A method, device and system for measuring corrosion thickness of pipeline
By using the zero group velocity Lamb wave mode to calculate the theoretical dispersion curve and the center frequency of the resonant peak, and measuring the corrosion thickness of the pipeline, it solves the problem of difficulty in accurately detecting the thickness of the pipeline wall in the existing technology and achieves high-accuracy corrosion detection. Thickness measurement improves safety.
Patent Information
- Application Number
- CN202411230613.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-09-04
AI Technical Summary
Existing pipe wall thickness detection methods are difficult to accurately measure corrosion thickness, especially in erosion environments, leading to increased leakage and safety risks.
The zero group velocity Lamb wave mode (ZGV Lamb Waves) is used to measure the pipeline corrosion thickness. The theoretical dispersion curve is calculated by obtaining the pipeline attribute parameters, the theoretical frequency thickness product and the resonance peak center frequency are determined, and the target excitation signal is sent and the reflected waveform is received. signal, determine the center frequency of the resonance peak, and calculate the corrosion thickness.
It realizes the timely measurement of the corrosion thickness of pipelines in erosion environments, improves the safety of pipeline use, has high accuracy, and the error is within 1.6%-4.8%.
Smart Images

Figure CN118730006B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of pipelines, and in particular to a method, device and system for measuring the corrosion thickness of pipelines. Background Art
[0002] Non-renewable energy such as oil and natural gas occupies an important position in the energy structure system and is one of the indispensable energy sources for industrial production. In order to realize the efficient and safe use of these energy sources, a complete transportation process must be established. Among them, oil and gas pipeline transportation has been widely used due to its low cost and high efficiency.
[0003] As the service time of pipelines increases, oil and gas pipelines are in an erosion environment of mixed media such as petroleum gas and impurity particles for a long time, resulting in varying degrees of erosion damage to the inner wall of the pipeline. This erosion and corrosion may cause the pipeline wall to become thinner or crack, increasing the risk of pipeline rupture or leakage. Pipeline leakage may lead to explosions, fires or other dangerous situations, posing a serious threat to the safety of personnel and property. Therefore, how to effectively and conveniently detect the corrosion thickness of oil and gas pipelines has become a technical problem waiting to be solved. Summary of the invention
[0004] The invention provides a method, a device and a system for measuring the corrosion thickness of a pipeline, which are used for measuring the corrosion thickness of the pipeline.
[0005] In one aspect, the present invention provides a method for measuring the corrosion thickness of a pipeline, comprising:
[0006] Acquiring property parameters of the pipeline to be detected, and calculating a theoretical dispersion curve of the pipeline to be detected according to the property parameters;
[0007] Determining the theoretical frequency-thickness product and the theoretical resonance peak center frequency of the zero group velocity Lamb wave mode from the theoretical dispersion curve;
[0008] Obtaining a target excitation signal corresponding to the theoretical resonance peak center frequency;
[0009] Sending a target excitation signal to the pipeline to be detected, and receiving a target waveform signal, wherein the target waveform signal is obtained by reflecting the target excitation signal through the pipeline to be detected;
[0010] Determining the resonance peak center frequency of the zero group velocity Lamb wave mode from the target waveform signal;
[0011] The corrosion thickness of the pipeline to be inspected is calculated based on the theoretical frequency-thickness product and the resonance peak center frequency of the zero group velocity Lamb wave mode.
[0012] Optionally, sending a target excitation signal to the pipeline to be inspected and receiving a target waveform signal specifically includes:
[0013] Using array elements of a linear phased array probe, a target excitation signal is sent to the pipeline to be inspected, and a target waveform signal is received;
[0014] Wherein, the linear phased array probe is provided with a plurality of array elements, and the number of the target waveform signals is consistent with the number of the array elements.
[0015] Optionally, determining the resonance peak center frequency of the zero group velocity Lamb wave mode from the target waveform signal specifically includes:
[0016] The resonance peak center frequency of the zero group velocity Lamb wave mode is determined from each group of the target waveform signals respectively, and a plurality of groups of resonance peak center frequencies of the zero group velocity Lamb wave modes are obtained.
[0017] Optionally, the calculating the corrosion thickness of the pipeline to be inspected according to the theoretical frequency-thickness product and the resonance peak center frequency of the zero group velocity Lamb wave mode specifically includes:
[0018] Performing thickness calculations on the resonance peak center frequencies of several groups of zero group velocity Lamb wave modes and the theoretical frequency-thickness product to obtain several groups of thickness values;
[0019] Fitting is performed on several groups of thickness values to obtain the corrosion thickness of the pipeline to be inspected.
[0020] Optionally, the thickness calculation formula is:
[0021]
[0022] in, is the theoretical frequency product, is the resonance peak center frequency of the zero group velocity Lamb wave mode, is the thickness value.
[0023] Another aspect of the present invention provides a device for measuring pipeline corrosion thickness, comprising:
[0024] A first acquisition module is used to acquire attribute parameters of the pipeline to be detected, and calculate a theoretical dispersion curve of the pipeline to be detected according to the attribute parameters;
[0025] A first determination module is used to determine the theoretical frequency-thickness product and the theoretical resonance peak center frequency of the zero group velocity Lamb wave mode from the theoretical dispersion curve;
[0026] A second acquisition module is used to acquire a target excitation signal corresponding to the theoretical resonance peak center frequency;
[0027] An excitation module, used for sending a target excitation signal to the pipeline to be detected and receiving a target waveform signal, wherein the target waveform signal is obtained by reflecting the target excitation signal through the pipeline to be detected;
[0028] A second determination module is used to determine the resonance peak center frequency of the zero group velocity Lamb wave mode from the target waveform signal;
[0029] The calculation module is used to calculate the corrosion thickness of the pipeline to be detected according to the theoretical frequency-thickness product and the resonance peak center frequency of the zero group velocity Lamb wave mode.
