A magnetic composite fiber cloth with electromagnetic shielding effect and preparation method thereof
By forming a magnetic adhesive that combines superparamagnetic iron tetroxide with silver plating on the fiber cloth, the problems of weak conductivity, easy oxidation and application limitations of existing electromagnetic shielding materials are solved, and the implementation of the problem of Long-term stable electromagnetic shielding effect and efficient electromagnetic wave absorption.
Patent Information
- Application Number
- CN202411212570.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-30
AI Technical Summary
During the use of existing electromagnetic shielding materials, there are problems such as weak conductivity, easy oxidation, high cost, complex synthesis and limited application, and it is difficult to provide long-term and stable electromagnetic shielding effects in many complex scenarios.
The magnetic adhesive is cured with superparamagnetic iron tetroxide and silver plating to form a magnetic composite fiber cloth. By combining the magnetic adhesive with the adhesive layer of the fiber cloth, the silver plating improves conductivity and toughness, and passes mild conditions. The nano-sized superparamagnetic iron trioxide and silver plating were synthesized to form a fiber cloth with excellent electromagnetic shielding performance.
It realizes the long-term stable electromagnetic shielding effect of fiber cloth in many complex scenarios, enhances the absorption and scattering ability of electromagnetic waves, improves the wear resistance and toughness, and has a simple synthesis process and mild conditions.
Smart Images

Figure CN118727436B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of materials, and in particular to a magnetic composite fiber cloth with electromagnetic shielding function and a preparation method thereof. Background Art
[0002] With the development of electronic information technology and the widespread application of wireless information transmission, people are increasingly relying on various electromagnetic wave transmission devices. The electromagnetic pollution hazards generated by these electronic devices during use cannot be ignored. The electromagnetic pollution caused by electromagnetic waves is mainly reflected in two aspects: one is the harm to human health. People living in an environment polluted by electromagnetic waves for a long time will have a certain negative impact on the nervous system and endocrine system; on the other hand, it interferes with the normal function of electronic equipment. Electromagnetic waves with similar frequencies will cause signal interference to the operation of surrounding electronic devices and communication systems, affecting the reception and transmission of communication signals by the equipment, and even causing information security problems. Therefore, the development of electromagnetic protection materials with high electromagnetic wave shielding performance to strengthen human protection and alleviate mutual interference among radiation sources has important research significance and application prospects.
[0003] As an emerging flexible electromagnetic shielding material, electromagnetic shielding fabric can be flexibly applied to various electromagnetic shielding fields and scenarios through the composite processing of fabric and electromagnetic shielding materials. As a material with good magnetic properties, ferroferric oxide can play a role in magnetic conductivity loss for electromagnetic waves. In addition, ferroferric oxide raw materials are abundant, low cost, and simple to synthesize. However, its weak conductivity and easy oxidation limit the application scope of ferroferric oxide in electromagnetic shielding. Therefore, compounding ferroferric oxide with other conductive materials to enhance conductivity loss and stability is a current research hotspot.
[0004] For example, a Chinese patent with publication number CN105219895A discloses a leather with electromagnetic shielding performance and a preparation method thereof, wherein metal powder, ferroferric oxide powder and a specific solvent are mixed to prepare a dispersion, the dispersion is sprayed on an animal leather containing a film-forming agent on the surface, and then a layer of film-forming agent is sprayed and dried to obtain electromagnetic shielding leather. The double-layer polymer film effectively protects the electromagnetic shielding material in the sandwich layer and prevents the metal powder from being oxidized, but the film-forming agent may enter the gap between the metal powders, reducing the conductivity of the metal powders in the sandwich layer, thereby reducing the electromagnetic shielding effect. At the same time, the animal leather is easily decomposed and destroyed by microorganisms, which makes the electromagnetic shielding leather have a short service life.
