Light gypsum mortar water retention capacity detection system
Through the lightweight gypsum mortar water retention performance detection system, the super-absorbent filter combined with the detection steps of lightweight gypsum mortar solves the problems of high equipment cost and troublesome operation in the existing technology, and achieves high-stability water retention performance detection, especially Lightweight gypsum mortar for highly effective water retaining agents.
Patent Information
- Application Number
- CN202410847076.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The equipment used to detect the water retention performance of lightweight gypsum mortar in the prior art is high in cost and troublesome to operate, and the measurement results have poor stability. This is especially suitable for lightweight gypsum mortar with high-efficiency water-retaining agents. The difference between the before and after measurement results is large, resulting in invalidity. test.
A lightweight gypsum mortar water retention performance testing system is used, including a circular trough, a sampling bucket, a scraper, a counterweight, a circular metal filter, a circular super-absorbent filter cake, a trough cover, a balance, a sample tray and an oven. The super-absorbent filter cake is combined with lightweight gypsum mortar for a water retention test. The measurement steps include weighing, pouring, covering, standing and drying to calculate the water retention rate, which avoids the use of vacuum pumps and filtration operations.
The system is simple to operate, has high stability of measurement results, and good consistency of measurement results. There is no need to purchase a vacuum pump. It is especially suitable for testing the water retention performance of lightweight gypsum mortar, which significantly improves the reliability and efficiency of testing.
Smart Images

Figure CN118730799A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a light gypsum mortar water retention performance detection system, belonging to the technical field of gypsum mortar detection. Background Art
[0002] Lightweight gypsum mortar is a newer, more environmentally friendly and more economical product that replaces cement mortar. It is mainly used for wall leveling in areas indoors that are not often in contact with water. It has the strength of cement and is healthier and more environmentally friendly than cement. It is also very common in interior wall plastering of buildings with high requirements due to its thermal insulation, sound insulation and thick layer construction characteristics.
[0003] Lightweight gypsum mortar is a green and environmentally friendly building material. It usually uses desulfurization gypsum produced in the flue gas desulfurization process of power plants as the main raw material. The product is lightweight, heat-insulating, fire-resistant, has a small shrinkage coefficient, has strong adhesion to the substrate, and does not hollow or crack. It is an excellent performance interior wall leveling and plastering material.
[0004] During the production process of lightweight gypsum mortar, water retaining agent needs to be added to increase its viscosity and water retention. If too much water retaining agent is added, not only will the cost increase, but the viscosity of the lightweight gypsum mortar will be too high, which will make it difficult to construct the product on site. If the amount of water retaining agent is too low, the product will lose water excessively before setting, resulting in low product strength and powdery surface. Therefore, it is very important to determine the water retention performance (water retention rate) of lightweight gypsum mortar.
[0005] At present, the determination of gypsum water retention rate is mainly carried out in accordance with the industry standard "Plastering Gypsum" (JC / T517-2004) and GB / T28627-2012 "Plastering Gypsum" for the determination of the water retention rate of plastering gypsum to evaluate the water retention rate of plastering gypsum. It can also be used to test the water retention rate of cement and mortar.
[0006] However, the equipment used to detect the water retention rate in the method in the above standard requires a vacuum pump, etc., which not only has high equipment cost but also is cumbersome to operate. Especially for lightweight gypsum mortar with some high-efficiency water-retaining agents added, the stability of the measurement results is poor, and invalid tests often occur due to large differences between the two measurement results.
[0007] Based on this, the present invention is proposed. Summary of the invention
[0008] In view of the shortcomings of the prior art, the present invention provides a lightweight gypsum mortar water retention performance detection system, and the specific technical scheme is as follows:
[0009] A light gypsum mortar water retention performance testing system comprises a circular trough, a sampling bucket, a scraper, a counterweight, a circular metal filter screen, a circular super absorbent filter cake, a trough cover adapted to the circular trough, a balance, a sample tray, and an oven;
[0010] The sampling bucket has a bucket cover, and the sampling bucket is used to sample the lightweight gypsum mortar to be tested on site;
[0011] The diameter of the metal filter screen is larger than the inner diameter of the circular groove, and the diameter of the super absorbent filter cake is larger than the inner diameter of the circular groove.