[0030] Optionally, the excitation module is specifically used to use a linear phased array probe to send a target excitation signal to the pipeline to be inspected and receive a target waveform signal; wherein the linear phased array probe is provided with a plurality of array elements, and the number of the target waveform signals is consistent with the number of the array elements.
[0031] Optionally, the second determination module is specifically used to determine the resonance peak center frequency of the zero group velocity Lamb wave mode from each group of the target waveform signals, and obtain several groups of resonance peak center frequencies of the zero group velocity Lamb wave modes.
[0032] Optionally, the calculation module includes:
[0033] A thickness value calculation subunit is used to calculate the thickness of a plurality of groups of resonance peak center frequencies of the zero group velocity Lamb wave modes and the theoretical frequency-thickness product to obtain a plurality of groups of thickness values;
[0034] The fitting subunit is used to fit several groups of thickness values to obtain the corrosion thickness of the pipeline to be detected.
[0035] On the other hand, the present invention provides a system for measuring the corrosion thickness of a pipeline, comprising: a linear array phased array probe, a phased array board, and a controller; the phased array board is connected to the linear array phased array probe, and the controller is respectively connected to the phased array board and the linear array phased array probe, for executing the method described above.
[0036] It can be seen from the above technical solutions that the present invention has the following advantages:
[0037] The invention provides a method for measuring the corrosion thickness of a pipeline, comprising: obtaining attribute parameters of a pipeline to be detected, and calculating a theoretical dispersion curve of the pipeline to be detected according to the attribute parameters; determining a theoretical frequency-thickness product and a theoretical resonance peak center frequency of a zero group velocity Lamb wave mode from the theoretical dispersion curve; obtaining a target excitation signal corresponding to the theoretical resonance peak center frequency; sending a target excitation signal to the pipeline to be detected, and receiving a target waveform signal, wherein the target waveform signal is obtained by reflecting the target excitation signal through the pipeline to be detected; determining the resonance peak center frequency of the zero group velocity Lamb wave mode from the target waveform signal; and calculating the corrosion thickness of the pipeline to be detected according to the theoretical frequency-thickness product and the resonance peak center frequency of the zero group velocity Lamb wave mode.
[0038] The present invention obtains the property parameters of the pipeline to be detected, calculates the theoretical dispersion curve of the pipeline to be detected according to the property parameters, realizes the acquisition of the theoretical dispersion curve of the pipeline to be detected, and provides a technical basis for the determination of the excitation signal; and from the theoretical dispersion curve, determines the theoretical frequency-thickness product and the theoretical resonance peak center frequency of the zero group velocity Lamb wave mode, realizes the determination of the theoretical frequency-thickness product and the theoretical resonance peak center frequency; obtains the target excitation signal corresponding to the theoretical resonance peak center frequency, realizes the determination of the target excitation signal, so that in actual measurement, the zero group velocity Lamb wave mode can be effectively excited in the pipeline to be detected; and by emitting the target excitation signal to the pipeline to be detected, A target excitation signal is sent, and a target waveform signal obtained by reflecting the target excitation signal through the pipeline to be detected is received, so as to provide effective data support for calculating the corrosion thickness of the pipeline; and the resonance peak center frequency of the zero group velocity Lamb wave mode is determined from the target waveform signal, and the corrosion thickness of the pipeline to be detected is calculated according to the theoretical frequency-thickness product and the resonance peak center frequency of the zero group velocity Lamb wave mode, so as to effectively realize the calculation of the corrosion thickness of the pipeline to be detected, so that in practical applications, the thickness of the pipeline to be detected in an erosion environment can be measured in time, the corrosion condition of the pipeline can be monitored, and the safety of pipeline use can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0040] Figure 1 A flow chart of the steps of a method for measuring corrosion thickness of a pipeline provided by an embodiment of the present invention;
[0041] Figure 2 A dispersion curve diagram of a 6061 aluminum plate provided in an embodiment of the present invention;
[0042] Figure 3 A flowchart of a method for measuring corrosion thickness of a pipeline provided by another embodiment of the present invention;
[0043] Figure 4 A two-dimensional finite element model diagram provided for another embodiment of the present invention;
[0044] Figure 5 A 900KHz time domain diagram of an excitation signal provided by another embodiment of the present invention;
[0045] Figure 6 A 900KHz frequency domain diagram of an excitation signal provided by another embodiment of the present invention;
[0046] Figure 7 A waveform diagram of a waveform signal provided by another embodiment of the present invention;
[0047] Figure 8 A frequency domain diagram of an S1-ZGV mode provided by another embodiment of the present invention;
[0048] Fig. 9 A simulation diagram of a two-dimensional structure with corrosion defects provided by another embodiment of the present invention;
[0049] Fig.10 A frequency domain diagram of signals received by nodes D4 and D5 provided in another embodiment of the present invention;
[0050] Fig.11 A comparison diagram of inversion thickness and true thickness provided in another embodiment of the present invention;
[0051] Fig.12 A technical flow chart provided for an application example of the present invention;
[0052] Fig.13 A schematic structural diagram of a device for measuring corrosion thickness of a pipeline provided by an embodiment of the present invention;
[0053] Fig.14 A schematic structural diagram of a system for measuring corrosion thickness of a pipeline provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0054] At present, the methods for detecting the wall thickness of oil and gas pipelines mainly include ultrasonic detection, eddy current detection, laser detection and X-ray detection. The eddy current detection method has the characteristics of no coupling and fast detection speed, but it is only suitable for the detection of conductive materials and thin layers of materials. The laser detection method is a non-contact detection method with fewer restrictions and high efficiency, but there are great challenges in subsequent data processing. The advantage of the X-ray detection method is that it has a wide detection range and can intuitively display the shape type of defects, but the radiation is very harmful to the human body and the cost is high. In comparison, the ultrasonic detection method also has a wide detection range and strong applicability. It is non-destructive and has good directionality in pipeline wall thickness detection. It has been gradually applied in the field of metal material thickness measurement, especially Lamb waves.