[0005] For example, the Chinese patent with publication number CN114351443A discloses a method for producing electromagnetic shielding fabric based on ferroferric oxide / polypyrrole, wherein ferroferric oxide powder is obtained by solvent thermal method and ligand exchange method, and after mixing with pyrrole, monodispersed ferroferric oxide / polypyrrole composite nanoparticles are obtained under oxidative polymerization of ferric chloride, and then the composite particles are dispersed in silicone oil and coated on Kevlar fiber to prepare electromagnetic shielding fabric. The polypyrrole coating effectively prevents the oxidation of ferroferric oxide powder, and polypyrrole has good conductivity, which greatly improves the electromagnetic effect, but the conductive polymer itself is unstable under light and oxygen conditions, and the material itself is hard and brittle, so its practical application on fabrics still has certain limitations.
[0006] For example, a Chinese patent with publication number CN110804772A discloses a core-shell fiber for electromagnetic shielding textiles and a preparation method thereof, wherein ferroferric oxide and graphene with high conductivity and high specific surface area are blown into glass microspheres, and magnetic core layer spinning solution and polyester shell layer spinning solution are prepared respectively by using composite glass microspheres, polyacrylamide, polyester and tetrachloroethane, and then core-shell fibers with excellent electromagnetic shielding performance are synthesized by coaxial electrospinning. The glass structure in the core layer improves the dispersibility of ferroferric oxide and graphene in the composite fiber, effectively protects the main material for electromagnetic shielding, and makes the conductivity loss and magnetic loss work together, while the polyester fiber of the shell layer effectively improves the toughness and human affinity of the composite fiber. However, the synthesis process of the composite glass microspheres in this method needs to be carried out under a high temperature and high pressure environment, and the electrospinning method has strict requirements on external conditions, and the output is extremely low, making it difficult to achieve industrialization.
[0007] In view of this, the present invention proposes a magnetic composite fiber cloth with electromagnetic shielding function and a preparation method thereof to solve the above problems. Summary of the invention
[0008] In order to overcome the shortcomings of the above-mentioned technology, the present invention provides a magnetic composite fiber cloth with electromagnetic shielding function. It has excellent magnetic loss and electrical conductivity loss capabilities, strong electromagnetic shielding ability, and the magnetic composite fiber cloth can withstand continuous bending tests. It can play a long-term and stable electromagnetic shielding role in a variety of complex application scenarios.
[0009] To achieve the above-mentioned purpose, the present invention provides a magnetic composite fiber cloth with electromagnetic shielding effect, including a fiber cloth, the surface of the fiber cloth is cured by a magnetic adhesive to form a magnetic bonding layer, the magnetic adhesive includes an adhesive and superparamagnetic ferroferric oxide; the surface of the magnetic bonding layer is coated with a silver plating layer.
[0010] Preferably, the silver plating layer is formed by reduction deposition of a silver ammonia solution, and a catalyst and a polymer for improving the adhesion of silver are provided on the surface of the magnetic adhesive layer.
[0011] Preferably, the fiber cloth is a roughened hydrophilic fiber cloth, and the adhesive is at least one of polyvinyl alcohol, polyurethane resin, acrylic resin, and phenolic resin.
[0012] Preferably, the mass ratio of the superparamagnetic ferroferric oxide to the adhesive is 0.1-5:1.
[0013] In order to overcome the deficiencies of the above-mentioned technologies, the present invention also provides a method for preparing a magnetic composite fiber cloth with electromagnetic shielding effect, which has simple operation and mild reaction conditions.