[0012] As a further improvement, the method for testing the water retention performance of lightweight gypsum mortar using the lightweight gypsum mortar water retention performance testing system comprises the following steps:
[0013] Step 1, using a balance to weigh the mass of the circular tank as m1; using a balance to weigh the mass of the super absorbent filter cake as m2;
[0014] Step 2, open the lid of the sampling bucket, use the sampling bucket to sample the lightweight gypsum mortar to be tested on site, and cover the lid of the sampling bucket after sampling to complete the sampling; then pour the lightweight gypsum mortar from the sampling bucket into the inside of the circular groove and fill it, use a scraper to scrape it flat at the notch of the circular groove and wipe off the excess lightweight gypsum mortar, and clean the outer wall and notch of the circular groove;
[0015] Step 3, weigh the total mass of the circular trough and the lightweight gypsum mortar inside it as m3;
[0016] Step 4, cover the notch of the circular tank with a metal filter, then cover the super absorbent filter cake on the metal filter, then cover the tank cover on the super absorbent filter cake, and then cover the tank cover with a counterweight, after standing for 2 to 5 minutes, remove the counterweight, tank cover and the super absorbent filter cake after water absorption;
[0017] Step 5, weighing the mass of the super absorbent filter cake after absorbing water as m4;
[0018] Step 6, weigh the mass of the sample pan as m5; open the lid of the sampling barrel, pour the lightweight gypsum mortar in the sampling barrel into the sample pan, weigh the total mass of the sample pan and the lightweight gypsum mortar inside as m6; dry the sample pan and the lightweight gypsum mortar inside in an oven at 105±3°C to constant weight, and weigh the total mass of the dried sample pan and the lightweight gypsum mortar inside as m7;
[0019] The moisture content of lightweight gypsum mortar is θm, θm = [(m6-m5)-(m7-m5)] / (m6-m5);
[0020] The water retention rate of lightweight gypsum mortar is R, R = 1-(m4-m2) / [θm·(m3-m1)].
[0021] As a further improvement, the mesh size of the metal filter is 270 to 400 meshes.
[0022] As a further improvement, the inner diameter of the circular groove is 100-200 mm, and the groove depth of the circular groove is 25-35 mm.
[0023] As a further improvement, the circular groove is an iron groove, the groove cover is a magnet, and the metal filter is an iron filter.
[0024] As a further improvement, in step 4, when a counterweight is not used to cover the top of the tank cover, after the tank cover is covered on the top of the super absorbent filter cake, the circular tank and the tank cover are turned upside down, and then after standing for 2 to 5 minutes, the tank cover and the super absorbent filter cake after water absorption are removed.
[0025] As a further improvement, the thickness of the super absorbent filter cake is 2 to 3.6 mm.
[0026] As a further improvement, the method for preparing the super absorbent filter cake comprises the following steps:
[0027] Step S1, stirring and mixing bagasse, super absorbent resin and ammonium bicarbonate to obtain a mixed material;
[0028] Step S2, pouring the mixed material into the iron ring, and then compacting it with a hydraulic press to obtain a half-cake layer, the thickness of the half-cake layer is half the thickness of the iron ring;
[0029] Step S3, brushing a saturated melamine ethanol solution on the upper surface of the half cake layer, and forming a melamine adhesion layer after the ethanol evaporates;
[0030] Step S4, pouring the mixed material into the iron ring and completely covering the melamine adhesion layer 30, and then compacting it with a hydraulic press to obtain a full cake layer;
[0031] Step S5, placing the iron ring and the entire cake layer inside it into a vacuum oven, and baking them at 180-200° C. and -75--55 kPa for 1 hour to obtain a super absorbent filter cake.
[0032] As a further improvement, the mass ratio of the bagasse, super absorbent resin and ammonium bicarbonate is 100:(5-7):3; the bagasse is crushed and then passed through a 16-mesh sieve.
[0033] As a further improvement, when a hydraulic press is used to compact the mixed material, the pressure of the hydraulic press is 12 bar.
[0034] Beneficial effects of the present invention:
[0035] The light gypsum mortar water retention performance testing system of the present invention does not require the purchase of a vacuum pump or filtration, is simple and convenient to operate, and mainly uses a super absorbent filter cake to perform a water retention test on the light gypsum mortar. The system is particularly suitable for light gypsum mortar water retention performance testing, and has high stability and good consistency in the measurement results. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a schematic diagram of the distribution of the half-cake layer and the iron ring;
[0037] Figure 2 Schematic diagram of the distribution of the entire cake layer and the iron ring. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0039] In the description of the present invention, it should be noted that, unless otherwise specified, "multiple" means two or more than two; the directions or positional relationships indicated by the terms "upper", "lower", "left", "right", "inner", "outer", "front end", "rear end", "head", "tail", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "third", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.
