Evaluation method for aging damage degree of low alloy steel in long-term service

The relationship established through low-cycle fatigue testing and the least squares method solves the problem of aging damage assessment of low-alloy steel, achieves a rapid and accurate assessment of the degree of aging damage of low-alloy steel, improves the assessment efficiency, and ensures the reliability of nuclear power plant materials. Security.

CN118730772APending Publication Date: 2024-10-01EAST CHINA UNIV OF SCI & TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410718787.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing technology makes it difficult to effectively evaluate the degree of aging damage of low-alloy steel under long-term high temperature and radiation environments, resulting in insignificant changes in material properties, making it difficult to conduct accurate damage assessments, and affecting the safety of nuclear power plants.

Method used

By conducting stress- or strain-controlled low-cycle fatigue tests on low-alloy steel specimens with different aging times, the strain/stress cycle response curve is obtained, the relative softening factor is calculated, and the relationship between the relative softening factor and aging damage parameters is established through the least squares method. Formula to evaluate the aging damage state of materials.

Benefits of technology

This method can quickly and accurately assess the degree of aging damage of low alloy steel, save time and cost, solve the problem of damage monitoring of long-life service parts, improve the efficiency of assessment, and verify its reliability and reliability under different working conditions. accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118730772A_ABST
    Figure CN118730772A_ABST
Patent Text Reader

Abstract

The invention discloses a method for evaluating the aging damage degree of low alloy steel in long-term service, which comprises the following steps of: S1, taking a plurality of samples with different aging durations, carrying out stress or strain controlled low-cycle fatigue test on each sample to obtain a strain / stress cycle response curve, linearly fitting the slope of a strain amplitude / stress amplitude stable increasing stage, and calculating the aging damage degree of the low alloy steel in the strain amplitude / stress amplitude stable increasing stage; calculating a relative softening factor; s2, determining aging damage parameters corresponding to different aging durations according to the difference between the service lives of the samples with the aging durations being zero and the service lives of the samples with the aging durations being greater than zero; s3, establishing a relational expression between the relative softening factor and the aging damage parameter; and S4, calculating relative softening factors of the material in the aging damage state under other working conditions, calculating corresponding aging damage parameters according to the relational expression, and evaluating the aging damage state. According to the evaluation method, the number of required fatigue cycles is small, the number of parameters is small, calculation is simple, and evaluation of the aging damage state of the material under different bearing working conditions can be achieved more quickly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal material detection, and in particular relates to a method for evaluating the degree of aging damage of low alloy steel after long-term service. Background Art

[0002] Low alloy steel refers to alloy steel with a total alloying element content of less than 5%. It is widely used in nuclear power plant reactor pressure vessels due to its good high temperature resistance and radiation resistance. The reactor pressure vessel is a closed container that houses the nuclear reactor and withstands its huge operating pressure. Its quality and life are directly related to the safety of the nuclear power plant. However, nuclear reactors usually operate at a temperature of 270-340°C. The material will age and become brittle after long-term service in a high temperature and radiation environment, which seriously affects the material performance. During the long-term aging process, the chemical-mechanical coupling factors cause changes in the microstructure and precipitates of the material, which in turn manifests itself in the macroscopic properties as increased strength, decreased ductility and impact toughness, etc., causing potential safety hazards.

[0003] In order to better manage the long-life service damage state of materials, it is necessary to evaluate the degree of aging damage. In the prior art, static methods are mainly used to evaluate material aging, such as hardness method and thermoelectric potential method. Among them, the hardness method is mainly used for duplex stainless steel. Since its hardness is sensitive to aging, the relationship between it and the low-cycle fatigue life can be established according to the hardness change of the aged material, thereby realizing the prediction of the low-cycle fatigue life under different aging times; the thermoelectric potential method mainly establishes the relationship between the material thermoelectric potential and the room temperature impact value, and then predicts the impact work of the aged material according to the thermoelectric potential measured in the test. However, for low-alloy steel materials, even under long-term aging, the changes in their hardness or impact work are not obvious, which brings difficulties to the aging damage evaluation of low-alloy steel. Summary of the invention

[0004] The present invention is made to solve the above-mentioned problem, and its purpose is to provide a method for evaluating the degree of aging damage of low alloy steel after long-term service.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A method for evaluating the degree of aging damage of low alloy steel during long-term service, comprising:

[0007] Step S1: taking a plurality of low alloy steel samples with different aging times and the aging time of one of the samples is zero, and carrying out a stress or strain controlled low cycle fatigue test on each sample under a certain working condition, and obtaining a corresponding strain / stress cyclic response curve, and calculating the corresponding relative softening factor by linearly fitting the slope of the stable growth stage of the strain amplitude / stress amplitude;

[0008] Step S2: Determine aging damage parameters corresponding to different aging times according to the life difference between samples with zero aging time and samples with greater than zero aging time under the same working conditions;

[0009] Step S3: establishing a relationship between the relative softening factor and the aging damage parameter by the least square method;

[0010] Step S4: Repeat step S1 to calculate the relative softening factor of the aging damage state of the material under other working conditions, calculate the corresponding aging damage parameter according to the relationship determined in step S3, and evaluate the aging damage state of the material under each working condition.

[0011] Furthermore, step S1 includes the following sub-steps:

[0012] Step S1-1: setting a suitable heat aging temperature under laboratory conditions according to the actual working environment of the material, and performing heat aging accelerated tests with different heat aging times on multiple samples;

[0013] Step S1-2: performing stress / strain controlled low cycle fatigue tests on each sample, obtaining the evolution law of strain amplitude / stress amplitude with the number of cycles, and performing linear fitting on the slope of the stable growth stage of strain amplitude / stress amplitude on the strain / stress cycle response curve;

[0014] Step S1-3: Based on the slope obtained by linear fitting, the relative softening factor RSF corresponding to the material at different heat aging times is calculated according to the following formula:

[0015]

[0016] Among them, K T K is the softening slope of a sample with a heat aging time of T and T>0 in the stable growth stage of strain amplitude / stress amplitude on the strain / stress cycle response curve; 0 It is the softening slope of the sample with zero thermal aging time in the stable growth stage of strain amplitude / stress amplitude on the strain / stress cyclic response curve.

[0017] Preferably, the number of nodes of the heat aging time is greater than or equal to 4, that is, at least 4 samples are taken corresponding to different heat aging times.

[0018] Further, in step S2, the aging damage parameter ADP corresponding to the samples with different thermal aging time is calculated according to the following formula:

[0019]

[0020] Among them, N T is the fatigue life of the specimen with thermal aging time T; N 0 is the fatigue life of the specimen with zero thermal aging time.

[0021] Furthermore, in step S3, the relational expression is in the form of:

[0022] ADP=αRSF β

[0023] Where α and β are material constants.

[0024] Furthermore, in step S3, the relative softening factor RSF and the heat aging damage parameter ADP corresponding to different heat aging times are input into the Origin software, and the material constants α and β are determined by fitting through the least squares method to obtain the relationship.

[0025] Furthermore, step S4 includes the following sub-steps:

[0026] Step S4-1: Change the load size, repeat step S1, and calculate the relative softening factor RSF of the material under other working conditions;

[0027] Step S4-2: Substitute the relative softening factor RSF calculated in step S4-1 into the relationship established in step S3, and further calculate the corresponding aging damage parameter ADP;

[0028] Step S4-3: Compare the aging damage parameter ADP corresponding to each working condition with the damage safety threshold A of the low alloy steel after aging required under the design conditions. 0 For comparison, when ADP≤A 0 When ADP>A 0 The material is judged to be unsafe.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. The method for evaluating the degree of aging damage of low alloy steel in long-term service of the present invention only requires a small number of fatigue cycles, which can effectively save time and cost and improve evaluation efficiency.

[0031] 2. The method for evaluating the degree of aging damage of low-alloy steel in long-term service of the present invention obtains the slope of the stable stage through linear fitting, calculates the relative softening factor based on the slope, and then predicts the aging damage parameters. It has fewer parameters and simple calculations, and can quickly realize the evaluation of the aging damage state of materials under different load conditions, thus solving the problem of damage monitoring of long-life service components. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a flow chart of the evaluation method of the degree of aging damage of low alloy steel in long-term service;

[0033] Figure 2It is the relationship between the strain amplitude and the number of cycles corresponding to different heat aging times under the condition of 10±420MPa;

[0034] Figure 3 It is a comparison chart of the calculated value and predicted value of the thermal aging damage parameter test of the material under different working conditions;

[0035] Figure 4 This is a comparison chart of the measured values ​​and predicted values ​​of fatigue life tests of materials under different working conditions. DETAILED DESCRIPTION

[0036] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the following embodiments and the accompanying drawings specifically illustrate the evaluation method for the degree of aging damage of low-alloy steel in long-term service of the present invention.

