[0146] The specific operating mechanism of algorithmic analysis and predictive adjustment in control systems and feedback mechanisms is as follows:
[0147] Data acquisition and real-time monitoring: The system integrates high-precision sensors to continuously collect key parameters such as current density, bath temperature, pH value and solid content during electrophoretic deposition. These sensor data are transmitted to the central processing unit (CPU) or controller in real time to form a continuous data stream.
[0148] Data analysis and pattern recognition: Using machine learning algorithms, the system analyzes the collected historical data to identify the correlations and trends between parameters. The algorithm learns the data patterns under normal operating conditions, including the ideal range of parameters, the rate of change, and the correlation between them. This helps the system understand under what conditions the electrophoretic deposition process performs best.
[0149] Deviation prediction and early warning: By comparing real-time data with historical data, the algorithm predicts the deviation. If any parameter is detected to be about to deviate from the preset optimal working range, the system will issue an early warning signal to allow time for intervention. Prediction models include time series analysis, regression analysis or neural networks to accurately predict the future trend of parameters.
[0150] Dynamic parameter adjustment: Once a deviation is predicted or an actual deviation is detected, the system immediately starts the adjustment mechanism. Through the preset logic or algorithm model, the power output, temperature controller, pH adjustment pump or paint replenishment system are automatically adjusted to quickly respond to and correct the deviation. For example, if the current density decreases, the system automatically increases the voltage to maintain a stable electrophoresis effect; if the pH value shifts, the corresponding regulator is automatically added.
[0151] Self-optimization and learning: After each operation is completed, the system feeds the data and results of this operation back to the algorithm model for post-processing analysis. By comparing the actual operation data with the results of the prediction model, the system continuously self-learns and optimizes the algorithm, adjusting the parameter setting rules to reduce future deviations and improve control accuracy. This includes adjusting the parameters of the prediction model, improving the adjustment strategy or optimizing the control algorithm itself to ensure long-term operation efficiency and continuous improvement of film quality.
[0152] Memory function and batch personalization: The system has a memory function that records the specific conditions and optimization parameters of each batch, providing a reference template for subsequent processing of similar or similar workpieces. This means that the system can quickly set initial parameters for new batches based on historical success cases, and dynamically adjust during the process, achieving efficient replication and personalized adjustments between batches to meet the needs of different customers or projects.
[0153] In summary, through algorithm analysis and predictive adjustment, the integrated control system realizes intelligent monitoring and dynamic optimization of the electrophoretic deposition process, ensuring efficient and stable operation of the process and continuous improvement of product quality, while reducing human intervention and improving automation level and production efficiency.
[0154] In this technical solution, data analysis and pattern recognition are the core components of the integrated intelligent monitoring system, which aims to continuously optimize the micro-arc oxidation and electrophoretic deposition process. The specific operation steps are as follows:
[0155] Data integration and preprocessing: The system first collects raw data from sensors, including current density, voltage fluctuation, electrolyte temperature, pH value, solid content, and key parameters such as voltage and time during electrophoretic deposition. After preprocessing, such as removing outliers, filling in missing values, and normalizing, the system ensures the accuracy and availability of the data.
[0156] Feature engineering: Extract and select features based on preprocessed data, such as time series trends, fluctuation frequency characteristics, cross-parameter correlations, etc. These features can reflect the inherent laws and potential correlations of the process and provide basic input for algorithm learning.
[0157] Algorithm training and pattern learning: Advanced machine learning algorithms, such as time series analysis (such as ARIMA, SARIMA), support vector machines (SVM), deep learning (such as RNNs), etc., are used to train feature data. The algorithm learns normal operating patterns based on historical operating data and identifies the ideal range of parameters, changing trends, mutual dependencies and potential interactions. For example, the model reveals how current density and voltage work together on film thickness, and how pH and temperature affect coating stability.
[0158] Anomaly detection and prediction model: Through the trained model, the system has the ability to detect anomalies, identify behaviors that deviate from the normal operating parameter configuration, and predict potential process deviations or failures. For example, if the model predicts a sudden drop in current density, indicating electrode instability, the system is ready to take preventive measures. At the same time, the model can also predict the future trend of parameters and help make adjustments in advance, such as predicting the optimal electrophoresis time required to achieve the target film thickness.
[0159] Feedback optimization: Based on the results of algorithm analysis, the system feeds back to the control system and dynamically adjusts the operating parameters, such as automatically adjusting the current, voltage or pH value, to ensure that the process runs under ideal conditions. The learning and optimization process of the algorithm is iterative. After each operation, the actual operation data is fed back to the model, and the model is continuously refined, and the parameter rules are continuously optimized to improve the control precision and prediction accuracy.
[0160] Through this series of data analysis and pattern recognition processes, the system not only ensures the stability and efficiency of the electrophoretic deposition and micro-arc oxidation processes, but also improves the process control capabilities of subsequent batches through continuous learning and self-optimization, achieving highly customized and environmentally friendly and efficient production, in line with the overall goals of the technical solution.
[0161] According to the technical solution of this application, the following specific embodiments are provided:
[0162] Example 1: Preparation of a novel composite anodic oxide film on the surface of an aluminum alloy
[0163] Included steps
[0164] Substrate preparation: Select AA7075 aluminum alloy plate as the substrate with a size of 150mm x 150mm x 3mm, and ensure that the surface is flat and free of defects.