[0040] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0041] Example 1
[0042] The light gypsum mortar water retention performance detection system comprises a circular trough, a sampling bucket, a scraper, a counterweight, a circular metal filter screen, a circular super absorbent filter cake, a trough cover adapted to the circular trough, a balance, a sample tray, and an oven;
[0043] The sampling bucket has a bucket cover, and the sampling bucket is used to sample the lightweight gypsum mortar to be tested on site;
[0044] The diameter of the metal filter screen is larger than the inner diameter of the circular groove, and the diameter of the super absorbent filter cake is larger than the inner diameter of the circular groove.
[0045] The method for detecting the water retention performance of lightweight gypsum mortar using the lightweight gypsum mortar water retention performance detection system comprises the following steps:
[0046] Step 1, using a balance to weigh the mass of the circular tank as m1; using a balance to weigh the mass of the super absorbent filter cake as m2;
[0047] Step 2, open the lid of the sampling bucket, use the sampling bucket to sample the lightweight gypsum mortar to be tested on site, and cover the lid of the sampling bucket after sampling to complete the sampling; then pour the lightweight gypsum mortar from the sampling bucket into the inside of the circular groove and fill it, use a scraper to scrape it flat at the notch of the circular groove and wipe off the excess lightweight gypsum mortar, and clean the outer wall and notch of the circular groove;
[0048] Step 3, weigh the total mass of the circular trough and the lightweight gypsum mortar inside it as m3;
[0049] Step 4, cover the notch of the circular tank with a metal filter, then cover the super absorbent filter cake on the metal filter, then cover the tank cover on the super absorbent filter cake, and then cover the tank cover with a counterweight, after standing for 2 to 5 minutes, remove the counterweight, tank cover and the super absorbent filter cake after water absorption;
[0050] Step 5, weighing the mass of the super absorbent filter cake after absorbing water as m4;
[0051] Step 6, weigh the mass of the sample pan as m5; open the lid of the sampling barrel, pour the lightweight gypsum mortar in the sampling barrel into the sample pan, weigh the total mass of the sample pan and the lightweight gypsum mortar inside as m6; dry the sample pan and the lightweight gypsum mortar inside in an oven at 105±3°C to constant weight, and weigh the total mass of the dried sample pan and the lightweight gypsum mortar inside as m7;
[0052] The moisture content of lightweight gypsum mortar is θm, θm = [(m6-m5)-(m7-m5)] / (m6-m5);
[0053] The water retention rate of lightweight gypsum mortar is R, R = 1-(m4-m2) / [θm·(m3-m1)].
[0054] The principle of the present invention is to use a super absorbent filter cake to absorb the water in the lightweight gypsum mortar. The water that can be absorbed is the water that cannot be "locked" by the water retaining agent. Compared with the negative pressure water removal generated by a vacuum pump, the present invention uses a super absorbent filter cake to adsorb the water in the lightweight gypsum mortar, which is closer to the water loss process between the lightweight gypsum mortar and the building materials, thereby effectively improving the stability of the measurement results.
[0055] The mesh number of the metal filter is 270 to 400. The inner diameter of the circular groove is 100 to 200 mm, and the groove depth of the circular groove is 25 to 35 mm.
[0056] Example 2
[0057] Based on Example 1, the circular groove is an iron groove, the groove cover is a magnet, and the metal filter is an iron filter.
[0058] At the same time, in step 4, when no counterweight is used to cover the top of the tank cover, after the tank cover is covered on the top of the super absorbent filter cake, the circular tank and the tank cover are turned upside down, and then after standing for 2 to 5 minutes, the tank cover and the super absorbent filter cake after water absorption are removed.
[0059] The use of magnetic adsorption combined with the gravity generated by inversion, as well as the downward penetration of water in the lightweight gypsum mortar under the action of gravity, can improve the stability of the final measurement results.
[0060] Example 3
[0061] The thickness of the super absorbent filter cake is 2 to 3.6 mm. The method for making the super absorbent filter cake comprises the following steps:
[0062] Step S1, stirring and mixing bagasse, super absorbent resin and ammonium bicarbonate to obtain a mixed material; the mass ratio of the bagasse, super absorbent resin and ammonium bicarbonate is 100:6.5:3; the bagasse is crushed and then passed through a 16-mesh sieve.
[0063] The super absorbent resin used was 101 type super absorbent resin SAP produced by Guangzhou Yourun Chemical Co., Ltd., and the water absorption rate was 763g / g.