[0037] The inventors observed in the low-cycle fatigue test of low-alloy steel materials that the strain amplitude / stress amplitude of the cyclic response is more sensitive to aging damage, and there are obvious differences in the cyclic response of materials with different aging times under the same working conditions. Therefore, establishing an evaluation method for the degree of aging damage through the cyclic response curve can solve the problem of evaluating the long-term aging damage of low-alloy steel.

[0038] like Figure 1 As shown, the present invention provides a method for evaluating the degree of aging damage of low alloy steel in long-term service, comprising:

[0039] Step S1: taking a plurality of low alloy steel samples with different aging times and the aging time of one of the samples is zero, and carrying out a stress or strain controlled low cycle fatigue test on each sample under a certain working condition (load), obtaining a corresponding strain / stress cyclic response curve, and calculating the corresponding relative softening factor by linearly fitting the slope of the stable growth stage of the strain amplitude / stress amplitude;

[0040] Step S2: Determine aging damage parameters corresponding to different aging times according to the life difference between samples with zero aging time and samples with greater than zero aging time under the same working conditions;

[0041] Step S3: establishing a relationship between the relative softening factor and the aging damage parameter by the least square method;

[0042] Step S4: Repeat step S1 to calculate the relative softening factor of the aging damage state of the material under other working conditions, calculate the corresponding aging damage parameter according to the relationship determined in step S3, and evaluate the aging damage state of the material under each working condition.

[0043] In this embodiment, thermal aging damage assessment is taken as an example, and only the service conditions of the material in a high temperature environment are considered.

[0044] Specifically, step S1 also includes the following sub-steps:

[0045] Step S1-1: setting a suitable heat aging temperature under laboratory conditions according to the actual working environment of the material, and performing heat aging accelerated tests with different heat aging times on multiple low alloy steel samples;

[0046] Preferably, the number of heat aging time nodes is greater than or equal to 4, that is, at least 4 samples are taken corresponding to different heat aging times.

[0047] Step S1-2: performing stress / strain controlled low cycle fatigue tests on each sample, obtaining the evolution law of strain amplitude / stress amplitude with the number of cycles, and performing linear fitting on the slope of the stable growth stage of strain amplitude / stress amplitude on the strain / stress cycle response curve;

[0048] Step S1-3: Based on the slope obtained by linear fitting, the relative softening factor RSF corresponding to the material at different heat aging times is calculated according to the following formula:

[0049]

[0050] Among them, K T K is the softening slope of a sample with a heat aging time of T (T>0) in the stable growth stage of strain amplitude / stress amplitude on the strain / stress cycle response curve; 0 It is the softening slope of the sample with zero thermal aging time (i.e., unaged) in the stable growth stage of strain amplitude / stress amplitude on the strain / stress cycle response curve. The relative softening factor RSF reflects the softening degree of low alloy steel after aging compared with the unaged state under the same working conditions.

[0051] Furthermore, since the fatigue life of low alloy steel is shortened due to aging, in step S2, the aging damage parameter ADP corresponding to each sample with different thermal aging time can be calculated according to the following formula:

[0052]

[0053] Among them, N T is the fatigue life of the specimen with thermal aging time T (T>0); N 0 It is the fatigue life of the specimen with zero thermal aging time (i.e. no aging).

[0054] The aging damage parameter ADP reflects the degree of damage caused by aging to fatigue life. The ADP value is between 0 and 1: when ADP = 0, it means that the effect of aging on the fatigue life of the material is 0, that is, the original material; when ADP = 1, it means that the effect of aging on the fatigue life of the material reaches 100%, and the specimen cannot withstand cyclic loads.

[0055] Furthermore, in step S3, a relationship between the relative softening factor RSF and the aging damage parameter ADP is established in the following form:

[0056] ADP=αRSF β

[0057] Among them, α and β are material constants, which are related to the properties of the low-alloy steel material being tested. There are also differences in the α and β values ​​corresponding to different types of low-alloy steels.

[0058] Furthermore, step S4 also includes the following sub-steps:

[0059] Step S4-1: Change the load size, repeat step S1, and calculate the relative softening factor RSF of the material under other working conditions;

[0060] Step S4-2: Substitute the relative softening factor RSF calculated in step S4-1 into the relationship established in step S3, and further calculate the corresponding aging damage parameter ADP;

[0061] Step S4-3: Compare the aging damage parameter ADP corresponding to each working condition with the damage safety threshold A of the low alloy steel after aging required under the design conditions. 0 For comparison, when ADP≤A 0 When ADP>A 0 The material is judged to be unsafe.