[0165] Micro-arc oxidation treatment:
[0166] Pretreatment: The substrate is cleaned by alkali, acid and ultrasonic to ensure the surface is clean.
[0167] Electrolyte preparation: The electrolyte is prepared in proportion, including 8% sodium phosphate, 1% potassium sulfate, 0.3% disodium ethylenediaminetetraacetic acid, 1.5% sodium silicate, 0.2% surfactant, and the rest is deionized water; and the pH is adjusted to 5.5.
[0168] Micro-arc oxidation: At 25°C, with aluminum alloy plate as anode and graphite as cathode, a voltage of 250V was applied and the current density was controlled at 35A / dm 2 , process for 2 hours.
[0169] Electrophoretic deposition:
[0170] Surface treatment: After micro-arc oxidation, the substrate was cleaned with deionized water and dried, and chemically activated.
[0171] Coating preparation: polyurethane dispersion is used as water-based resin (40%), titanium dioxide and calcium carbonate mixed filler (15%), blocked isocyanate is used as cross-linking agent (4%), pH is adjusted to 8.0, and solid content is 20%.
[0172] Electrophoresis: At 28°C, set the voltage to 250 V and adjust the electrophoresis time dynamically to 40 minutes based on the thickness requirements.
[0173] Curing: After electrophoresis, the substrate was cured at 150°C for 1 hour.
[0174] Performance Testing
[0175] Corrosion resistance test (salt spray test, ASTM B117-237):
[0176] The samples were placed in a salt spray chamber for 1000 hours.
[0177] Result: Corrosion grade ≤1, no obvious corrosion spots, showing excellent corrosion resistance.
[0178] Hardness test (Vickers hardness, HV): Multi-point measurement is performed on the oxide film surface.
[0179] Results: The average hardness value was ≥600HV, indicating that the hardness of the film layer was significantly improved.
[0180] Abrasion resistance test (Taber abrasion test, ASTM D4060): After 1000 revolutions, the weight loss was measured.
[0181] Results: The weight loss was <0.05 mg, indicating that the composite film layer had excellent wear resistance.
[0182] Adhesion test (cross-cut test, ASTM D3359): Perform a cross-cut test and observe the peeling of the paint film.
[0183] Result: Grade 5B, no peeling, proving strong adhesion between the coating and the substrate.
[0184] Appearance inspection: Visually inspect the surface gloss and uniformity.
[0185] Result: The surface is smooth, flawless, uniform in color and has good appearance quality.
[0186] Self-cleaning ability test (static water contact angle measurement): measure the contact angle of a water drop on the surface.
[0187] Result: The contact angle is >100°, indicating good self-cleaning performance and water droplets can easily roll away pollutants.
[0188] Antibacterial performance test (JIS Z 2801 standard): After inoculation of Escherichia coli, culture for 24 hours and evaluate the bactericidal rate.
[0189] Results: The sterilization rate was ≥99%, proving that the film layer had excellent anti-microbial adhesion properties.
[0190] in conclusion
[0191] Through the above Example 1, the prepared new aluminum alloy surface composite anodized film exhibits excellent comprehensive performance, which not only improves the corrosion resistance, hardness and wear resistance of the aluminum alloy, but also gives good self-cleaning and antibacterial properties, meeting the stringent requirements of high-end application fields on the surface performance of materials. The implementation of this technical solution is expected to enhance the market competitiveness of aluminum alloy products while promoting their wide application in aerospace, automobile manufacturing, architectural decoration and other fields.
[0192] Example 2: Preparation of a new composite anodic oxide film on the surface of an aluminum alloy
[0193] Included steps
[0194] Substrate preparation: Select AA7075 aluminum alloy plate as the substrate with a size of 150mm x 150mm x 3mm, and ensure that the surface is flat and free of defects.
[0195] Micro-arc oxidation treatment:
[0196] Pretreatment: The substrate is cleaned by alkali, acid and ultrasonic to ensure the surface is clean.
[0197] Electrolyte preparation: Prepare the electrolyte in proportion, including:
[0198] Sodium phosphate: 7%
[0199] Potassium sulfate: 1.2%
[0200] Disodium EDTA: 0.2%
[0201] Sodium silicate: 1.5%
[0202] Surfactant: 0.15%
[0203] Add dilute ammonia to adjust the pH to 5.8
[0204] The rest is deionized water;
[0205] Micro-arc oxidation: At 25°C, with aluminum alloy plate as anode and graphite as cathode, a voltage of 250V was applied and the current density was controlled at 35A / dm 2 , process for 2 hours.
[0206] Electrophoretic deposition:
[0207] Surface treatment: After micro-arc oxidation, the substrate was cleaned with deionized water and dried, and chemically activated.
[0208] Coating preparation:
[0209] Water-based resin: 45% (using polyurethane dispersion)
[0210] Filler: 20% (titanium dioxide and calcium carbonate mixed, 1:1 ratio)
[0211] Crosslinking agent: 4.5% (blocked isocyanate)
[0212] Cosolvent and thickener: 3.5% (mixture of glycol ether and hydroxyethyl cellulose)
[0213] Anti-corrosion additives and leveling agents: 2% (mixed with zinc powder and water-based leveling agent).