[0055] Among various Lamb wave types, there is a special mode called Zero-Group-Velocity Lamb Waves (ZGV Lamb Waves). The group velocity of ZGV Lamb waves is zero, which indicates that the acoustic energy is confined around the excitation area. Therefore, it has extremely high sensitivity for the detection of local material properties, defects and thickness changes. However, at present, the application of ZGV mode is mainly focused on local stress detection, and there is little research on local thickness changes.
[0056] As can be seen from the above, most of the existing measurement technologies rely on the amplitude characteristics of the received signal, and the signal amplitude is usually affected by external parameters (such as coatings and corrosion plaques), which cannot accurately represent the wall thickness loss, resulting in measurement difficulties. Therefore, how to effectively and conveniently detect the thickness of the pipeline wall has become a technical problem waiting to be solved.
[0057] The embodiments of the present invention provide a method, device and system for measuring the corrosion thickness of a pipeline, which are used to measure the corrosion thickness of the pipeline.
[0058] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the drawings in the embodiments of the present invention. Obviously, the embodiments described below are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0059] See also Figure 1 The present invention provides a method for measuring the corrosion thickness of a pipeline, comprising:
[0060] 101. Obtain attribute parameters of the pipeline to be detected, and calculate a theoretical dispersion curve of the pipeline to be detected according to the attribute parameters.
[0061] It should be noted that this embodiment uses zero-group-velocity Lamb Waves (ZGV Lamb Waves) to measure the corrosion thickness of the pipeline. The effective excitation of the ZGV mode is closely related to the selected excitation signal, and the excitation frequency of the excitation signal mainly depends on the thickness and material properties of the pipeline. Since only a specific position on the pipeline cross section is scanned when the pipeline is inspected, this embodiment solves the dispersion curve of the corresponding plate-like structure and determines the excitation frequency of the excitation signal according to the frequency of the Lamb wave mode with zero group velocity, so as to effectively excite the ZGV mode in the pipeline to be inspected.
[0062] The property parameters of the pipeline to be tested include pipeline thickness and linear elastic constants, wherein the linear elastic constants include: material density, Young's modulus, Poisson's ratio, etc. This embodiment uses the property parameters of the pipeline to be tested, adopts COMSOL Multiphysics software, constructs a plate structure model, sets corresponding boundary conditions, research types, scanning parameters, and runs the plate structure model to obtain the corresponding theoretical dispersion curve.
[0063] The pipeline to be inspected can be determined according to actual inspection requirements. The present invention is described by taking a pipeline structure of a 6061 aluminum tube with a thickness of 3 mm as an example.
[0064] Among them, the calculation principle of the theoretical dispersion prediction curve is as follows:
[0065] Lamb waves refer to guided waves formed by ultrasonic body waves after multiple reflections and superpositions on the upper and lower surfaces of a thin plate, resulting in complex mutual interference and geometric diffusion. They are named after Mr. Lamb's research on free-boundary thin plates, so they are called "Lamb waves".
[0066] Lamb waves have multi-modal and dispersive propagation characteristics. In a free boundary thin plate, the dispersion characteristics of elastic waves can be solved by the Rayleigh-Lamb equation:
[0067] For the symmetric mode (S):
[0068]
[0069] For the antisymmetric mode (A):
[0070]
[0071] Where h is half of the plate thickness, k is the wave number, p and q are propagation constants, and satisfy the following equation:
[0072]
[0073]
[0074] In the formula, is the angular frequency, and are the longitudinal wave velocity and the transverse wave velocity in the plate, respectively. By solving the above equations (1) and (2), the dispersion curve of the 6061 aluminum plate with a thickness of 3 mm can be obtained, as shown in Figure 2 shown.
[0075] 102. From the theoretical dispersion curve, determine the theoretical frequency-thickness product and the theoretical resonance peak center frequency of the zero group velocity Lamb wave mode.
[0076] It should be noted that the zero group velocity Lamb wave mode refers to the S1-ZGV mode with zero group velocity.
[0077] The theoretical dispersion curve obtained in step 101 is as follows: Figure 2 As shown in the figure, the interaction between the forward wave of the S1 mode and the backward wave of the S2 mode produces the S1-ZGV mode with a group velocity of zero. Due to the interaction between the forward wave and the backward wave, the acoustic energy is confined near the excitation point. The frequency-thickness product of the S1-ZGV mode in the black box in the figure is 2.877MHzmm, so its theoretical resonance peak center frequency is 0.959MHz.
[0078] 103. Obtain a target excitation signal corresponding to the theoretical resonance peak center frequency.
[0079] It should be noted that the target excitation signal is used to excite the S1-ZGV mode in the pipeline to be tested so as to effectively measure the corrosion thickness. The effective excitation of the S1-ZGV mode is closely related to the selected excitation signal. It can be known in step 102 that the center frequency of the theoretical resonance peak of the S1-ZGV mode is 0.959 MHz. However, in order to make the S1-ZGV mode amplitude higher and better identify the S1-ZGV mode, the target excitation signal in this embodiment is preferably a sinusoidal signal modulated by a three-cycle Hanning window with a center frequency of 0.9 MHz, so that the S1-ZGV frequency is effectively covered with a wider excitation bandwidth, which can more effectively excite the S1-ZGV mode. The time domain and frequency domain of the excitation signal are respectively as shown in FIG. Figure 5 and Figure 6 shown.