[0014] A method for preparing a magnetic composite fiber cloth having an electromagnetic shielding effect comprises the following steps:
[0015] Step 1: adding an aqueous solution of iron salt and ferrous salt into a reactor, slowly dropping an alkali solution into the reactor under the condition of isolating oxygen, reacting for a period of time after the addition of the alkali solution is completed; then adding a hydrophilic surfactant and continuing the reaction for a period of time to obtain superparamagnetic ferroferric oxide nanoparticles, and washing and drying the superparamagnetic ferroferric oxide nanoparticles;
[0016] Step 2: roughening the surface of the fiber cloth by using an alkaline solution;
[0017] Step 3: evenly dispersing superparamagnetic ferroferric oxide nanoparticles in an adhesive to form a magnetic adhesive; soaking the roughened fiber cloth in the magnetic adhesive for a period of time, then taking out the fiber cloth, and curing the magnetic adhesive to obtain a superparamagnetic fiber cloth;
[0018] Step 4: Soak the superparamagnetic fiber cloth in a silanization agent to silanize the superparamagnetic fiber cloth, then soak the silanized superparamagnetic fiber cloth in a graft polymerization monomer solution, and add a polymerization initiator to react for a period of time; after the polymerization is completed, soak the fiber cloth in tetrachloropalladium salt to make the surface of the fiber cloth adhere to [PdCl4] 2- ;
[0019] Step 5: Soak the fiber cloth in a silver ammonia solution, slowly add a reducing agent, heat in a water bath and react for a period of time to obtain a magnetic composite fiber cloth with electromagnetic shielding effect.
[0020] Preferably, in step 3, the silanization agent comprises 3-(trimethoxysilyl)propyl methacrylate, C 1~4 Alcohol, C 1~4 acid and deionized water.
[0021] Preferably, in step 4, the polymerization reaction temperature is 50-90° C., and the polymerization time is 1-12 hours.
[0022] Preferably, the graft polymerization monomer is an acrylic acid monomer containing trimethylammonium salt.
[0023] Preferably, in step 4, the fiber cloth is immersed in tetrachloropalladium salt to undergo ion exchange reaction at a temperature of 10-60° C. and a reaction time of 10-300 min.
[0024] Preferably, in step five, the reducing agent is at least one of glucose, citric acid, ascorbic acid, and potassium sodium tartrate.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] 1. The present invention uniformly solidifies superparamagnetic ferroferric oxide on the surface of the fiber cloth through an adhesive, and the superparamagnetic ferroferric oxide can play a role in magnetic conductivity loss on electromagnetic waves, and the superparamagnetic ferroferric oxide is nanometer-sized and has a high specific surface area, and can more fully interact with electromagnetic waves, thereby enhancing the absorption and scattering effect of electromagnetic waves. In addition, the superparamagnetic ferroferric oxide wrapped by the adhesive can avoid further oxidation of the superparamagnetic ferroferric oxide in a humid environment, and can also prevent the superparamagnetic ferroferric oxide from reacting with other substances or adsorbing other substances on the surface of the superparamagnetic ferroferric oxide, thereby preventing other substances from affecting the electromagnetic shielding ability of the superparamagnetic ferroferric oxide.
[0027] 2. The silver coating has high electrical conductivity, which makes the magnetic composite fiber cloth have high electrical conductivity loss. Electrical conductivity loss will cause the energy of electromagnetic waves to gradually decay during propagation. When electromagnetic waves encounter high-conductivity shielding materials, part of the energy will be converted into heat energy and lost, thereby reducing the intensity of electromagnetic waves. In addition, the silver coating can also improve the wear resistance, strength and toughness of the fiber cloth, and the fiber cloth can withstand harsh repeated bending tests.
[0028] 3. The present invention synthesizes superparamagnetic ferroferric oxide by ferric ion and ferrous ion in an alkaline environment, the process synthesis rate is fast and the conversion rate is high, and a hydrophilic surfactant is added during the synthesis process to avoid superparamagnetic ferroferric oxide from agglomerating into a block, and the superparamagnetic ferroferric oxide is nanometer-sized and has a narrow particle size distribution, and has superparamagnetism. Subsequent superparamagnetic ferroferric oxide modified by a hydrophilic surfactant can be evenly dispersed in an adhesive, which helps the superparamagnetic ferroferric oxide to be evenly distributed on a fiber cloth.