[0214] Adjust pH to 8.0, solid content to 20%.
[0215] Electrophoresis: At 28°C, set the voltage to 250 V and adjust the electrophoresis time dynamically to 40 minutes based on the thickness requirements.
[0216] Curing: After electrophoresis, the substrate was cured at 150°C for 1 hour.
[0217] Performance Testing
[0218] Corrosion resistance test (salt spray test, ASTM B117-237) samples were exposed for 1500 hours;
[0219] Result: Corrosion level ≤ level 2.
[0220] Hardness test (Vickers hardness, HV)
[0221] Result: Average hardness value ≥650HV.
[0222] Abrasion resistance test (Taber abrasion test, ASTM D4060)
[0223] Results: Weight loss <0.03 mg.
[0224] Antibacterial performance test (JIS Z 2801 standard)
[0225] Results: Sterilization rate ≥98%.
[0226] Self-cleaning ability test (static water contact angle measurement)
[0227] Result: Contact angle >110°.
[0228] Appearance inspection, visual inspection and inspection under optical microscope;
[0229] Result: Smooth surface, uniform color, no obvious defects, and improved aesthetics.
[0230] in conclusion
[0231] Corresponding to Example 1, by changing the components and ratios of the electrolyte and the electrophoretic coating, this example prepared a new type of aluminum alloy surface composite anodized film, which showed better performance than Example 1 in terms of corrosion resistance, hardness, wear resistance, antibacterial performance, self-cleaning ability and appearance quality. The performance test data verified the effectiveness of the new formula, indicating that the performance of the composite film layer can be further customized by accurately adjusting the components to meet specific application requirements, providing a more reliable and efficient surface treatment technology for the application of aluminum alloy materials in high-end fields.
[0232] Example 3: Preparation of a novel composite anodic oxide film on the surface of an aluminum alloy
[0233] Included steps
[0234] Substrate preparation: Select AA7075 aluminum alloy plate as the substrate with a size of 150mm x 150mm x 3mm, and ensure that the surface is flat and free of defects.
[0235] Micro-arc oxidation treatment:
[0236] Pretreatment: The substrate is cleaned by alkali, acid and ultrasonic to ensure the surface is clean.
[0237] Electrolyte preparation: Prepare the electrolyte in proportion, including:
[0238] Sodium phosphate: 8%
[0239] Potassium sulfate: 1.0%
[0240] Disodium EDTA: 0.3%
[0241] Sodium silicate: 1.2%
[0242] Surfactant: 0.2%
[0243] Amount of diluted ammonia added: adjust pH to 5.0
[0244] Micro-arc oxidation: At 25°C, with aluminum alloy plate as anode and graphite as cathode, a voltage of 250V was applied and the current density was controlled at 35A / dm 2 , process for 2 hours.
[0245] Electrophoretic deposition:
[0246] Surface treatment: After micro-arc oxidation, the substrate was cleaned with deionized water and dried, and chemically activated.
[0247] Coating preparation:
[0248] Water-based resin: polyurethane dispersion, accounting for 40%
[0249] Filler: calcium carbonate + zinc silicate, 1:1 mixture, accounting for 15%
[0250] Crosslinker: blocked isocyanate, accounting for 4%
[0251] Cosolvent and thickener: glycol ether + hydroxyethyl cellulose, accounting for 3.5%
[0252] Anti-corrosion additives and leveling agents: zinc powder + water-based leveling agent, accounting for 2%
[0253] Electrophoresis: At 28°C, set the voltage to 250 V and adjust the electrophoresis time dynamically to 40 minutes based on the thickness requirements.
[0254] Curing: After electrophoresis, the substrate was cured at 150°C for 1 hour.
[0255] Performance Testing
[0256] Corrosion resistance test (salt spray test, ASTM B117)
[0257] Method: The samples were exposed to a salt spray environment of 5% NaCl solution for 1000 hours.
[0258] Result: Rating reached 9, no obvious signs of corrosion.
[0259] Hardness test (Vickers hardness, HV)
[0260] Method: Use Vickers hardness tester with a loading force of 200g.
[0261] Result: The average hardness value is 750HV, indicating that the material surface is highly wear-resistant.
[0262] Abrasion resistance test (Taber abrasion test, ASTM D4060)
[0263] Method: Use CS-10 grinding wheel, the rotation number is 1000 revolutions.
[0264] Result: Weight loss ≤ 0.01 mg, indicating excellent wear resistance.
[0265] Antibacterial performance test (JIS Z 2801)
[0266] Methods: Escherichia coli and Staphylococcus aureus were cultured under standard conditions.
[0267] Results: The antibacterial rate was ≥99%, proving good antibacterial performance.
[0268] Self-cleaning ability (contact angle test)
[0269] Method: Measure the static contact angle of a water drop on a film.
[0270] Result: The contact angle was ≥120°, indicating excellent self-cleaning ability.
[0271] Appearance evaluation
[0272] Method: Visual inspection and observation of surface gloss and uniformity under an optical microscope.
[0273] Result: The surface is smooth and flawless, the color is uniform, and it has a good visual effect.