[0064] Step S2, pour the mixed material into the iron ring 10, and then use a hydraulic press to compact it to obtain a half cake layer 20, the thickness of the half cake layer 20 is half the thickness of the iron ring 10, such as Figure 1 shown.
[0065] Step S3, brushing a saturated ethanol solution of melamine (melamine is dissolved in ethanol to form a saturated solution) on the upper surface of the half cake layer 20, and forming a melamine adhesion layer 30 after the ethanol evaporates;
[0066] Step S4, pouring the mixed material into the iron ring and completely covering the melamine adhesion layer 30, and then compacting it with a hydraulic press to obtain a full cake layer 50;
[0067] Step S5, placing the iron ring 10 and the whole cake layer 50 inside it into a vacuum oven, and baking them at 180-200° C. and -75--55 kPa for 1 hour to obtain a super absorbent filter cake.
[0068] When using a hydraulic press to compact the mixed material, the pressure of the hydraulic press is 12 bar.
[0069] 《Consistency Evaluation Test》
[0070] With plaster as the test object, the test was conducted according to the present invention and the method for determining the water retention rate of plaster in "Plaster Gypsum" (JC / T517-2004), respectively. The test method of the present invention is Example 1; the method for determining the water retention rate of plaster in "Plaster Gypsum" (JC / T517-2004) is the reference group.
[0071] When testing the water retention rate, take the arithmetic mean of the two test results as the water retention rate, accurate to 0.1%; and the second test should be re-sampled and measured. When the difference between the two measured values exceeds 2%, this set of test results should be invalid.
[0072] Table 1
[0073]
[0074]
[0075] Table 1 shows the data obtained from 12 effective measurements of Example 1 and the reference group. It can be seen that the error between the two is less than 3% (error rate), and the consistency is good.
[0076] In addition, if lightweight gypsum mortar is used as the test object, the test is carried out according to the "Consistency Evaluation Test", and the test is performed 50 times. The number of invalid test results is counted, and the inefficiency is calculated; inefficiency = invalid number / 50. The invalidity rate in Example 1 is 4%, and the invalidity rate in the reference group is 20%.
[0077] The super absorbent filter cake of the present invention can be reused 100 times. After being reused 100 times, the inefficiency rate is less than 6% and the error rate does not exceed 3.2%.
[0078] Comparative Example 1
[0079] In Example 1, if the super absorbent filter cake is not used, but 10 to 20 sheets of filter paper are used instead, the test can also be completed. However, in this test, the ineffectiveness rate is 16%. In addition, the filter paper is a disposable item and cannot be dried and reused.
[0080] Comparative Example 2
[0081] The difference between this example and Example 3 is that in step S3, the melamine ethanol saturated solution is not applied, the melamine adhesion layer 30 is not provided, and the rest remains unchanged; the invalidity rate is 14%.
[0082] Comparative Example 3
[0083] The difference between this example and Example 3 is that in step S3, a mixture of melamine and water is applied, and the corresponding melamine adhesion layer 30 is formed after drying, and the rest remains unchanged; finally, the corresponding filter cake can only be reused 21 times; after being reused 22 times, the inefficiency of the filter cake exceeds 8%.
[0084] In the above embodiment, in the process of making the super absorbent filter cake, after the bagasse is compacted, the ammonium bicarbonate added can be thermally decomposed to produce bubbles, thereby forming a large number of micropores inside the super absorbent filter cake, and the capillary pores formed by the fibers of the bagasse itself after compaction, resulting in the super absorbent filter cake having a strong water absorption capacity. In addition, the super absorbent resin has a super strong water absorption capacity, which further improves the water absorption capacity of the super absorbent filter cake. The addition of super absorbent resin is mainly considered to be that if the water retention performance is too poor, or the water retention rate of the mortar is directly measured, the super absorbent filter cake is generally small in size. In order to ensure that there is no overflow or water seepage, the addition of super absorbent resin can also avoid overflow and water seepage. In addition, the super absorbent resin can be dehydrated by heating the super absorbent resin (such as the heating temperature is 155°C).
[0085] The melamine attachment layer 30 is arranged in the central area of the super absorbent filter cake, so as to improve the defect of uneven water absorption of the super absorbent filter cake caused by repeated use.
[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A light gypsum mortar water retention performance detection system, characterized in that: It includes a round trough, a sampling bucket, a scraper, a counterweight, a round metal filter screen, a round super absorbent filter cake, a trough cover adapted to the round trough, a balance, a sample tray, and an oven; The sampling bucket has a bucket cover, and the sampling bucket is used to sample the lightweight gypsum mortar to be tested on site; The diameter of the metal filter screen is larger than the inner diameter of the circular groove, and the diameter of the super absorbent filter cake is larger than the inner diameter of the circular groove.