[0029] 4. Before depositing the silver coating, the present invention uses a silanization agent to treat the fiber cloth so that the surface of the fiber cloth is connected to the polymer, and the polymer is easy to adsorb palladium salt. The palladium salt serves as a good catalyst and reduction site to effectively assist the reduction of silver ions. The silver plating method is simple and fast, and the reaction is mild. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a SEM test analysis diagram of the superparamagnetic ferroferric oxide of the present invention;
[0031] Figure 2 is a particle size distribution diagram of superparamagnetic ferroferric oxide of the present invention;
[0032] Figure 3 is the XRD spectrum of the superparamagnetic ferroferric oxide of the present invention;
[0033] Figure 4 is the hysteresis loop of the superparamagnetic ferroferric oxide of the present invention;
[0034] Figure 5 is a schematic diagram of magnetic attraction of the magnetic composite fiber cloth according to Example 1 of the present invention;
[0035] Figure 6 is a schematic diagram of magnetic attraction of the magnetic composite fiber cloth according to Example 2 of the present invention;
[0036] Figure 7 These are the electromagnetic shielding test results of Examples 1-2 and Comparative Examples 1-2;
[0037] Figure 8 This is the electromagnetic shielding test result after repeated bending in Example 2;
[0038] Fig. 9 This is a resistance change analysis diagram after repeated bending in Example 2;
[0039] The implementation, functional features and advantages of the present invention will be further described in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0040] The features of the present invention and other related features are further described in detail below through embodiments to facilitate understanding by those skilled in the art:
[0041] An embodiment of the present invention provides a magnetic composite fiber cloth with electromagnetic shielding function, including a fiber cloth, the surface of the fiber cloth is cured by a magnetic adhesive to form a magnetic bonding layer, the magnetic adhesive includes an adhesive and superparamagnetic ferroferric oxide; the surface of the magnetic bonding layer is coated with a silver plating layer.
[0042] In some embodiments, the silver plating layer is formed by reduction deposition of a silver ammonia solution, and a catalyst and a polymer for improving the adhesion of silver are provided on the surface of the magnetic adhesive layer.
[0043] In some embodiments, the fiber cloth is a roughened hydrophilic fiber cloth, and the adhesive is at least one of polyvinyl alcohol, polyurethane resin, acrylic resin, and phenolic resin.
[0044] In some embodiments, the mass ratio of the superparamagnetic ferroferric oxide to the adhesive is 0.1~5:1.
[0045] An embodiment of the present invention further provides a method for preparing a magnetic composite fiber cloth having an electromagnetic shielding function, comprising the following steps:
[0046] Step 1: adding an aqueous solution of iron salt and ferrous salt into a reactor, slowly dropping an alkali solution into the reactor under the condition of isolating oxygen, reacting for a period of time after the addition of the alkali solution is completed; then adding a hydrophilic surfactant and continuing the reaction for a period of time to obtain superparamagnetic ferroferric oxide nanoparticles, and washing and drying the superparamagnetic ferroferric oxide nanoparticles;
[0047] Step 2: Roughen the surface of the fiber cloth with an alkaline solution; the alkaline solution can hydrolyze and remove grease stains on the surface of the fiber cloth, and some ester groups in the fiber can be hydrolyzed into carboxyl groups, which increases the hydrophilicity of the fiber cloth and its ability to stably combine with the adhesive.
[0048] Step 3: evenly dispersing superparamagnetic ferroferric oxide nanoparticles in an adhesive to form a magnetic adhesive; soaking the roughened fiber cloth in the magnetic adhesive for a period of time, then taking out the fiber cloth, and curing the magnetic adhesive to obtain a superparamagnetic fiber cloth;
[0049] Step 4: Soak the superparamagnetic fiber cloth in a silanization agent to silanize the superparamagnetic fiber cloth, then soak the silanized superparamagnetic fiber cloth in a graft polymerization monomer solution, and add a polymerization initiator to react for a period of time; after the polymerization is completed, soak the fiber cloth in tetrachloropalladium salt to make the surface of the fiber cloth adhere to [PdCl4] 2- ;
[0050] Step 5: Soak the fiber cloth in a silver ammonia solution, slowly add a reducing agent, heat in a water bath and react for a period of time to obtain a magnetic composite fiber cloth with electromagnetic shielding effect.
[0051] In some embodiments, in step 1, Fe 3+ with Fe 2+ The molar ratio is 1.5~2.2:1.
[0052] In some embodiments, the alkaline solution in step 1 is a sodium hydroxide solution.
