Treatment method for increasing active sites of polyimide fiber

By immersing the polyimide fiber in ring-opening and chemical treatment, active sites are provided, which solves the problem of fiber surface inertness, improves the adhesion of the fiber, and is suitable for structural reinforcement applications of a variety of materials.

CN118727445AInactive Publication Date: 2024-10-01邓皓琦
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411153097.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Due to the lack of active sites on the inert surface of polyimide fiber, the reliability of bonding cannot be guaranteed when using adhesives.

Method used

The polyimide fiber is immersed in distilled water for ring opening, and potassium hydroxide and silane coupling agent are added to the ring opening to provide an appropriate amount of active sites to improve the adhesion of the fiber.

Benefits of technology

Without destroying the overall chain segment of the polyimide material, it successfully provides active sites for the fiber surface, improving the fiber bonding reliability and practicality. It is suitable for surface coatings, resin structure reinforcement, rubber materials and ablation. The carbon-fixing layer of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention relates to the field of polyimide fibers, in particular to a treatment method for increasing active sites of polyimide fibers, and aims to solve the problems that the fiber surface in the current market is an inert surface and has no active sites, and the bonding reliability cannot be ensured by using a bonding agent. The method comprises the following steps: immersing polyimide in water for ring opening, and immersing dried polyimide fibers in absolute ethyl alcohol until the polyimide fibers are completely infiltrated; according to the invention, ring opening is carried out on the polyimide chain link part on the fiber surface under the condition that the overall chain segment of the polyimide material is not damaged, and then coupling agent molecules are connected to the ring opening part through a chemical treatment method to provide a proper amount of active sites, so that the possibility is provided for polyimide bonding, and the problems that the polyimide fiber belongs to a difficult-to-bond material and cannot be bonded easily are solved. The surface of the common fiber sold in the market is an inert surface and has no active site, and the bonding reliability cannot be ensured by using a bonding agent, so that the practicability is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyimide fibers, in particular to a treatment method for increasing active sites of polyimide fibers. Background Art

[0002] Polyimide fiber is a fibrous material made from polyimide resin through spinning, stretching and other processes. Polyimide is a high-performance organic polymer material with excellent thermal stability, chemical stability, mechanical properties and electrical properties. Therefore, it is widely used in aerospace, electronics, automobiles, medical and other fields.

[0003] Currently, polyimide fibers are difficult to bond. Most common fiber surfaces on the market are inert surfaces with no active sites. When adhesives are used, the bonding reliability cannot be guaranteed.

[0004] In view of the above problems, a treatment method for increasing the active sites of polyimide fibers is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a treatment method for increasing the active sites of polyimide fibers. The device is used to work, thereby solving the problem that most common fiber surfaces in the above background are inert surfaces without active sites, and the bonding reliability cannot be guaranteed when using adhesives.

[0006] To achieve the above object, the present invention provides the following technical solution: a treatment method for increasing active sites of polyimide fibers, comprising the following steps: S1: Immerse the polyimide in water to open the ring; S2: Immerse the dried polyimide fiber in anhydrous ethanol until it is completely soaked.

[0007] Furthermore, the specific steps of water-immersing and ring-opening the polyimide in S1 are as follows: S101: immersing the polyimide fiber in distilled water under standard conditions, and oscillating the polyimide fiber with low-temperature ultrasound at a frequency of 80 to 100 kHz for 0.5 h; S102: taking the fiber out of the distilled water, placing it in a potassium hydroxide-water solution, and performing continuous stirring treatment in a water bath heating state; S103: Take out the fiber, filter out the treatment liquid, and then immediately rinse it with distilled water that covers the surface of the fiber, and then filter it, and repeat the rinsing operation again, and then filter it clean; S104: Place in an oven for drying.

[0008] Furthermore, the concentration of the potassium hydroxide-water solution in S102 is 0.5 mol / L.

[0009] Furthermore, the water bath heating temperature in S102 is 35±5° C., and the continuous stirring treatment time is 3 hours.

[0010] Furthermore, in S104, if the requirements for the product are not high, the temperature is controlled between 50 and 60°C and air drying is used. If the product has high requirements and the surface of the short fibers or powder is treated, freeze drying is performed using a freeze dryer.

[0011] Furthermore, in S2, the specific steps of immersing the dried polyimide fiber in anhydrous ethanol until it is completely soaked are: S201: Take out the fiber, put it into the silane coupling agent KH560-anhydrous ethanol solution, and perform continuous stirring treatment in a water bath heating state; S202: Take out the fiber, filter out the treatment liquid, and then immediately soak and wash it with anhydrous ethanol that covers the surface of the fiber, and then filter it, and then repeat the soaking and washing operation and filter it clean; S203: placing in an oven for drying.

[0012] Furthermore, the concentration of the silane coupling agent in S201 is 0.5 mol / L, the water bath heating temperature in S201 is 50±5° C., and the continuous stirring treatment time is 1 hour.

