Electric field enhancement element and Raman spectroscopy device
By designing an electric field enhancement element with cooperative plasmons in the Raman spectroscopy device, and using a combination of conductive fine structures and transparent layers, the problems of insufficient detection sensitivity and signal deviation are solved, and high sensitivity and high reproducibility are achieved. detection effect and improves the durability of the equipment.
Patent Information
- Application Number
- CN202410365741.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-01
AI Technical Summary
The existing localized surface plasmon resonance Raman spectroscopy device has insufficient sensitivity when detecting low-concentration samples, and the position deviation of the target substance causes deviation of the detection signal, making it difficult to improve the reproducibility and durability of detection.
An electric field enhancement element is designed, which includes a substrate, a conductive microstructure and a transparent layer. It generates cooperative plasmons through plasmon resonance and surface lattice resonance. The enhanced electric field has a maximum value in the vertical direction, independent of The position of the fine structure improves the detection signal and inhibits oxidation and chemical changes of the fine structure through the transparent layer.
It improves the detection sensitivity, reduces the deviation of the detection signal, enhances the reproducibility and durability of the detection, can enhance the detection signal without relying on the target substance being located near the fine structure pole, and extends the service life of the equipment.
Smart Images

Figure CN118730994A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an electric field enhancement element and a Raman spectroscopy device. Background Art
[0002] In recent years, as one of the spectroscopic techniques for detecting low-concentration sample molecules, a Raman spectroscopic device using localized surface plasmon resonance (LSPR) is known. In such a Raman spectroscopic device, an electric field enhancement element having a nanoscale concave-convex structure forms an enhanced electric field, generating surface enhanced Raman scattering (SERS) in which Raman scattered light is enhanced.
[0003] For example, Patent Document 1 describes an optical device including a substrate, a metal microstructure composed of a plurality of metal particles formed on a surface of the substrate, and an organic molecular film formed on the metal microstructure.
[0004] Patent Document 1: Japanese Patent Application Publication No. 2013-96939
[0005] In the optical device described above, it is desired to improve the detection sensitivity. Summary of the invention
[0006] One embodiment of the electric field enhancing element of the present invention comprises: a substrate; a plurality of fine structures which are arranged on the substrate and have conductivity; and a transparent layer which covers the plurality of fine structures and the substrate, wherein the enhanced electric field generated by the plurality of fine structures has a maximum value in a perpendicular direction to the substrate at a position on the side of the plurality of fine structures opposite to the substrate and separated from the plurality of fine structures.
[0007] One embodiment of the Raman spectroscopic apparatus of the present invention comprises: one embodiment of the electric field enhancing element; a light source for irradiating light to the electric field enhancing element; and a detector for detecting the light from the electric field enhancing element. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 It is a cross-sectional view schematically showing the electric field enhancing element according to the present embodiment.
[0009] Figure 2 It is a plan view schematically showing the electric field enhancing element according to this embodiment.
[0010] Figure 3 It is a plan view schematically showing the electric field enhancing element according to this embodiment.
[0011] Figure 4It is a plan view schematically showing the electric field enhancing element according to this embodiment.
[0012] Figure 5 It is a plan view schematically showing the electric field enhancing element according to this embodiment.
[0013] Figure 6 It is a plan view schematically showing the electric field enhancing element according to this embodiment.
[0014] Figure 7 It is a diagram for explaining plasmon resonance in the electric field enhancing element according to the present embodiment.
[0015] Figure 8 It is a diagram for explaining plasmon resonance in the electric field enhancing element according to the present embodiment.
[0016] Fig. 9 This is a diagram for explaining the enhanced electric field generated by a plurality of fine structures of the electric field enhancing element according to the present embodiment.
[0017] Fig.10 It is a cross-sectional view schematically showing an electric field enhancing element according to a modification of the present embodiment.
[0018] Fig.11 It is a cross-sectional view schematically showing the Raman spectroscopic apparatus according to the present embodiment.
[0019] Fig.12 This is a diagram for explaining the principle of Raman scattering spectroscopy.
[0020] Fig.13 It is a schematic diagram showing an example of a Raman spectrum obtained by Raman scattering spectroscopy.
[0021] Fig.14 It is an XZ cross-sectional view schematically showing the model used for simulation.
[0022] Fig.15 It is an XY cross-sectional view schematically showing a model used for simulation.
[0023] Fig.16 It is an XY cross-sectional view schematically showing a model used for simulation.
[0024] Fig.17 It is an XZ cross-sectional view schematically showing the model used for simulation.
[0025] Fig.18 This is a table showing dimensions and changing main parameters in Examples 1 to 16 and Comparative Example 1.
[0026] Fig.19 This is the simulation result of Example 1.
[0027] Fig. 20 This is the simulation result of Example 2.
[0028] Fig.21 This is the simulation result of Example 3.
[0029] Fig. 22 This is the simulation result of Example 4.
[0030] Fig.23 This is the simulation result of Example 5.
[0031] Fig.24 This is the simulation result of Example 6.
[0032] Fig.25 This is the simulation result of Example 7.
[0033] Fig.26 This is the simulation result of Example 8.
[0034] Fig. 27 This is the simulation result of Example 9.
[0035] Fig.28 This is the simulation result of Example 10.
[0036] Fig.29 This is the simulation result of Example 11.
[0037] Fig.30 This is the simulation result of Example 12.
[0038] Fig.31 This is the simulation result of Example 13.
[0039] Fig.32 This is the simulation result of Example 14.
[0040] Fig.33 This is the simulation result of Example 15.
[0041] Fig.34 This is the simulation result of Example 16.
[0042] Fig.35 This is the simulation result of Comparative Example 1.