[0053] In some embodiments, the sodium hydroxide and Fe 2+ The molar ratio is 8~12:1.
[0054] In some embodiments, the step 1 synthesizes superparamagnetic ferroferric oxide under water bath heating conditions, and the water bath heating temperature is 30-70°C.
[0055] In some embodiments, after the alkaline solution in step 1 is added dropwise, the reaction is continued to be kept warm and aged for 15 to 60 minutes.
[0056] In some embodiments, the hydrophilic surfactant is at least one of polyethylene glycol, sodium citrate, sodium dodecyl sulfate, sodium hexadecyl sulfate, and sodium dodecylbenzene sulfonate.
[0057] In some embodiments, the mass ratio of the hydrophilic surfactant to superparamagnetic ferroferric oxide is 0.01-0.2:1.
[0058] In some embodiments, after the hydrophilic surfactant in step 1 is added, the reaction is carried out at 60-90° C. for 30-240 min.
[0059] In some embodiments, the fiber cloth is one of carbon fiber cloth, polyester fiber cloth, and aramid fiber cloth.
[0060] In some embodiments, the alkaline solution in step 2 is a sodium hydroxide solution with a concentration of 0.5-10 mol / L.
[0061] In some embodiments, the step 2 is to synthesize the roughened fiber cloth under water bath heating conditions, and the water bath heating temperature is 40-80°C.
[0062] In some embodiments, the roughening reaction time of step 2 is 30 to 240 minutes.
[0063] In some embodiments, in step 3, the silanization agent includes 3-(trimethoxysilyl)propyl methacrylate, C 1~4 Alcohol, C 1~4 acid and deionized water.
[0064] In some embodiments, in step 4, the polymerization reaction temperature is 50-90° C., and the polymerization time is 1-12 hours.
[0065] In some embodiments, the graft polymerization monomer is an acrylic acid monomer containing trimethylammonium salt.
[0066] In some embodiments, the polymerization initiator is potassium permanganate or persulfate.
[0067] In some embodiments, the polymerization temperature of the graft polymerization monomer is 50-90° C.; and the polymerization reaction time is 1-12 hours.
[0068] In some embodiments, in step 4, the fiber cloth is immersed in tetrachloropalladium salt to undergo an ion exchange reaction at a temperature of 10-60° C. and a reaction time of 10-300 min.
[0069] In some embodiments, in step five, the reducing agent is at least one of glucose, citric acid, ascorbic acid, and potassium sodium tartrate.
[0070] In some embodiments, the silver ammonia solution reduction reaction temperature in step 5 is 20-60° C., and the reaction time is 15-240 min.
[0071] Example 1
[0072] Embodiment 1 of the present invention provides a method for preparing a magnetic composite fiber cloth having an electromagnetic shielding function, comprising the following steps:
[0073] Step 1: Ultrasonic dissolve 15.6 g FeCl3 and 9.5 g FeCl2·4H2O in 40 g pure water, transfer the solution to a three-necked flask, heat it to 40°C in a water bath, turn on the ultrasonic device to quickly stir the reagents in the three-necked flask, and introduce nitrogen to deoxygenate for 30 min.
[0074] 15.5 g of NaOH was dissolved in 36.0 g of pure water, and the obtained NaOH solution was added to the reaction system using a peristaltic pump. After the addition was completed, the reaction system was kept at a specific temperature for 30 min.
[0075] 1.0 g of trisodium citrate was dissolved in 4.0 g of purified water to obtain a hydrophilic surfactant, which was added to the reaction system. The reaction temperature was raised to 90 °C. During this period, a condenser was used to condense the reflux water vapor and N2 was continuously introduced. After four hours of heat preservation, superparamagnetic ferroferric oxide modified with sodium citrate was obtained.
[0076] Afterwards, the superparamagnetic ferroferric oxide was washed with pure water for three times and dried to obtain superparamagnetic ferroferric oxide.