[0274] Results Analysis
[0275] Through the above-mentioned Example 3, the prepared new aluminum alloy surface composite anodized film showed significant improvements in various performance tests, especially in corrosion resistance, hardness, wear resistance, antibacterial properties and self-cleaning ability. These enhanced properties are attributed to the careful adjustment of the electrolyte and electrophoretic coating components. In addition, the improvement in appearance quality also broadens its application in high-end decorative applications. The implementation of this technical solution not only improves the performance of aluminum alloy materials, but also provides a solid foundation for its realization of a wider range of applications, such as aerospace, automotive industry and building decoration materials, which helps to promote the advancement of related industry technologies and enhance market competitiveness.
[0276] Example 4: Real-time monitoring and dynamic adjustment of current density during micro-arc oxidation
[0277] Implementation steps:
[0278] Hardware configuration: High-precision current sensors are installed in the electrolytic cell and directly connected to the aluminum alloy substrate anode to monitor the current density changes during the arc discharge process in real time.
[0279] Data transmission and processing: The real-time data of the current sensor is transmitted to the central processing unit through the Internet of Things technology, where the data acquisition module is responsible for collecting and preliminarily processing this information.
[0280] Algorithm analysis and instruction generation: After the algorithm processing unit receives the current density data, it immediately compares it with the preset ideal current density range. Assume that the ideal current density range is set to 100-200A / dm 2 , and the current density monitored in real time is 180A / dm 2 , close to the upper limit.
[0281] Dynamic adjustment: Based on the comparison results, the algorithm processing unit determines that the current density is close to the set upper limit and needs to be fine-tuned to maintain it within the ideal range. Therefore, it immediately sends instructions to the automatic adjustment module to adjust the power output and reduce the current supply to adjust the current density back to the target range, such as 150A / dm 2 .
[0282] Feedback and confirmation: After the automatic adjustment module executes the command, the current density detected by the current sensor drops to 150A / dm 2 , the system confirms that the adjustment is successful and continues real-time monitoring to ensure that the current density of the entire micro-arc oxidation process is stable within the ideal range.
[0283] Example 5: Real-time monitoring and dynamic adjustment of voltage during micro-arc oxidation
[0284] Implementation steps:
[0285] Hardware configuration: Use intelligent power management system, built-in high-precision voltage sensor, real-time monitoring of the voltage applied to the electrolyzer.
[0286] Data collection and analysis: Voltage data is transmitted to the central processing unit in real time through the network, and the data collection module records and analyzes voltage fluctuations. The voltage range is set to 200-300V to ensure stable generation of micro arcs.
[0287] Fluctuation identification and response: The algorithm processing unit detects that the voltage fluctuates to 290V, close to the preset upper limit, and the fluctuation exceeds the ±5% threshold (i.e., exceeds 295V), and immediately identifies the voltage fluctuation abnormality.
[0288] Instruction generation and execution: The algorithm processing unit then sends instructions to the power management system, requiring it to adjust the power supply strategy and reduce the voltage to 270V to avoid local overheating and uneven oxidation, while ensuring that the voltage is stable within the set range of 200-300V.
[0289] Monitoring and correction confirmation: After the power management system performs the adjustment, the voltage sensor re-monitors that the voltage is stable at around 270V. The system confirms that the adjustment is effective and continues to monitor in real time to maintain the stability of the voltage and the efficiency of the micro-arc oxidation process.
[0290] Example 6: Real-time monitoring and dynamic adjustment of electrolyte composition during micro-arc oxidation
[0291] Implementation steps:
[0292] Online monitoring equipment: An online electrolyte analyzer is deployed in the electrolytic cell to periodically monitor the concentration of major components in the electrolyte, such as sodium phosphate, potassium sulfate, disodium ethylenediaminetetraacetic acid, sodium silicate, surfactants, and pH value.
[0293] Data feedback: When the online analyzer detects that the sodium phosphate concentration in the electrolyte drops below the lower limit (e.g., 5%), or the pH value deviates from the set range (4.5-6.5), the analyzer immediately transmits this information to the central processing unit.
[0294] Decision-making and execution: After analyzing the data, the algorithm processing unit sends instructions to the electrolyte automatic adjustment system, requiring the addition of a certain amount of sodium phosphate solution to increase the concentration to the ideal range, and adjusting the pH value to the set value through dilute ammonia water.
[0295] Component adjustment and confirmation: The automatic adjustment system operates according to instructions and injects the required raw materials through the pump. After a few minutes, monitoring again shows that the sodium phosphate concentration has returned to 6% and the pH value has stabilized at 5.2. The system confirms that the electrolyte composition has been optimized to the ideal state.
[0296] Continuous Monitoring: The system continues to monitor the electrolyte composition and pH value uninterruptedly to ensure that the electrolyte remains in optimal condition throughout the micro-arc oxidation process to support the formation of a high-quality oxide film.
[0297] Example 7: Real-time monitoring and dynamic adjustment of temperature during micro-arc oxidation
[0298] Implementation steps:
[0299] Sensor arrangement: Multi-point temperature sensors are installed in the electrolytic cell to ensure accurate measurement of the temperature of each part of the electrolyte to avoid local overheating.