[0080] In order to ensure that the target excitation signal can effectively excite the S1-ZGV mode, this step verifies the existence of the S1-ZGV mode in the complete plate structure. The verification steps are as follows:
[0081] S1. Perform a two-dimensional finite element simulation on the pipeline to be inspected to obtain a two-dimensional finite element model.
[0082] It should be noted that, in this embodiment, Abaqus / Explicit CAE software is used to perform a two-dimensional finite element simulation on the pipeline to be inspected to obtain a corresponding two-dimensional finite element model.
[0083] Taking the pipeline structure as a 6061 aluminum tube with a thickness of 3 mm as an example, this embodiment performs a two-dimensional finite element simulation on a complete and defect-free 6061 aluminum plate with a thickness of 3 mm. The two-dimensional component module provided by the Abaqus / Explicit CAE software is used to create a plate structure with a total length of 100 mm and a thickness of 3 mm. Absorption layers are set at both ends of the aluminum plate to avoid boundary reflections at both ends of the aluminum plate and eliminate the existing reflection signals as much as possible. The constructed two-dimensional finite element model is as follows: Figure 4 shown.
[0084] This embodiment obtains a two-dimensional finite element model of a thin-walled pipe (i.e., constructs a two-dimensional finite element model of a thin plate) by establishing a function optimization detection model containing only two variables, which not only simplifies the two-dimensional finite element model of the pipe to be tested and reduces the solution dimension, but also better conforms to the actual detection situation.
[0085] S2. Send a target excitation signal to a preset point source position on the two-dimensional finite element model, and receive a waveform signal reflected from the point source position.
[0086] It should be noted that a point source position is set on the two-dimensional finite element model, and an excitation signal is sent at the point source position and a waveform signal is received after the excitation signal is reflected by the two-dimensional finite element model. Figure 4 As shown, the receiving point and the excitation point are the same point. This embodiment saves simulation time and reduces computing power requirements by adopting point source excitation.
[0087] S3. Calculate the resonance peak center frequency of the waveform signal.
[0088] It should be noted that, in this embodiment, the waveform signal is received at the point source position, and corresponding data processing is performed on the waveform signal to obtain the resonance peak center frequency.
[0089] Wherein, step S3 specifically includes the following sub-steps:
[0090] S31. Calculate the wave packet sound velocity of the waveform signal, and determine the resonant wave in the waveform signal according to the wave packet sound velocity.
[0091] It should be noted that by calculating the wave packet sound velocity of the waveform signal, the mode in the waveform signal can be determined. The waveform signal received at the point source position is as follows: Figure 7As shown in the figure, the sound wave type in the dotted box is a direct wave. According to the wave packet sound velocity, it can be determined that the mode of the direct wave is the A0 mode, and the sound wave type following it is a resonant wave, and its mode is the S1-ZGV mode.
[0092] S32. In the resonance wave, intercept a regional signal within a preset regional range.
[0093] It should be noted that the preset area range is selected according to the actual situation. In this embodiment, the resonant wave in the range of [4, 30] μs is preferably used as the area signal. Figure 7 shown.
[0094] S33, performing fast Fourier transform on the regional signal to obtain the resonance peak center frequency corresponding to the regional signal.
[0095] It should be noted that if Figure 8 As shown in FIG. 1 , after fast Fourier transform of the intercepted regional signal, the transformed signal is analyzed in the frequency domain. It can be seen that a sharp resonance peak appears in the frequency domain. This resonance peak is the resonance peak of the S1-ZGV mode. Figure 8 It can be seen that the center frequency of the resonance peak is 0.953MHz, which is close to the theoretical resonance peak center frequency of the S1-ZGV mode (0.959MHz), and the difference between the two is within the allowable error range, so it is shown that the resonance wave received at the point source position is the S1-ZGV mode, proving that the S1-ZGV mode can be excited in the two-dimensional finite element model by using a three-cycle Hanning window modulated sine signal with a center frequency of 0.9MHz as an excitation signal. Therefore, the three-cycle Hanning window modulated sine signal with a center frequency of 0.9MHz can be used as an excitation signal for measuring the corrosion thickness of the pipeline to be tested, that is, it can be used as a target excitation signal.
[0096] 104. Send a target excitation signal to the pipeline to be detected, and receive a target waveform signal, where the target waveform signal is obtained by reflecting the target excitation signal from the pipeline to be detected.
[0097] It should be noted that, in this embodiment, the target excitation signal is specifically sent to the area to be tested of the pipeline to be tested, wherein the area to be tested can be selected from the pipeline to be tested according to actual conditions.
[0098] When the pipeline to be detected receives the target excitation signal, the target excitation signal propagates in the pipeline to be detected, and after being reflected by the pipeline to be detected, a target waveform signal is formed, and the target waveform signal is reflected to the point source that sends the target excitation signal.
[0099] 105. Determine the resonance peak center frequency of the zero group velocity Lamb wave mode from the target waveform signal.
[0100] It should be noted that, according to step 103, the target excitation signal is used to excite the S1-ZGV mode in the pipeline to be detected, so the obtained target waveform signal contains information of the zero group velocity Lamb wave mode (S1-ZGV mode). Therefore, by intercepting and fast Fourier transforming the target waveform signal, the center frequency of the resonance peak of the zero group velocity Lamb wave mode can be obtained.
[0101] 106. The corrosion thickness of the pipeline to be inspected is calculated based on the theoretical frequency-thickness product and the resonance peak center frequency of the zero group velocity Lamb wave mode.
[0102] It should be noted that the thickness of the pipeline to be inspected is inverted using the theoretical frequency-thickness product and the resonance peak center frequency of the zero group velocity Lamb wave mode to obtain the corresponding corrosion thickness.