[0077] Step 2: Place the carbon fiber in a 2 mol / L NaOH solution and soak it at room temperature for 1 hour. Then take out the carbon fiber cloth and rinse it with deionized water for 5 times, and dry it in an oven to obtain a roughened hydrophilic carbon fiber cloth.
[0078] Step 3: Mix polyvinyl alcohol and deionized water in a mass ratio of 1:9, place in a water bath at 85 °C for heating and stirring continuously until the polyvinyl alcohol is completely dissolved, then cool to room temperature while stirring to prepare a polyvinyl alcohol solution with a mass fraction of 10%. Take 2 g of the superparamagnetic ferroferric oxide prepared in step 1 and disperse it in 10 ml of polyvinyl alcohol solution, and ultrasonically disperse it for 30 min to obtain a magnetic adhesive.
[0079] The carbon fiber cloth obtained in step 2 is immersed in the magnetic adhesive and ultrasonically treated for 30 minutes. Then, the carbon fiber cloth is taken out, and the excess magnetic adhesive on the surface is removed. The surface of the carbon fiber cloth is solidified to obtain a superparamagnetic carbon fiber cloth.
[0080] Step 4: Soak the superparamagnetic carbon fiber cloth in a silanization reagent and let it stand for 1 hour. The silanization reagent includes the following components by volume fraction: 95% 3-(trimethoxysilyl) propyl methacrylate ethanol solution, 1% acetic acid and 4% deionized water.
[0081] The ethanol solution of 3-(trimethoxysilyl) propyl methacrylate includes 4% 3-(trimethoxysilyl) propyl methacrylate and 96% ethanol. 40 ml of [2-(methacryloyloxy)ethyl]trimethylammonium chloride is dissolved in 200 ml of deionized water to obtain a graft polymerization monomer reagent. The silanized carbon fiber cloth is then soaked in the graft polymerization monomer reagent, and then 400 mg of potassium permanganate is added, and the polymerization reaction is carried out at 80 ° C for 3 h.
[0082] The carbon fiber cloth after polymerization was placed in a 5mmol / L ammonium tetrachloropalladate solution and allowed to stand for 30 minutes to attach [PdCl4] to the surface of the carbon fiber cloth through ion exchange reaction. 2- catalyst.
[0083] Step 5: Add 25% ammonia water to 100 ml of 30 g / L silver nitrate solution until the solution changes from clear to dark gray and then to transparent. Stop adding ammonia water to prepare a silver ammonia solution. Dissolve 60 g of glucose and 6 g of potassium sodium tartrate tetrahydrate in pure water to obtain a reducing solution. 2- The carbon fiber cloth was soaked in the silver ammonia solution for 30 min, and the reducing solution was added dropwise to the silver ammonia solution for reaction at room temperature for 2 h. The carbon fiber cloth was taken out, washed with deionized water for 3 times, and then washed with anhydrous ethanol twice. After drying at room temperature, a magnetic composite fiber cloth with electromagnetic shielding effect was obtained, named C@ Fe-2@Ag.
[0084] Example 2
[0085] Example 2 of the present invention provides a method for preparing a magnetic composite fiber cloth with electromagnetic shielding effect, using 3g of superparamagnetic ferroferric oxide to prepare a magnetic composite fiber cloth with electromagnetic shielding effect, named C@Fe-3Ag. Except that the amount of superparamagnetic ferroferric oxide used in Example 2 is different from that in Example 1, the other operating steps are the same as those in Example 1.
[0086] Comparative Example 1
[0087] Comparative Example 1 of the present invention provides a method for preparing a magnetic composite fiber cloth, including steps 1, 2, and 3 of Example 1, but Comparative Example 1 uses 3g of superparamagnetic ferroferric oxide to prepare the magnetic composite fiber cloth, named C@Fe.
[0088] Comparative Example 2
[0089] Comparative Example 2 of the present invention provides a method for preparing a composite fiber cloth, including steps 2, 4, and 5 of Example 1. The prepared composite fiber cloth is named C@Ag.