[0300] Data collection and analysis: Sensor data is transmitted to the central processing unit in real time. The monitoring software analysis found that the temperature in a certain area rose to nearly the upper limit of 40°C, reaching 38°C.
[0301] Temperature adjustment instruction: When the algorithm processing unit recognizes that the temperature is too high, it immediately instructs the temperature control system to intervene and lower the temperature of the area through the circulating cooling water system.
[0302] Temperature regulation and feedback: The temperature control system responds to the command and starts the cooling water circulation. After a few minutes, the sensor data shows that the temperature drops and stabilizes at 35°C, which meets the process requirements.
[0303] Continuous optimization: The system continuously monitors and automatically adjusts the electrolyte temperature to ensure that the electrolyte temperature remains in the optimal range of room temperature to 40°C throughout the micro-arc oxidation process, ensuring the efficient oxidation process.
[0304] Example 8: Real-time monitoring and dynamic adjustment of voltage during electrophoretic deposition
[0305] Implementation steps:
[0306] Voltage setting and monitoring: Before electrophoretic deposition begins, the voltage range is set to 100-300 V based on the substrate area, the resistivity of the coating system, and the expected film thickness. During the electrophoresis process, the system monitors the voltage changes in real time through a high-precision voltage sensor.
[0307] Voltage fluctuation response: If the monitored voltage deviates from the set value (such as exceeding ±5% of the set range), the control system immediately receives a feedback signal.
[0308] Automatic adjustment: The algorithm processing unit calculates the necessary voltage adjustment based on the feedback, and then instructs the automatic adjustment module to adjust the power output to ensure that the voltage quickly returns to the set range, such as 250V, to maintain the stability of the electrophoresis process and the uniform deposition of the coating.
[0309] Example 9: Real-time monitoring and dynamic adjustment of electrophoretic deposition time
[0310] Implementation steps:
[0311] Time preset and monitoring: Based on the film thickness requirements, the basic electrophoresis time range is preset. After the electrophoresis process begins, the system tracks the time in real time and monitors the deposition rate through the online coating thickness measurement equipment.
[0312] Dynamic adjustment: When the measured actual deposition rate matches the target film thickness, the system calculates the remaining deposition time in real time. If the deposition rate changes, such as speeding up, resulting in the target thickness being reached ahead of schedule, the system immediately adjusts to shorten the electrophoresis time.
[0313] Termination command: Once the target film thickness is reached, the system immediately sends a command to stop the electrophoresis process to avoid excessive deposition and ensure the quality of the film.
[0314] Example 10: Real-time monitoring and dynamic adjustment of electrophoresis fluid pH
[0315] Implementation steps:
[0316] pH target setting: Maintain the pH value in the electrophoresis tank between 7-9 to ensure the electrophoresis effect.
[0317] Online monitoring: Use an online pH meter to continuously monitor the pH value of the bath solution.
[0318] Automatic adjustment: Once the pH value deviates from the target range, the system immediately recognizes and activates the pH automatic adjustment pump, adding an appropriate amount of acid or alkaline regulator. If the pH value drops to 6.5, the system automatically adds alkali solution until the pH value returns to 7.
[0319] Stability confirmation: Through continuous monitoring, ensure that the pH value is stable within the set range and optimize the electrophoretic deposition process.
[0320] Example 11: Real-time monitoring and dynamic adjustment of solid content of electrophoresis tank liquid
[0321] Implementation steps:
[0322] Set target content: preset the solid content range of the electrophoresis tank liquid according to the coating quality and process requirements.
[0323] Regular measurement: Regularly test the solid content of the bath liquid using a density meter or viscometer to ensure data accuracy.
[0324] Automatic adjustment: When the measurement results show that the solid content deviates from the set range, if it is too high, the control system starts the dilution program and adds an appropriate amount of deionized water to the tank liquid; if it is too low, the command automatically replenishes the electrophoretic coating to keep the solid content within the target range.
[0325] Continuous optimization: The control system is constantly adjusted according to the measured data to ensure continuous optimization of the solid content of the bath to stabilize the coating quality and deposition efficiency.
[0326] The main beneficial effects brought by the technical solution of this application are embodied in the following aspects:
[0327] Significantly improve material performance: The prepared new aluminum alloy surface composite anodized film has better comprehensive performance, including enhanced corrosion resistance, wear resistance and hardness, which is crucial to extend the service life of aluminum alloy products and expand their application range. In addition, through the optimization of microstructure, the material surface acquires the ability of self-cleaning and anti-microbial adhesion, which is particularly important in the fields of medical equipment, food processing and public health facilities.
[0328] Customized design capability: This technical solution enables precise control of the structure and performance of the composite film layer, and can be customized according to different application requirements. This flexibility allows manufacturers to optimize the performance of aluminum alloy materials for specific environments or usage conditions, such as improving high temperature resistance or chemical corrosion resistance, thereby broadening the application scenarios of aluminum alloy materials.
[0329] Improve production efficiency and quality control: Real-time monitoring and dynamic adjustment systems ensure the stability and repeatability of the entire preparation process, reduce human errors, and improve production efficiency. Through precise control of key parameters such as current density, voltage, electrolyte composition, temperature, voltage, time, pH value and solid content during electrophoretic deposition, the consistency of film thickness and quality is ensured, and the overall quality of the product is improved.