[0103] This embodiment obtains the property parameters of the pipeline to be detected, calculates the theoretical dispersion curve of the pipeline to be detected according to the property parameters, thereby obtaining the theoretical dispersion curve of the pipeline to be detected, and provides a technical basis for determining the excitation signal; and determines the theoretical frequency-thickness product and the theoretical resonance peak center frequency of the zero group velocity Lamb wave mode from the theoretical dispersion curve, thereby determining the theoretical frequency-thickness product and the theoretical resonance peak center frequency; obtains the target excitation signal corresponding to the theoretical resonance peak center frequency, thereby determining the target excitation signal, so that the zero group velocity Lamb wave mode can be effectively excited in actual measurement; and sends the target excitation signal to the pipeline to be detected. The target excitation signal is received, and the target waveform signal obtained by reflecting the target excitation signal through the pipeline to be detected is received, which provides effective data support for calculating the corrosion thickness of the pipeline; and the resonance peak center frequency of the zero group velocity Lamb wave mode is determined from the target waveform signal, and the corrosion thickness of the pipeline to be detected is calculated according to the theoretical frequency-thickness product and the resonance peak center frequency of the zero group velocity Lamb wave mode, which effectively realizes the calculation of the corrosion thickness of the pipeline to be detected. Therefore, in practical applications, the thickness of the pipeline to be detected in the erosion environment can be measured in time, the corrosion condition of the pipeline can be monitored, and the safety of pipeline use can be improved.
[0104] See also Figure 3 The embodiment of the present invention provides a method for measuring the corrosion thickness of a pipeline, comprising:
[0105] 201. Obtain attribute parameters of the pipeline to be detected, and calculate a theoretical dispersion curve of the pipeline to be detected according to the attribute parameters.
[0106] 202. From the theoretical dispersion curve, determine the theoretical frequency-thickness product and the theoretical resonance peak center frequency of the zero group velocity Lamb wave mode.
[0107] 203. Obtain a target excitation signal corresponding to the theoretical resonance peak center frequency.
[0108] It should be noted that steps 201-203 may refer to steps 101-103, which will not be repeated here.
[0109] 204. Use array elements of a linear phased array probe to send a target excitation signal to the pipeline to be inspected and receive a target waveform signal; the target waveform signal is obtained by reflecting the target excitation signal through the pipeline to be inspected, wherein the linear phased array probe is provided with a plurality of array elements, and the number of the target waveform signals is consistent with the number of array elements.
[0110] It should be noted that, in this embodiment, a linear phased array probe of a corresponding frequency is selected according to the theoretical resonance peak center frequency. According to the aforementioned steps S1-S5, it can be known that the S1-ZGV mode can be excited by point source excitation. Therefore, in the linear phased array probe used in this embodiment, a number of array elements are provided, each array element is spaced a certain distance apart, and each array element sends a target excitation signal to the pipeline to be detected in turn, and receives a target waveform signal obtained by the pipeline to be detected reflecting the target excitation signal. Therefore, in this step, the number of groups of target waveform signals obtained is consistent with the number of array elements, and multi-point source excitation of a partial area of the pipeline to be detected is realized.
[0111] Specifically, the linear phased array probe has a custom mode and a plane wave imaging mode. After selecting the linear phased array probe, you can select different modes for testing according to actual needs. The following is an instruction for using each mode.
[0112] The first mode is the custom mode. In the custom mode, one or more array elements can be set to send an excitation signal, and one or more array elements can also be set to receive a signal. For example, an array element is set to transmit an excitation signal, and four or eight array elements behind the array element are set to receive the signal, and then the signals received by these four or eight array elements are superimposed to obtain the target waveform signal received this time. After that, the second array element is set to transmit an excitation signal, and the four or eight array elements behind the second array element are used to receive the signal, and the signals received by these four or eight array elements are superimposed to obtain the second received signal, and so on, and the above operations are repeated until the last array element completes the transmission of the excitation signal and obtains several groups of received signals. It can be understood that the superposition of signals from multiple array elements can enhance the signal amplitude of the S1-ZGV mode.
[0113] Next, the resonance wave in the received signal is range-intercepted and then fast Fourier transformed to obtain the frequency domain diagram of the resonance wave. In the frequency domain diagram, a resonance peak close to the theoretical frequency of the S1-ZGV mode can be seen, and the thickness information of the position point is solved by the zero group velocity mode frequency-thickness product formula. And by scanning the received signals of array elements at different positions or the mobile phased array probe, the frequency domain information of the S1-ZGV mode at multiple positions in the pipeline to be tested can be obtained. Finally, the thickness values of different positions obtained are linearly fitted or quadratic curve fitted to invert the thickness size of the corrosion defect in the test area of the pipeline to be tested.
[0114] In addition, in the custom mode, the phase delay of the transmitting array element can also be controlled to control the deflection angle of the wavefront to further enhance the excitation of the S1-ZGV mode and better detect the thickness loss of the pipeline to be tested.
[0115] The second mode is the plane wave imaging mode. In the plane wave imaging mode, a polycrystalline aperture (usually the full aperture of the probe) can be selected. Compared with the first mode, the second mode does not transmit each element separately during transmission, but records basic A-wave data during reception, and each array element receives an A-wave data. Among them, the A-wave data received by the right-end array element is more worthy of attention (assuming that the deflection angle of the PWI is deflected to the right end at this time). Therefore, after the A-wave signal of the right-end array element is range-intercepted, a fast Fourier transform is performed to obtain the frequency domain diagram of the resonance wave, and the thickness information of the position point can be obtained. Then, by scanning the mobile phased array, the thickness size of the corrosion defect in the area of interest can be inverted.
[0116] 205. Determine the resonance peak center frequency of the zero group velocity Lamb wave mode from each group of target waveform signals respectively, and obtain several groups of resonance peak center frequencies of the zero group velocity Lamb wave modes.