[0062] The implementation process of the present invention is described below with reference to specific examples.

[0063] Step S1: For a certain Mn-Ni-Mo low alloy reactor pressure vessel steel in service, an accelerated heat aging test is carried out at 480°C, and the heat aging time is 0h, 1000h, 5000h and 10000h respectively. A stress-controlled ratchet fatigue test is carried out at a high temperature of 350°C for samples that have not been heat aged (heat aging time is 0h) and other samples after heat aging (aging time is greater than zero). The working condition (load) is 10±420MPa, where 10MPa is the average stress and 420MPa is the stress amplitude. The evolution curve of the strain amplitude with the number of cycles is obtained, such as Figure 2 As shown, it can be seen that the cyclic evolution under different heat aging durations can be basically divided into three stages: initial cyclic hardening (the curve drops rapidly), then cyclic softening (the curve rises steadily), and finally accelerated softening (the curve rises rapidly). The second stage, that is, the stable stage of cyclic softening, occupies the main part of the material life. At the same time, with the increase of heat aging time, the degree of softening of the material is greater, that is, the corresponding slope of the second stage is larger, and the fatigue life is reduced. By linearly fitting the slope of the second stage under different heat aging durations, according to The relative softening factor RSF of the material under different thermal aging times is calculated.

[0064] Step S2: Calculate the thermal aging damage parameter ADP corresponding to different thermal aging times according to the fatigue life of the material under different thermal aging times. Where N 0 N when T = 0 T The results are shown in the table below.

[0065] Aging time T Relative softening factor RSF <![CDATA[Lifespan N T > Thermal aging damage parameter ADP 0h 0 5434 0 1000h 3.217 2335 0.570 5000h 12.684 1760 0.676 10000h 31.763 941 0.826

[0066] Step S3: Input the relative softening factor RSF and thermal aging damage parameter ADP corresponding to different thermal aging durations into the Origin software, and determine the material constants α and β by fitting using the least squares method to obtain the relationship: ADP = 0.484RSF 0.163 .

[0067] Step S4: Ratchet fatigue tests are performed on other different service conditions at the same heat aging temperature to obtain the slope of the second stage of the cyclic response (strain amplitude stable growth stage), calculate the corresponding relative softening factor RSF, and then substitute it into the relationship ADP=0.484RSF in step S3 0.163 The thermal aging damage parameter ADP is calculated in .

[0068] In order to verify the reliability of the above calculation formula under different load conditions, the thermal aging damage parameter ADP (i.e., "predicted ADP") calculated according to the relationship in step S4 is used. Reversely calculate the fatigue life (i.e., "predicted life"). Compare the "predicted ADP" obtained by this method with the ADP value (i.e., "experimentally calculated ADP") calculated based on the fatigue life actually measured by the fatigue test (i.e., "experimentally measured life"), and compare the "predicted life" reversely calculated based on the "predicted ADP" with the "experimentally measured life", such as Figure 3 , 4 As shown, it can be seen that the horizontal axis corresponding to each working condition is the experimental calculated ADP / experimental measured life, and the vertical axis is the predicted ADP / predicted life. The coordinate points all fall near the straight line with a slope of 1, which verifies the reliability and accuracy of this method.

[0069] Finally, the test material is subjected to a thermal aging safety assessment, and the aging damage parameter ADP is compared with the damage safety threshold A0 of the low alloy steel after aging required under the design conditions. In this embodiment, the design requires that the damage safety threshold A0 of the material under various load conditions is 0.4. Figure 3It can be seen that the ADP corresponding to each working condition is greater than 0.4. Therefore, the tested material will suffer greater thermal aging damage if it is in service under high temperature conditions for a long time. The material is judged to be unsafe and not suitable for continued service and should be replaced in time.

[0070] In summary, the method for evaluating the degree of aging damage of low-alloy steel in long-term service of the present invention only needs to pass through a small number of fatigue cycles (i.e., a few cycles after the cyclic response enters the stable stage), and obtain the slope of the stable stage of cyclic softening evolution through linear fitting, and calculate the relative softening factor based on the slope, and then predict the aging damage parameters, so as to realize the evaluation of the aging damage state of the material under different load conditions, and solve the problem of damage monitoring of long-life service components. This method has the advantages of fewer parameters and simple calculations, which can effectively save time and cost and improve evaluation efficiency. In addition, this method is not only applicable to the damage assessment of thermal aging, but also to aging damage caused by other related factors, and has a high value of promotion and application.