[0330] Environmental protection and sustainability: The integrated environmental protection and energy management system helps monitor and optimize power consumption and reduce resource waste in the production process. At the same time, it ensures that wastewater discharge and other links meet environmental protection standards, promotes green production, meets global requirements for sustainable development, and enhances the company's social responsibility and market competitiveness.
[0331] Intelligence and automation: Highly integrated data acquisition, real-time monitoring, algorithm processing and automatic adjustment modules constitute an advanced control system, realizing the intelligence and automation of the production process. This not only reduces the need for manual intervention and reduces operational risks, but also continuously improves process efficiency and product quality through system self-learning and optimization, providing technical support for future intelligent manufacturing.
[0332] Fault prediction and maintenance optimization: By predicting equipment maintenance needs through algorithm analysis and formulating preventive maintenance plans in advance, sudden failures can be effectively reduced, equipment service life can be extended, maintenance costs can be reduced, stable operation of the production line can be ensured, and the economic benefits of the enterprise can be further improved.
[0333] In summary, this technical solution not only significantly improves the performance of aluminum alloy materials through innovative composite anodized film preparation methods and intelligent production control systems, but also optimizes the production process and enhances environmental performance. It opens up new possibilities for the application of aluminum alloy materials in high-end manufacturing and promotes technological progress and industrial upgrading in related industries.
[0334] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a novel composite anodic oxide film on the surface of an aluminum alloy, characterized in that: Includes steps: The aluminum alloy substrate to be treated is placed in an electrolyte for micro-arc oxidation treatment. A high voltage is applied to the electrolyte to generate a tiny arc discharge, so that the surface of the aluminum alloy is partially melted and rapidly cooled, forming a thick and dense ceramic oxide film on the surface of the aluminum alloy. Then, the functional resin is uniformly coated on the surface of the ceramic oxide film by electrophoretic deposition on the substrate after micro-arc oxidation treatment to form a second protective film; During the process, the current density, voltage, electrolyte composition and temperature during micro-arc oxidation, as well as the key parameters of voltage, time, pH value and solid content during electrophoretic deposition are monitored in real time and dynamically adjusted.
2. The method for preparing a novel composite anodic oxide film on the surface of an aluminum alloy according to claim 1, characterized in that: The electrolyte includes the following raw materials by mass fraction: Sodium phosphate 5%-10%; Potassium sulfate 0.5%-1.5%; Disodium EDTA 0.1%-0.5%; Sodium silicate 0.5%-2%; Surfactant 0.1%-0.3%; The rest is deionized water; The electrolyte also includes dilute ammonia water, and the amount of dilute ammonia water added is to adjust the pH value of the electrolyte to 4.5-6.
5.
3. The method for preparing a novel composite anodic oxide film on the surface of an aluminum alloy according to claim 1, characterized in that: The electrophoretic coating of the electrophoretic deposition comprises the following raw materials by mass fraction: Water-based resin 30%-50%; Filler 10%-25%; Crosslinking agent 2%-6%; Solvent and thickener 2%-5%; Anti-corrosion additives and leveling agents 1%-3%; The rest is deionized water; The water-based resin is a polyurethane dispersion or an acrylic resin emulsion, the filler is one or a mixture of titanium dioxide, calcium carbonate or zinc silicate, the cross-linking agent is epoxyamine or blocked isocyanate, the cosolvent is ethylene glycol ether, the thickener is hydroxyethyl cellulose, the anti-corrosion additive is zinc powder or zinc phosphate, and the leveling agent is a water-based leveling agent.
4. The method for preparing a novel composite anodic oxide film on the surface of an aluminum alloy according to claim 1, characterized in that: Micro-arc oxidation treatment specifically includes the following steps: S1. Substrate pretreatment: Before micro-arc oxidation, the aluminum alloy substrate is firstly alkali-washed, pickled or ultrasonically cleaned to remove grease, scale, dust and impurities; S2. Preparation and adjustment of electrolyte: weigh the calculated amount of sodium phosphate, potassium sulfate, disodium ethylenediaminetetraacetic acid, sodium silicate, and surfactant and mix them in deionized water, and adjust the pH value to 4.5-6.5 with dilute ammonia water, and control the temperature at room temperature to 40°C; S3. Electrode setting: The aluminum alloy substrate is used as the anode and the graphite or stainless steel is used as the cathode, which are placed in the electrolyte, and the electrodes are kept at an appropriate distance to avoid short circuit; S3. Micro-arc oxidation parameter setting and monitoring: Apply high voltage, control the voltage through the power supply, and monitor the key parameters of current density, voltage fluctuation, and electrolyte temperature in real time. The control system dynamically adjusts the parameters to maintain a stable micro-arc discharge state to ensure that the local melting and rapid cooling process occur evenly; S4. Processing time and film quality control: Set the processing time according to the required film thickness and performance, and regularly check the morphology and structure of the oxide film on the surface of the aluminum alloy; S5. Post-treatment and testing: After the micro-arc oxidation treatment is completed, water washing is immediately performed to remove residual electrolyte, followed by drying.