[0090] 1. The superparamagnetic ferroferric oxide obtained in Example 1 was subjected to SEM test analysis, as shown in FIG. Figure 1 As shown in the SEM image, superparamagnetic ferroferric oxide appears as spherical nanoparticle aggregates. Figure 2 As shown, statistical analysis of the particle size shows that the particle size distribution of single particles is in the range of 20~70 nm, the particle size distribution is narrow, and the average particle size is 46nm.
[0091] By X-ray diffraction analysis of superparamagnetic iron oxide, such as Figure 3 As shown, the diffraction peaks at 2θ=30.01°, 35.45°, 43.09°, 56.98°, and 62.58° correspond to (2,2,0), (3,1,1), (4,0,0), (5,1,1), and (4,4,0) crystal planes, respectively, indicating that the prepared superparamagnetic ferroferric oxide has an inverse spinel structure. Compared with the XRD spectrum of standard Fe3O4, the position and intensity of each diffraction peak are basically consistent, and the phase is single, without the presence of diffraction peaks of other impurity crystal phases, indicating that the product has high purity.
[0092] 2. The magnetic properties of the superparamagnetic iron oxide of Example 1 were measured using a vibrating sample magnetometer, such as Figure 4 As shown, the saturation magnetization of superparamagnetic ferroferric oxide is 63.5 emu / g, and there is no residual magnetization and coercive force, indicating that it has good superparamagnetism.
[0093] 3. Conduct magnetic tests on the magnetic composite fiber cloth with electromagnetic shielding function of Examples 1 and 2. Use magnets to magnetically attract samples C@ Fe-2@Ag and C@ Fe-3@Ag respectively. Figures 5 and 6 As shown, samples C@Fe-2@Ag and C@Fe-3@Ag can be adsorbed by magnets, indicating that the preparation method of the present invention can successfully form superparamagnetic ferroferric oxide on fiber cloth, and the subsequent deposition of silver plating will not cause the superparamagnetic ferroferric oxide to fall off.
[0094] 4. Electromagnetic shielding test was performed on the composite fiber cloths of Examples 1-2 and Comparative Examples 1-2. Samples C@Fe-2@Ag, C@Fe-3@Ag, C@Fe, and C@Ag were used to shield electromagnetic waves of 8.2-12.4 GHz. Figure 7 As shown, the total shielding effectiveness SE T The average values are 60.6 dB, 55.2 dB, 41.5 dB, and 52.4 dB, respectively. The electromagnetic shielding capability of Examples 1 and 2 is better than that of Comparative Examples 1 and 2, indicating that the superparamagnetic ferroferric oxide and the silver coating work synergistically to enhance the electromagnetic shielding effectiveness of the fabric.
[0095] In contrast to Examples 1 and 2, the electromagnetic shielding effectiveness of C@Fe-2@Ag is better than that of C@Fe-3@Ag. This is because the content of superparamagnetic ferroferric oxide in the magnetic adhesive is relatively high, which may cause the superparamagnetic ferroferric oxide to be exposed on the surface of the magnetic adhesive layer, affecting the deposition of the silver reagent and causing the electromagnetic shielding ability of the fiber cloth to decrease.
[0096] 5. Repeated bending test was performed on the sample C@Fe-3@Ag of Example 2. The sample C@Fe-3@Ag was bent in half to form a double-layer fiber cloth, and the double-layer fiber cloth was named DC@Fe-3@Ag. After being bent 10,000 times at a bending radius of 5 mm, the bent double-layer fiber cloth was named DC@Fe-3@Ag-10000.
[0097] The samples DC@Fe-3@Ag and DC@Fe-3@Ag-10000 are shielded against electromagnetic waves of 8.2~12.4GHz. Figure 8 As shown, the total electromagnetic shielding effectiveness SE of samples DC@Fe-3@Ag and DC@Fe-3@Ag-10000 T The average values were 83.1dB. After the bending test, the total shielding effectiveness decreased by 14.8% compared with the initial value, but still maintained excellent electromagnetic shielding performance.