[0071] The above-mentioned embodiments are preferred examples of the present invention and are not intended to limit the protection scope of the present invention.

Claims

1. A method for evaluating the degree of aging damage of low alloy steel after long-term service, characterized in that: include: Step S1: taking a plurality of low alloy steel samples with different aging times and the aging time of one of the samples is zero, and carrying out a stress or strain controlled low cycle fatigue test on each sample under a certain working condition, and obtaining a corresponding strain / stress cyclic response curve, and calculating the corresponding relative softening factor by linearly fitting the slope of the stable growth stage of the strain amplitude / stress amplitude; Step S2: Determine aging damage parameters corresponding to different aging times according to the life difference between samples with zero aging time and samples with greater than zero aging time under the same working conditions; Step S3: establishing a relationship between the relative softening factor and the aging damage parameter by the least square method; Step S4: Repeat step S1 to calculate the relative softening factor of the aging damage state of the material under other working conditions, calculate the corresponding aging damage parameter according to the relationship determined in step S3, and evaluate the aging damage state of the material under each working condition.

2. The method for evaluating the degree of long-term service aging damage of low alloy steel according to claim 1, characterized in that: The step S1 includes the following sub-steps: Step S1-1: setting a suitable heat aging temperature under laboratory conditions according to the actual working environment of the material, and performing heat aging accelerated tests with different heat aging times on a plurality of the samples; Step S1-2: performing stress / strain controlled low cycle fatigue tests on each sample, obtaining the evolution law of strain amplitude / stress amplitude with the number of cycles, and performing linear fitting on the slope of the stable growth stage of strain amplitude / stress amplitude on the strain / stress cycle response curve; Step S1-3: Based on the slope obtained by linear fitting, the relative softening factor RSF corresponding to the material under different heat aging times is calculated according to the following formula: Among them, K T It is the softening slope of a sample with a heat aging time of T and T>0 during the stable growth stage of strain amplitude / stress amplitude on the strain / stress cyclic response curve; K0 is the softening slope of a sample with a heat aging time of zero during the stable growth stage of strain amplitude / stress amplitude on the strain / stress cyclic response curve.

3. The method for evaluating the degree of long-term service aging damage of low alloy steel according to claim 2, characterized in that: Preferably, the number of nodes of the heat aging time is greater than or equal to 4, that is, at least 4 samples are taken to correspond to different heat aging time.

4. The method for evaluating the degree of long-term service aging damage of low alloy steel according to claim 1, characterized in that: In step S2, the aging damage parameter ADP corresponding to the samples with different thermal aging times is calculated according to the following formula: Among them, N T is the fatigue life of the specimen with thermal aging time T; N0 is the fatigue life of the specimen with thermal aging time zero.

5. The method for evaluating the degree of long-term service aging damage of low alloy steel according to claim 1, characterized in that: In step S3, the relational expression is in the form of: ADP=αRSF β Where α and β are material constants.

6. The method for evaluating the degree of long-term service aging damage of low alloy steel according to claim 5, characterized in that: In step S3, the relative softening factor RSF and the heat aging damage parameter ADP corresponding to different heat aging times are input into the Origin software, and the material constants α and β are determined by fitting using the least squares method to obtain the relationship.

7. The method for evaluating the degree of long-term service aging damage of low alloy steel according to claim 1, characterized in that: The step S4 includes the following sub-steps: Step S4-1: Change the load size, repeat step S1, and calculate the relative softening factor RSF of the material under other working conditions; Step S4-2: Substituting the relative softening factor RSF calculated in step S4-1 into the relationship established in step S3, and further calculating the corresponding aging damage parameter ADP; Step S4-3: Compare the aging damage parameter ADP corresponding to each working condition with the damage safety threshold A0 of low alloy steel after aging required under design conditions. When ADP≤A0, the material is judged to be safe; when ADP>A0, the material is judged to be unsafe.

Citation Information

Cited By

  • Method, device and equipment for predicting and evaluating thermal aging damage of dual-phase steel

    CN119170171A

  • Quantitative design method for resisting unsteady-state damage of bearing

    CN119862350A