[0117] It should be noted that in actual detection, each target waveform signal is processed in the same manner, thereby obtaining the resonance peak center frequency of the zero group velocity Lamb wave mode corresponding to each point source position. Therefore, the number of the resonance peak center frequencies of the zero group velocity Lamb wave mode in this step is consistent with the number of target waveform signals. Among them, the specific processing steps are: intercepting the signal within the preset area range in the target waveform signal, and performing fast Fourier transform on the intercepted signal to obtain the frequency domain diagram of the S1-ZGV mode, and determining the resonance peak center frequency of the zero group velocity Lamb wave mode according to the frequency domain diagram of the S1-ZGV mode.
[0118] 206. The corrosion thickness of the pipeline to be inspected is calculated based on the theoretical frequency-thickness product and the resonance peak center frequency of the zero group velocity Lamb wave mode.
[0119] It should be noted that after obtaining the resonance peak center frequency of the zero group velocity Lamb wave mode, the thickness can be inverted using the theoretical frequency-thickness product and the resonance peak center frequency of the zero group velocity Lamb wave mode to obtain the corresponding thickness value. Step 206 specifically includes the following sub-steps:
[0120] S61, respectively calculating the thickness of a plurality of groups of zero group velocity Lamb wave modes' resonant peak center frequencies and theoretical frequency-thickness products to obtain a plurality of groups of thickness values;
[0121] It should be noted that based on the calculation formula for thickness calculation, thickness inversion is performed on the resonance peak center frequency of the zero group velocity Lamb wave mode and the theoretical frequency-thickness product to obtain the corresponding thickness value.
[0122] In a specific embodiment, the thickness calculation formula is:
[0123]
[0124] in, is the theoretical frequency product, is the resonance peak center frequency of the zero group velocity Lamb wave mode, is the thickness value.
[0125] It can be understood that the corresponding thickness value is obtained by substituting the resonance peak center frequency of the zero group velocity Lamb wave mode and the theoretical frequency-thickness product into formula (5), and there are several groups of resonance peak center frequencies of the zero group velocity Lamb wave mode measured in this embodiment. By substituting several groups of resonance peak center frequencies of the zero group velocity Lamb wave mode into formula (5), several groups of thickness values can be obtained.
[0126] S62 performs fitting on several groups of thickness values to obtain the corrosion thickness of the pipeline to be inspected.
[0127] It should be noted that, in this implementation, by fitting the thickness value of each node, the thickness information of the corrosion defect can be inverted. Therefore, when the linear phased array probe detects the corrosion area of the pipeline to be inspected, the thickness value obtained by fitting is the corrosion thickness of the pipeline to be inspected.
[0128] In another preferred embodiment, when the thickness value of the entire pipeline needs to be checked, the pipeline can be divided into sections according to the length of the mobile phased array probe, and each section can be scanned in turn to obtain the thickness information of the entire pipeline.
[0129] It can be understood that the aforementioned embodiment measures the local thickness on a certain cross section of the pipeline, which describes the process of measuring the phased array probe at a certain position on the pipeline. When it is necessary to view the thickness value of the entire pipeline, the phased array probe matrix can be moved to calculate the thickness value of each regional position in turn, thereby obtaining the overall thickness value of the pipeline and realizing the monitoring of the thickness of the entire pipeline.
[0130] In order to clearly illustrate the effect of the method for measuring the corrosion thickness of a pipeline provided in this embodiment, a simulation application example will be used for illustration below.
[0131] In this simulation application example, a two-dimensional structure with corrosion defects is first constructed. The corrosion defects are obtained by removing grid cells, and the defect size is set to a rounded rectangle with a length of 4 mm, a thickness of 0.5 mm, and a fillet of 0.2 mm, as shown in Figure 2. Fig. 9 As shown. 32 nodes are set above the corrosion defect, named D1-D32. The excitation signal is a sinusoidal signal with a three-cycle Hanning window modulation and a center frequency of 0.9MHz. The 32 nodes excite and receive signals in turn (self-transmitting and self-receiving). In this simulation application example, a linear array point source is used to simulate the phased array probe excitation. In the linear array point source, the number of array elements is set to 32, the array element spacing is 0.3mm, the total length of the linear array is 9.3mm, and the 32 array elements spontaneously transmit target excitation signals and self-receive target waveform signals, so 32 groups of A-wave signals can be obtained. After obtaining 32 groups of A-wave signals, the signal data of [4,30]μs in the A-wave signal is intercepted for fast Fourier transform, and finally the frequency domain diagram of the S1-ZGV mode at each point source position is obtained.
[0132] Taking nodes D4 and D5 as an example, the frequency domain comparison of the received signals of nodes D4 and D5 and the complete model is shown in the figure below: Fig.10 As shown in the figure, it can be seen that due to the presence of corrosion defects, the resonance peak shifts to the right, and as the node is closer to the defect, the right frequency shift of the resonance peak is more obvious, and so on. At this time, the resonance peak frequency of node D4 is 0.9605MHz, and the resonance peak frequency of node D5 is 0.965MHz. The theoretical frequency-thickness product of S1-ZGV is 2.877MHzmm, so the thickness value can be solved by formula (5): =2.9754mm, =2.9608mm.
[0133] The thickness value of each node is calculated and then fitted to invert the thickness information of the corrosion defect. The thickness diagram after fitting is as follows: Fig.11As shown, the inverted defect thickness value range is 0.476mm-0.508mm, and compared with the true thickness, the error range is 1.6%-4.8%. It can be seen that there is only a small error between the corrosion thickness measured by the method provided by the present invention and the true thickness. It can be seen that the method provided by the present invention can complete the inversion of the approximate thickness of the defect, and the measurement accuracy is relatively high.
[0134] In another application example, the technical process of the present invention in practical application is as follows: Fig.12 As shown, the process may include exciting the ZGV mode, detecting the resonance signal, solving the local thickness, and comprehensively scanning the pipeline.