[0013] Furthermore, the temperature of the oven in S203 is 50±5°C.

[0014] Furthermore, the processable materials include: surface treatment of polyimide plants, surface treatment of polyimide chopped fibers, and pretreatment of polyimide powders.

[0015] Furthermore, the application scope of the treated fiber is: structural reinforcement of surface coatings or resins, structural reinforcement of rubber materials, and solid carbon fiber layer of ablative material solid carbon layer.

[0016] Compared with the prior art, the present invention has the following beneficial effects: This solution is to open the polyimide chain segments on the fiber surface without destroying the overall chain segments of the polyimide material, and then connect coupling agent molecules at the open loops through chemical treatment to provide an appropriate amount of active sites, thereby providing the possibility for polyimide bonding. This solves the problem that the current fiber surface is an inert surface with no active sites and the use of adhesives cannot guarantee bonding reliability, thereby improving practicality. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of the overall process of the present invention; Figure 2 This is a schematic diagram of a specific process of water-immersing and ring-opening polyimide in the present invention; Figure 3This is a schematic diagram of a specific process of immersing the dried polyimide fiber in anhydrous ethanol until it is completely soaked in the present invention; Figure 4 A schematic diagram of the chemical mechanism of the treatment method of the present invention; Figure 5 This is a schematic diagram of a picture of polyimide chopped fibers treated in the present invention; Figure 6 This is a schematic diagram of cutting the surface of the fiber after the treated fiber is compounded with other materials in the present invention. DETAILED DESCRIPTION

[0018] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] In order to solve the technical problem that the current polyimide fiber is a difficult-to-bond material, most of the common fiber surfaces on the market are inert surfaces with no active sites, and the bonding reliability cannot be guaranteed when using adhesives, such as Figure 1 - Figure 2 and Figure 4 - Figure 6 As shown, the following preferred technical solutions are provided: A method for increasing active sites of polyimide fibers comprises the following steps: S1: Immerse the polyimide in water to open the ring;

[0020] S2: Immerse the dried polyimide fiber in anhydrous ethanol until it is completely soaked.

[0021] The polyimide fiber is completely soaked with distilled water and washed once, and the dried polyimide fiber is immersed in anhydrous ethanol until it is completely soaked, so that the polyimide chain segments on the fiber surface are partially opened without destroying the overall chain segments of the polyimide material, and then coupling agent molecules are connected at the open loops by chemical treatment to provide an appropriate amount of active sites, thereby making polyimide bonding possible.

[0022] The specific steps of water-immersing and ring-opening the polyimide in S1 are as follows: S101: immersing the polyimide fiber in distilled water under standard conditions, and oscillating the polyimide fiber with low-temperature ultrasound at a frequency of 80 to 100 kHz for 0.5 h; S102: The fiber is taken out from the distilled water, placed in a potassium hydroxide-water solution, and continuously stirred in a water bath heating state.

[0023] S103: Take out the fiber, filter out the treatment liquid, filter by suction, and then immediately rinse with distilled water that covers the surface of the fiber, filter by suction, repeat the rinsing operation, and filter by suction.

[0024] S104: Place in an oven for drying.

[0025] The concentration of the potassium hydroxide-water solution in S102 is 0.5 mol / L.

[0026] The water bath heating temperature in S102 is 35±5° C., and the continuous stirring treatment time is 3 hours.

[0027] In S104, if the requirements for the product are not high, the temperature is controlled between 50 and 60°C and air drying is used. If high requirements are for the product, in the case of short fibers or powder surface treatment, freeze drying is performed using a freeze dryer.

[0028] In this scheme: first, the polyimide fiber is completely soaked and washed with distilled water under standard conditions; then the fiber is immersed in a potassium hydroxide-water solution with a concentration of 0.5 mol / L, and then continuously stirred for 3 hours in a water bath heated at a water temperature of 35±5°C. After 3 hours, the fiber is taken out, the treatment liquid is filtered out, and then immediately immersed in distilled water covering the surface of the fiber, and filtered, and the immersion operation is repeated again, and filtered clean; finally, the fiber is dried. If the product requirements are not high, the temperature is controlled between 40 and 60°C, and the fiber is dried by air blast. If the product requirements are high, a freeze dryer is used for surface treatment of short fibers or powders.

[0029] like Figure 3 - Figure 6 As shown, the following preferred technical solutions are provided: In S2, the specific steps of immersing the dried polyimide fiber in anhydrous ethanol until it is completely soaked are: S201: Take out the fiber, put it into the silane coupling agent KH560-anhydrous ethanol solution, and carry out continuous stirring treatment in a water bath heating state.

[0030] S202: Take out the fiber, filter out the treatment liquid, filter by suction, and then immediately rinse with anhydrous ethanol that covers the surface of the fiber, filter by suction, repeat the rinsing operation, and filter by suction.