2. A light gypsum mortar water retention performance detection system according to claim 1, characterized in that: The method for detecting the water retention performance of lightweight gypsum mortar using the lightweight gypsum mortar water retention performance detection system comprises the following steps: Step 1, using a balance to weigh the mass of the circular tank as m1; using a balance to weigh the mass of the super absorbent filter cake as m2; Step 2, open the lid of the sampling bucket, use the sampling bucket to sample the lightweight gypsum mortar to be tested on site, and cover the lid of the sampling bucket after sampling to complete the sampling; then pour the lightweight gypsum mortar from the sampling bucket into the inside of the circular groove and fill it, use a scraper to scrape it flat at the notch of the circular groove and wipe off the excess lightweight gypsum mortar, and clean the outer wall and notch of the circular groove; Step 3, weigh the total mass of the circular trough and the lightweight gypsum mortar inside it as m3; Step 4, cover the notch of the circular tank with a metal filter, then cover the super absorbent filter cake on the metal filter, then cover the tank cover on the super absorbent filter cake, and then cover the tank cover with a counterweight, after standing for 2 to 5 minutes, remove the counterweight, tank cover and the super absorbent filter cake after water absorption; Step 5, weighing the mass of the super absorbent filter cake after absorbing water as m4; Step 6, weigh the mass of the sample pan as m5; open the lid of the sampling barrel, pour the lightweight gypsum mortar in the sampling barrel into the sample pan, weigh the total mass of the sample pan and the lightweight gypsum mortar inside as m6; dry the sample pan and the lightweight gypsum mortar inside in an oven at 105±3°C to constant weight, and weigh the total mass of the dried sample pan and the lightweight gypsum mortar inside as m7; The moisture content of lightweight gypsum mortar is θm, θm = [(m6-m5)-(m7-m5)] / (m6-m5); The water retention rate of lightweight gypsum mortar is R, R = 1-(m4-m2) / [θm·(m3-m1)].
3. A light gypsum mortar water retention performance detection system according to claim 1, characterized in that: The mesh number of the metal filter is 270 to 400 meshes.
4. A light gypsum mortar water retention performance detection system according to claim 1, characterized in that: The inner diameter of the circular groove is 100-200 mm, and the groove depth of the circular groove is 25-35 mm.
5. A light gypsum mortar water retention performance detection system according to claim 2, characterized in that: The circular groove is an iron groove, the groove cover is a magnet, and the metal filter is an iron filter.
6. A light gypsum mortar water retention performance detection system according to claim 5, characterized in that: In step 4, when no counterweight is used to cover the top of the tank cover, after the tank cover is covered on the top of the super absorbent filter cake, the circular tank and the tank cover are turned upside down, and then after standing for 2 to 5 minutes, the tank cover and the super absorbent filter cake after water absorption are removed.
7. A light gypsum mortar water retention performance detection system according to claim 1, characterized in that: The thickness of the super absorbent filter cake is 2 to 3.6 mm.
8. A light gypsum mortar water retention performance detection system according to claim 1, characterized in that: The method for preparing the super absorbent filter cake comprises the following steps: Step S1, stirring and mixing bagasse, super absorbent resin and ammonium bicarbonate to obtain a mixed material; Step S2, pouring the mixed material into the iron ring, and then compacting it with a hydraulic press to obtain a half-cake layer, the thickness of the half-cake layer is half the thickness of the iron ring; Step S3, brushing a saturated melamine ethanol solution on the upper surface of the half cake layer, and forming a melamine adhesion layer after the ethanol evaporates; Step S4, pouring the mixed material into the iron ring and completely covering the melamine adhesion layer 30, and then compacting it with a hydraulic press to obtain a full cake layer; Step S5, placing the iron ring and the entire cake layer inside it into a vacuum oven, and baking them for 1 hour at 180-200° C. and -75--55 kPa to obtain a super absorbent filter cake.
9. A light gypsum mortar water retention performance detection system according to claim 8, characterized in that: The mass ratio of the bagasse, the super absorbent resin and the ammonium bicarbonate is 100:(5-7):3; the bagasse is crushed and then passed through a 16-mesh sieve.
10. A light gypsum mortar water retention performance detection system according to claim 8, characterized in that: When using a hydraulic press to compact the mixed material, the pressure of the hydraulic press is 12 bar.