[0135] Specifically, in the present invention, since only a local area on a certain cross section is scanned when a phased array probe is used for scanning, only the dispersion curve of the plate structure needs to be solved in detail, without involving the dispersion characteristics of the pipeline structure. Therefore, the present invention first uses COMSOL Multiphysics commercial software to simulate and analyze the dispersion characteristics to determine the theoretical frequency of the excited zero group velocity Lamb wave (ZGV).
[0136] Secondly, after determining the excitation frequency of the ZGV mode, the present invention intercepts the resonance wave in the received signal and performs fast Fourier transform to observe the resonance peak in the frequency domain and verify whether its center frequency is close to the theoretical frequency, thereby verifying the existence of the ZGV mode in the complete plate structure.
[0137] Once again, after confirming the existence of the ZGV mode, the present invention sets a suitable excitation signal and uses a linear phased array probe to detect the pipeline. The linear phased array probe uses multiple array elements to form an array to form a waveform transmitter, which can change the beam direction according to the monitor's instructions to achieve an overall scan of the structure. That is, the linear phased array probe controls the direction of the signal beam by controlling the phase of the signal emitted by each square array in the array, thereby achieving a comprehensive scan of the pipeline.
[0138] In the present invention, the linear phased array probe will excite and receive signals in sequence (i.e., self-transmitting and self-receiving), intercept the resonant wave in the signal received by each array element, and perform a fast Fourier transform. By observing whether the resonance peak has a frequency shift phenomenon, and extracting its center frequency, it will be compared with the frequency-thickness product of the ZGV mode in the complete plate structure. The thickness at the position of the array element is solved with the help of the zero group velocity mode frequency-thickness product formula (i.e., the thickness calculation formula). By analogy, a corresponding amount of thickness information can be obtained with several array elements, and then the obtained thickness values are fitted, and finally the thickness of the area detected by the phased array probe can be obtained, thereby obtaining local thickness information.
[0139] Finally, the entire pipeline is scanned by manually or automatically moving the phased array probe. At each inspection location, the above steps are performed to obtain comprehensive thickness information of the pipeline.
[0140] Therefore, the method for measuring the corrosion thickness of a pipeline provided by the present invention, combined with the advantages of phased array technology and ZGV mode, can more conveniently reconstruct the thickness in the pipeline and promptly discover corrosion defects to avoid unnecessary losses.
[0141] See also Fig.13 , a device for measuring pipeline corrosion thickness provided by an embodiment of the present invention comprises:
[0142] The first acquisition module 301 is used to acquire the property parameters of the pipeline to be detected, and calculate the theoretical dispersion curve of the pipeline to be detected according to the property parameters;
[0143] A first determination module 302 is used to determine the theoretical frequency-thickness product and the theoretical resonance peak center frequency of the zero group velocity Lamb wave mode from the theoretical dispersion curve;
[0144] The second acquisition module 303 is used to acquire the target excitation signal corresponding to the theoretical resonance peak center frequency;
[0145] The excitation module 304 is used to send a target excitation signal to the pipeline to be detected and receive a target waveform signal, where the target waveform signal is obtained by reflecting the target excitation signal from the pipeline to be detected;
[0146] The second determination module 305 is used to determine the resonance peak center frequency of the zero group velocity Lamb wave mode from the target waveform signal;
[0147] The calculation module 306 is used to calculate the corrosion thickness of the pipeline to be inspected according to the theoretical frequency-thickness product and the resonance peak center frequency of the zero group velocity Lamb wave mode.
[0148] In a specific embodiment, the excitation module 304 is specifically used to use a linear phased array probe to send a target excitation signal to the pipeline to be inspected, and receive a target waveform signal;
[0149] The linear phased array probe is provided with a number of array elements, and the number of target waveform signals is consistent with the number of array elements.
[0150] In a specific embodiment, the second determination module 305 is specifically used to determine the resonance peak center frequency of the zero group velocity Lamb wave mode from each group of target waveform signals, and obtain several groups of resonance peak center frequencies of the zero group velocity Lamb wave modes.
[0151] In a specific embodiment, the calculation module 306 includes:
[0152] The thickness value calculation subunit is used to calculate the thickness of a plurality of groups of zero group velocity Lamb wave modes by using the resonance peak center frequency and the theoretical frequency-thickness product to obtain a plurality of groups of thickness values;
[0153] The fitting subunit is used to fit several groups of thickness values to obtain the corrosion thickness of the pipeline to be inspected.
[0154] See also Fig.14 The present invention also provides a system for measuring the corrosion thickness of a pipeline, comprising: a linear array phased array probe, a phased array board, and a controller; the phased array board is connected to the linear array phased array probe, and the controller is respectively connected to the phased array board and the linear array phased array probe, for executing the method of any of the above embodiments.
[0155] It should be noted that the controller in this embodiment may be a computer.
[0156] Those skilled in the art can clearly understand that, for the convenience and brevity of description, the specific working processes of the systems, devices and units described above can refer to the corresponding processes in the aforementioned method embodiments and will not be repeated here.
[0157] In the several embodiments provided in the present application, it should be understood that the disclosed systems, devices and methods can be implemented in other ways. For example, the device embodiments described above are only schematic. For example, the division of units is only a logical function division. There may be other division methods in actual implementation, such as multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed. Another point is that the mutual coupling or direct coupling or communication connection shown or discussed can be an indirect coupling or communication connection through some interfaces, devices or units, which can be electrical, mechanical or other forms.
[0158] The units described as separate components may or may not be physically separated, and the components shown as units may or may not be physical units, that is, they may be located in one place or distributed on multiple network units. Some or all of the units may be selected according to actual needs to achieve the purpose of the solution of this embodiment.