5. The method for preparing a novel composite anodic oxide film on the surface of an aluminum alloy according to claim 1, characterized in that: Electrophoretic deposition specifically includes the following steps: S1. Cleaning and activation treatment: rinse with deionized water and dry the surface of the aluminum alloy substrate after micro-arc oxidation treatment, and then perform chemical activation treatment; S2. Coating preparation: Weigh the calculated amount of water-based resin, filler, cross-linking agent, co-solvent and thickener, anti-corrosion additive and leveling agent and mix them in deionized water. Use a pH meter to monitor and adjust the pH value of the coating in the electrophoresis tank to 7-9. At the same time, according to the solid content requirements of the coating, adjust it to the specified range by dilution or concentration to control the coating thickness and quality; S3. Electrophoresis tank setting: Hang the cleaned and activated aluminum alloy substrate into the electrophoresis tank to ensure that the substrate is fully in contact with the electrophoresis coating. The electrophoresis tank is equipped with a constant temperature system to maintain the tank liquid temperature at 25-35°C; S4. Electrophoresis parameter control: Set the voltage to 100-300V, and dynamically adjust it according to the substrate area, coating properties and tank resistance factors. At the same time, monitor the electrophoresis time and adjust the duration of electrophoresis according to the required film thickness; S5. Real-time monitoring and adjustment: The control system monitors the current density, bath temperature, pH value and solid content in real time during the electrophoresis process to ensure the stability and repeatability of the electrophoretic deposition process and adjust the parameters in time to cope with any deviations; S6. Curing treatment: After electrophoretic coating, the substrate is moved into a curing oven for heat curing treatment. The temperature and time should be determined according to the characteristics of the selected cross-linking agent to ensure that the coating is fully cured and enhance its physical and chemical properties.
6. The method for preparing a novel composite anodic oxide film on the surface of an aluminum alloy according to claim 1, characterized in that: The current density, voltage, electrolyte composition and temperature during micro-arc oxidation are monitored in real time and dynamically adjusted during the process, including: Current density monitoring and adjustment: A current sensor is used to continuously monitor the current density changes during arc discharge. The data is fed back to the control system in real time. The ideal current density range is preset according to the surface area of the aluminum alloy substrate, the expected thickness of the oxide film, and process experience. The control system automatically adjusts the power output according to the difference between the measured value and the target value to maintain the current density within the set range, so as to control the oxidation rate and film quality. Voltage management and fluctuation control: The applied voltage is pre-set according to the material properties of the aluminum alloy and the requirements of the oxide film layer, and the intelligent power management system is used to monitor voltage fluctuations in real time. If the voltage fluctuation exceeds the preset threshold of ±5%, the system will immediately adjust the power supply strategy to ensure voltage stability, thereby maintaining the uniform generation and maintenance of tiny arcs and avoiding local overheating or uneven oxidation; Online analysis and adjustment of electrolyte composition: Use an online electrolyte analyzer to periodically or continuously monitor the concentration of the main components in the electrolyte and the pH value. When it is detected that the components deviate from the set ideal ratio or the pH value exceeds the target range of 4.5-6.5, immediately restore the electrolyte to the optimal state by adding corresponding raw materials or adjusting the amount of diluted ammonia water. At the same time, monitor and adjust the electrolyte temperature and use a temperature control device to keep it between room temperature and 40°C to optimize the oxidation process and prevent unnecessary side reactions; Temperature control and environmental adaptability: Install a temperature sensor in the electrolytic cell to accurately control and record the electrolyte temperature; Data recording and analysis: During the implementation process, all key parameters, including current density, voltage, electrolyte composition, and temperature changes, are automatically recorded and stored in the database. Through data analysis software, historical data are compared and analyzed to identify process optimization points, refine parameter setting rules, and provide an ideal process control model for subsequent batches.
7. The method for preparing a novel composite anodic oxide film on the surface of an aluminum alloy according to claim 1, characterized in that: During the process, the key parameters of electrophoretic deposition, such as voltage, time, pH value and solid content, are monitored in real time and dynamically adjusted, including: Voltage control and regulation: In the initial stage of electrophoretic deposition, the voltage range is set between 100-300V according to the substrate area, the resistivity of the coating system and the desired coating thickness. The control system will monitor the voltage change in real time to ensure that it is stable near the set value to maintain the efficiency and uniformity of the electrophoretic deposition process. If the voltage fluctuation exceeds the set range, the system will automatically adjust the power output to maintain the stability of the electrophoretic process; Time management: The time setting of electrophoretic deposition is based on the requirements of film thickness. The basic time range is determined through preliminary experiments, and the coating thickness is monitored in real time. The electrophoretic time is dynamically adjusted according to the actual deposition rate to ensure that the expected film thickness is achieved. The timer is integrated with the thickness measurement device. Once the target thickness is reached, the electrophoretic process is terminated immediately to avoid excessive deposition. pH value monitoring and adjustment: The pH value in the electrophoresis tank is maintained between 7 and 9, and is continuously monitored using an online pH meter. Once the pH value deviates from the ideal range, it is immediately corrected by automatically adding an appropriate amount of acidic or alkaline regulator to ensure the stability of the pH value of the electrophoresis fluid; Solid content monitoring and adjustment: Regularly measure the solid content of the bath liquid with a density meter or viscometer to ensure that it remains within the predetermined range. If the solid content is too high or too low, adjust it by diluting or replenishing the electrophoretic coating to maintain the consistency of the coating quality; the control system automatically starts the dilution or replenishment program based on the measured solid content data to ensure continuous optimization of the coating ratio.