[0098] During the repeated bending process of the sample C@Fe-3@Ag, the resistance of the fiber cloth was tested after each bending. When testing the resistance, the fiber cloth was a single layer. Fig. 9 As shown, the resistance of the sample C@Fe-3@Ag is 1.169Ω and the conductivity is 78.5S / cm when it is not bent. After bending 10,000 times, the resistance is 1.22Ω and the conductivity is 69.4 S / cm, which means the resistance has increased by 4.3%. The resistance has changed little after 10,000 bending tests, and it still maintains a high conductivity loss capacity for electromagnetic waves.
[0099] During the repeated bending of sample C@Fe-3@Ag, the rate of increase in the resistance of the fiber cloth gradually slowed down from about the 7000th to 10000th bending times, indicating that the internal structure of the fiber cloth of the present invention can remain stable during a large number of bendings. This is due to the fact that the adhesive solidifies the superparamagnetic ferroferric oxide on the fiber cloth, and the silver plating improves the wear resistance, strength and toughness of the fiber cloth, making it less likely for the fiber cloth to break or undergo serious structural changes during the bending process, and the fiber cloth has good flexibility.
[0100] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. Any equivalent structural transformation made by using the contents of the present invention description and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a magnetic composite fiber cloth having electromagnetic shielding effect, It is characterized in that The following steps are involved: Step 1: adding an aqueous solution of iron salt and ferrous salt into a reactor, slowly dropping an alkali solution into the reactor under the condition of isolating oxygen, reacting for a period of time after the addition of the alkali solution is completed; then adding a hydrophilic surfactant and continuing the reaction for a period of time to obtain superparamagnetic ferroferric oxide nanoparticles, and washing and drying the superparamagnetic ferroferric oxide nanoparticles; Step 2: roughening the surface of the fiber cloth by using an alkaline solution; Step 3: evenly dispersing superparamagnetic ferroferric oxide nanoparticles in an adhesive to form a magnetic adhesive; soaking the roughened fiber cloth in the magnetic adhesive for a period of time, then taking out the fiber cloth, and curing the magnetic adhesive to obtain a superparamagnetic fiber cloth; Step 4: soaking the superparamagnetic fiber cloth in a silanization agent to silanize the superparamagnetic fiber cloth, then soaking the silanized superparamagnetic fiber cloth in a graft polymerization monomer solution, and adding a polymerization initiator to react for a period of time; After the polymerization is completed, the fiber cloth is immersed in tetrachloropalladium salt to make the surface of the fiber cloth adhere to [PdCl4] 2- ; Step 5: Soak the fiber cloth in a silver ammonia solution, slowly add a reducing agent, heat in a water bath for a period of time, and obtain a magnetic composite fiber cloth with electromagnetic shielding effect; The fiber cloth is a roughened hydrophilic fiber cloth, and the adhesive is at least one of polyvinyl alcohol, polyurethane resin, acrylic resin, and phenolic resin; The mass ratio of superparamagnetic ferroferric oxide to adhesive is 0.1-5:1; In the step 3, the silanization reagent includes C 1~4 Alcohol, C 1~4 acid, deionized water, and 3-(trimethoxysilyl)propyl methacrylate; The graft polymerization monomer is an acrylic acid monomer containing trimethylammonium salt.
2. The method for preparing a magnetic composite fiber cloth having electromagnetic shielding effect according to claim 1, It is characterized in that In the step 4, the polymerization reaction temperature is 50-90° C., and the polymerization time is 1-12 hours.
3. The method for preparing a magnetic composite fiber cloth having electromagnetic shielding effect according to claim 1, It is characterized in that In the step 4, the fiber cloth is immersed in tetrachloropalladium salt to undergo an ion exchange reaction at a temperature of 10-60° C. and a reaction time of 10-300 min.
4. The method for preparing a magnetic composite fiber cloth having electromagnetic shielding effect according to claim 1, It is characterized in that In the step 5, the reducing agent is at least one of glucose, citric acid, ascorbic acid, and potassium sodium tartrate.
5. A magnetic composite fiber cloth with electromagnetic shielding effect, It is characterized in that The invention is prepared by the method for preparing the magnetic composite fiber cloth with electromagnetic shielding function as claimed in claim 1.