[0159] In addition, each functional unit in each embodiment of the present invention may be integrated into one processing unit, or each functional unit may be physically separate, or two or more functional units may be integrated into one processing unit. The above integrated unit may be implemented in the form of hardware or in the form of software functional units.
[0160] If the integrated unit is implemented in the form of a software functional unit and sold or used as an independent product, it can be stored in a computer-readable storage medium. Based on this understanding, the technical solution of the present invention is essentially or the part that contributes to the prior art or all or part of the technical solution can be embodied in the form of a software product. The computer software product is stored in a storage medium, including several instructions to enable a computer device (which can be a personal computer, server, or network device, etc.) to perform all or part of the steps of the method described in each embodiment of the present invention. The aforementioned storage medium includes: U disk, mobile hard disk, read-only memory (ROM, Read-Only Memory), random access memory (RAM, Random Access Memory), disk or optical disk and other media that can store program codes.
[0161] The terms "first", "second", "third", "fourth", etc. (if any) in the specification of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0162] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for measuring the corrosion thickness of a pipeline, characterized in that: include: Acquiring property parameters of the pipeline to be detected, and calculating a theoretical dispersion curve of the pipeline to be detected according to the property parameters; Determining the theoretical frequency-thickness product and the theoretical resonance peak center frequency of the zero group velocity Lamb wave mode from the theoretical dispersion curve; Obtaining a target excitation signal corresponding to the theoretical resonance peak center frequency; Sending a target excitation signal to the pipeline to be detected, and receiving a target waveform signal, wherein the target waveform signal is obtained by reflecting the target excitation signal through the pipeline to be detected; Determining the resonance peak center frequency of the zero group velocity Lamb wave mode from the target waveform signal; The corrosion thickness of the pipeline to be inspected is calculated based on the theoretical frequency-thickness product and the resonance peak center frequency of the zero group velocity Lamb wave mode.
2. The measuring method according to claim 1, characterized in that: Sending a target excitation signal to the pipeline to be inspected and receiving a target waveform signal specifically includes: Using array elements of a linear phased array probe, a target excitation signal is sent to the pipeline to be inspected, and a target waveform signal is received; Wherein, the linear phased array probe is provided with a plurality of array elements, and the number of the target waveform signals is consistent with the number of the array elements.
3. The measuring method according to claim 2, characterized in that: Determining the resonance peak center frequency of the zero group velocity Lamb wave mode from the target waveform signal specifically includes: The resonance peak center frequency of the zero group velocity Lamb wave mode is determined from each group of the target waveform signals respectively, and a plurality of groups of resonance peak center frequencies of the zero group velocity Lamb wave modes are obtained.
4. The measuring method according to claim 3, characterized in that: The step of calculating the corrosion thickness of the pipeline to be inspected according to the theoretical frequency-thickness product and the resonance peak center frequency of the zero group velocity Lamb wave mode specifically includes: Performing thickness calculations on the resonance peak center frequencies of several groups of zero group velocity Lamb wave modes and the theoretical frequency-thickness product to obtain several groups of thickness values; Fitting is performed on several groups of thickness values to obtain the corrosion thickness of the pipeline to be inspected.
5. The measuring method according to claim 4, characterized in that: The calculation formula for the thickness calculation is: in, is the theoretical frequency product, is the resonance peak center frequency of the zero group velocity Lamb wave mode, is the thickness value.
6. A device for measuring pipeline corrosion thickness, characterized in that: include: A first acquisition module is used to acquire attribute parameters of the pipeline to be detected, and calculate a theoretical dispersion curve of the pipeline to be detected according to the attribute parameters; A first determination module is used to determine the theoretical frequency-thickness product and the theoretical resonance peak center frequency of the zero group velocity Lamb wave mode from the theoretical dispersion curve; A second acquisition module is used to acquire a target excitation signal corresponding to the theoretical resonance peak center frequency; An excitation module, used for sending a target excitation signal to the pipeline to be detected and receiving a target waveform signal, wherein the target waveform signal is obtained by reflecting the target excitation signal through the pipeline to be detected; A second determination module is used to determine the resonance peak center frequency of the zero group velocity Lamb wave mode from the target waveform signal; The calculation module is used to calculate the corrosion thickness of the pipeline to be detected according to the theoretical frequency-thickness product and the resonance peak center frequency of the zero group velocity Lamb wave mode.
7. The device according to claim 6, characterized in that The excitation module is specifically used to use a linear phased array probe to send a target excitation signal to the pipeline to be inspected and receive a target waveform signal; wherein the linear phased array probe is provided with a plurality of array elements, and the number of the target waveform signals is consistent with the number of the array elements.
8. The device according to claim 7, characterized in that The second determination module is specifically used to determine the resonance peak center frequency of the zero group velocity Lamb wave mode from each group of the target waveform signals, and obtain several groups of resonance peak center frequencies of the zero group velocity Lamb wave modes.
9. The device according to claim 8, characterized in that The calculation module comprises: A thickness value calculation subunit is used to calculate the thickness of a plurality of groups of resonance peak center frequencies of the zero group velocity Lamb wave modes and the theoretical frequency-thickness product to obtain a plurality of groups of thickness values; The fitting subunit is used to fit several groups of thickness values to obtain the corrosion thickness of the pipeline to be detected.
10. A system for measuring corrosion thickness of a pipeline, characterized in that: include: A linear array phased array probe, a phased array board, and a controller; the phased array board is connected to the linear array phased array probe, and the controller is respectively connected to the phased array board and the linear array phased array probe, for executing the measurement method according to any one of claims 1 to 5.
Citation Information
Patent Citations
Method for detecting thickness reduction of heated surface tube of boiler
CN107632068A
Sheet stress measurement method and sheet stress measurement system
CN110243521A