[0031] S203: placing in an oven for drying.

[0032] The concentration of the silane coupling agent in S201 is 0.5 mol / L, the water bath heating temperature in S201 is 50±5° C., and the continuous stirring treatment time is 1 hour.

[0033] The temperature of the oven in S203 is 50±5°C.

[0034] In this scheme: the fiber is taken out, placed in a 0.5 mol / L silane coupling agent KH560-anhydrous ethanol solution, immersed in water, and then heated in a water bath at a water temperature of 50±5°C, continuously stirred for 1 hour. After 1 hour, the fiber is taken out, the treated liquid is filtered, and then immediately immersed in anhydrous ethanol that covers the surface of the fiber, and filtered, and the immersion operation is repeated again, and the fiber is filtered clean, and finally the fiber is placed in a 60°C oven for drying.

[0035] like Figure 4 - Figure 6 As shown, the following preferred technical solutions are provided: The materials that can be treated include: surface treatment of polyimide plants, surface treatment of polyimide chopped fibers, and pretreatment of polyimide powders.

[0036] The application scope of the treated fiber: structural reinforcement of surface coatings or resins, structural reinforcement of rubber materials, and solid carbon fiber layer of the carbon layer of ablative materials.

[0037] In this scheme: during the surface treatment of polyimide fabrics, the water-immersion and ring-opening time of polyimide needs to be appropriately extended, and the recommended time is 4 hours, at which time the effect is best; during the surface treatment of polyimide chopped fibers, the water-immersion and ring-opening time of polyimide needs to be appropriately extended, and the recommended time is 2 to 3 hours, at which time the effect is best; during the pretreatment of polyimide powders, the water-immersion and ring-opening time of polyimide needs to be appropriately shortened, and it is recommended not to exceed 1 hour to avoid any impact.

[0038] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0039] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for increasing active sites of polyimide fibers, characterized in that: The following steps are involved: S1: Immerse the polyimide in water to open the ring; S2: Immerse the dried polyimide fiber in anhydrous ethanol until it is completely soaked.

2. A method for increasing active sites of polyimide fibers according to claim 1, characterized in that: The specific steps of water-immersing and ring-opening the polyimide in S1 are as follows: S101: immersing the polyimide fiber in distilled water under standard conditions, and oscillating the polyimide fiber with low-temperature ultrasound at a frequency of 80 to 100 kHz for 0.5 h; S102: taking the fiber out of the distilled water, placing it in a potassium hydroxide-water solution, and performing continuous stirring treatment in a water bath heating state; S103: Take out the fiber, filter out the treatment liquid, and then immediately rinse it with distilled water that covers the surface of the fiber, and then filter it, and repeat the rinsing operation again, and then filter it clean; S104: Place in an oven for drying.

3. A method for increasing active sites of polyimide fibers according to claim 2, characterized in that: The concentration of the potassium hydroxide-water solution in S102 is 0.5 mol / L.

4. A method for increasing active sites of polyimide fibers according to claim 3, characterized in that: The water bath heating temperature in S102 is 40±5° C., and the continuous stirring treatment time is 3 hours.

5. A method for increasing active sites of polyimide fibers according to claim 4, characterized in that: In S104, if the requirements for the product are not high, the temperature is controlled between 50 and 60°C and air drying is used. If high requirements are for the product, in the case of short fibers or powder surface treatment, freeze drying is performed using a freeze dryer.

6. A method for increasing active sites of polyimide fibers according to claim 5, characterized in that: In S2, the specific steps of immersing the dried polyimide fiber in anhydrous ethanol until it is completely soaked are: S201: Take out the fiber, put it into the silane coupling agent KH560-anhydrous ethanol solution, and perform continuous stirring treatment in a water bath heating state; S202: Take out the fiber, filter out the treatment liquid, and then immediately rinse it with anhydrous ethanol that covers the surface of the fiber, and then filter it, and repeat the rinsing operation again, and then filter it clean; S203: placing in an oven for drying.

7. A method for increasing active sites of polyimide fibers according to claim 6, characterized in that: The concentration of the silane coupling agent in S201 is 0.5 mol / L, the water bath heating temperature in S201 is 50±5° C., and the continuous stirring treatment time is 1 hour.

8. A method for increasing active sites of polyimide fibers according to claim 7, characterized in that: The temperature of the oven in S203 is 50±5°C.

9. A method for increasing active sites of polyimide fibers according to claim 8, characterized in that: The materials that can be treated include: surface treatment of polyimide plants, surface treatment of polyimide chopped fibers, and pretreatment of polyimide powders.

10. A method for increasing active sites of polyimide fibers according to claim 9, characterized in that: The application scope of the treated fiber: structural reinforcement of surface coatings or resins, structural reinforcement of rubber materials, and solid carbon fiber layer of the carbon layer of ablative materials.