8. The control system of the method for preparing the novel aluminum alloy surface composite anodized film according to any one of claims 1 to 7 comprises: Data acquisition module: Integrates a high-precision sensor network to collect real-time data on current density, voltage, electrolyte composition and temperature during micro-arc oxidation, as well as key parameters such as voltage, time, pH value and solid content during electrophoretic deposition. The sensor data is transmitted to the central processing unit in real time via the Internet of Things. Real-time monitoring center: The central processing unit is equipped with dedicated monitoring software to display the status of all parameters in real time. The visual interface is used to intuitively display the process flow chart and key indicator trends, making it easy for operators to grasp the process status in real time; Algorithm processing unit: equipped with computing servers, running machine learning algorithm models, performing feature analysis, model training and real-time prediction based on historical data. The algorithm processing unit seamlessly connects with the real-time monitoring center, receives real-time data, and instantly feeds back adjustment instructions. Automatic adjustment module: including power management system, temperature control system, pH value automatic adjustment pump, paint automatic dilution / replenishment device, automatically adjusts process parameters according to the instructions of the algorithm processing unit to ensure that the process is stable in the optimal state; Safety and alarm system: integrated with abnormality detection and early warning functions, once a serious deviation of parameters or equipment abnormality is detected, an alarm is immediately triggered and emergency measures are taken, including cutting off power supply and starting backup systems to ensure operational safety; Data analysis and reporting module: automatically summarizes the process data of each operation and generates detailed reports, including operation parameters, key indicator change trends, abnormal situation records and optimization suggestions, providing data support for process improvement and quality management; Human-computer interaction interface: The touch screen interface displays the process flow chart, real-time parameters, alarm information and system status, and provides remote access function for remote monitoring and debugging through the network. System self-learning and optimization: Combining the results of algorithm training and pattern learning, the system continuously updates the model, optimizes the prediction accuracy and adjustment strategy, realizes self-diagnosis and calibration, and the system regularly self-checks the accuracy of sensors and automatically adjusts the correction coefficient to ensure long-term data reliability; Environmental protection and energy consumption management: integrated energy consumption monitoring module, real-time tracking of power consumption, correlation analysis with process parameters, and optimization of energy consumption efficiency; Environmental parameter monitoring ensures that electrolyte composition and wastewater discharge meet environmental standards and achieves green production; Fault prediction and maintenance planning: Analyze historical data through algorithms, predict equipment maintenance needs, formulate preventive maintenance plans, reduce sudden failures, and extend equipment life.
9. The control system according to claim 8, characterized in that: The algorithm processing unit operation process includes the following steps: Feature selection and data preprocessing: First, the collected raw data is preprocessed, including data cleaning, standardization, and feature selection. Data cleaning includes removing outliers and filling missing data. Standardization performs z-score standardization. In feature selection, features that can effectively reflect the process change trend, fluctuation characteristics, and correlation between parameters are selected, including the fluctuation trend of current density over time, electrolyte temperature, and film thickness. Time series analysis: The autoregressive integrated moving average model and its variant autoregressive conditional heteroskedastic moving average model are used to capture and predict the dynamic trend and cyclical fluctuations of key parameters; Classification and regression analysis: Use support vector machines to perform classification tasks, including identifying whether process parameters are in the ideal working range, or using SVR regression models to predict continuous variables of film thickness; Deep learning model: build deep neural networks or recurrent neural networks to process time series data, especially complex nonlinear relationships and long-term and short-term dependencies, such as the complex interaction between current density and voltage and pH value; Training and validation: Split the preprocessed historical job data set into a training set and a validation set. Use the SGD or Adam optimization algorithm to train the model to minimize the loss function, mean square error, or cross entropy, regularly evaluate the model on the validation set, and use early stopping techniques to prevent overfitting. Parameter tuning: Use grid search, random search, or Bayesian optimization methods to find the optimal hyperparameter combination of the model, including learning rate, number of hidden layers, number of nodes, and regularization parameters, to maximize the performance of the model on the validation set; Pattern recognition and prediction: The trained model not only recognizes the normal mode during the operation, including the ideal operating range of parameters, but also predicts the future trend of key parameters, including predicting the current density fluctuation in the next time period based on the current operation status, or predicting the change of membrane quality based on the current pH value; Model fusion: Adopt model fusion strategies to combine the prediction results of different algorithms, including weighted average or performance-based dynamic fusion, to improve the stability and accuracy of the final prediction.
Citation Information
Cited By
Aluminum alloy anodic oxidation process parameter control method and system based on environmental protection
CN119130445A
Aluminum Alloy Anodic Oxidation Process Parameter Control Method and System Based on Environmental Protection
CN119130445B
Uniformity control method for antibacterial coating production
CN119168430A
Uniformity Control Method for Antimicrobial Coating Production
CN119168430B
Alloy film layer and preparation method and application thereof
CN119465335A