[0043] Description of symbols
[0044] 10: substrate; 20: dielectric layer; 30: microstructure; 40: transparent layer; 42: upper surface; 50: molecule capture layer; 100, 200: electric field enhancement element; 300: Raman spectrometer; 310: light source; 320: collimating lens; 330: polarization control element; 340: dichroic mirror; 350: objective lens; 360: focusing lens; 370: detector. DETAILED DESCRIPTION
[0045] The preferred embodiments of the present invention are described in detail below using the accompanying drawings. In addition, the embodiments described below do not inappropriately limit the contents of the present invention described in the technical solution. Moreover, not all the structures described below are necessary structural elements of the present invention.
[0046] 1. Electric field enhancement element
[0047] 1.1. Structure
[0048] First, the electric field enhancing element according to the present embodiment will be described with reference to the drawings. Figure 1 1 is a cross-sectional view schematically showing the electric field enhancing element 100 according to the present embodiment. Figure 2 is a top view schematically showing the electric field enhancement element 100 of this embodiment. Figure 1 yes Figure 2 In addition, Figure 1 and Figure 2 In the figure, an X-axis, a Y-axis, and a Z-axis are illustrated as three axes perpendicular to each other.
[0049] like Figure 1 and Figure 2 As shown in FIG. 1 , the electric field enhancement element 100 includes a substrate 10, a dielectric layer 20, a microstructure 30, and a transparent layer 40. Figure 2 The transparent layer 40 is omitted in the figure.
[0050] The substrate 10 supports the microstructure 30 via the dielectric layer 20. Figure 1 and Figure 2 When light from a light source (hereinafter also referred to as “light source”) not shown in the figure is incident from the substrate 10 side, the substrate 10 transmits the light. When light from the light source is incident from the transparent layer 40 side, the substrate 10 may also reflect the light toward the transparent layer 40 side.
[0051] The substrate 10 is, for example, a glass substrate or a silicon substrate. The material of the substrate 10 is, for example, SiO2 or Si. The substrate 10 has a vertical line Q. The vertical line Q is a vertical line to the upper surface of the substrate 10. In the example shown in the figure, the vertical line Q is parallel to the Z axis, and the direction of the vertical line Q is the Z axis direction.
[0052] like Figure 1 As shown, the dielectric layer 20 is provided on the substrate 10. The dielectric layer 20 is provided between the substrate 10 and the microstructure 30. The thickness of the dielectric layer 20 is, for example, 1 nm to 2000 nm, preferably 10 nm to 1000 nm. In addition, the dielectric layer 20 may not be provided.
[0053] The dielectric layer 20 is transparent to light from the light source. The material of the dielectric layer 20 is, for example, Al2O3, TiO2, MgO, LiNbO3, HfO2, Ta2O5, SiON, Si3N4, etc. The dielectric layer 20 may also be composed of a plurality of layers. In this case, the materials of the plurality of layers may also be different.
[0054] The fine structure 30 is provided on the dielectric layer 20. The fine structure 30 is provided on the substrate 10 via the dielectric layer 20. The fine structure 30 is provided between the dielectric layer 20 and the transparent layer 40. The shape of the fine structure 30 is, for example, a cylinder. The diameter of the fine structure 30 is, for example, greater than 1 nm and less than 1000 nm, preferably greater than 5 nm and less than 500 nm, and more preferably greater than 10 nm and less than 400 nm.
[0055] In addition, the “diameter of the microstructure 30” is the diameter when the planar shape of the microstructure 30 is a circle, and is the diameter of the smallest circle when the planar shape of the microstructure 30 is a non-circular shape. For example, when the planar shape of the microstructure 30 is a polygon, the diameter of the microstructure 30 is the diameter of the smallest circle that includes the polygon inside, and when the planar shape of the microstructure 30 is an ellipse, the diameter of the microstructure 30 is the diameter of the smallest circle that includes the ellipse inside.
[0056] There are multiple fine structures 30. The multiple fine structures 30 are separated from each other. A transparent layer 40 is provided between adjacent fine structures 30. The distance between adjacent fine structures 30 is, for example, greater than 20 nm and less than 1000 nm, preferably greater than 100 nm and less than 900 nm. When viewed from the Z-axis direction, the multiple fine structures 30 are arranged at a predetermined pitch in a predetermined direction. The multiple fine structures 30 are periodically provided. Figure 2 In the example shown, a plurality of microstructures 30 are arranged in a square lattice.
[0057] In addition, the "pitch between the microstructures 30" refers to the distance between the centers of the adjacent microstructures 30 in a predetermined direction. The "center of the microstructure 30" is the center of the circle when the planar shape of the microstructure 30 is a circle, and is the center of the smallest circle when the planar shape of the microstructure 30 is a non-circular shape. For example, when the planar shape of the microstructure 30 is a polygon, the center of the microstructure 30 is the center of the smallest circle that includes the polygon inside, and when the planar shape of the microstructure 30 is an ellipse, it is the center of the smallest circle that includes the ellipse inside.
[0058] In addition, if Figure 3As shown, the plurality of microstructures 30 may be arranged in a triangular lattice when viewed from the Z-axis direction. Although not shown, the periodicity of the plurality of microstructures 30 may be expanded or contracted at a certain ratio, and the plurality of microstructures may include a fractal structure.
[0059] In addition, the planar shape of the microstructure 30 is not limited to a circle. For example, the planar shape of the microstructure 30 may be as follows: Figure 4 As shown, it is an ellipse, or it can be Figure 5 As shown in FIG. 1 , the microstructure 30 may be rectangular. Figure 6 As shown in the figure, it has various planar shapes such as granular, polygonal, wheel-shaped, linear, etc. In addition, multiple fine structures 30 can also be combined with fine structures of different shapes. In this way, the intensity and distribution of the enhanced electric field generated by the multiple fine structures 30 can also be controlled in the in-plane direction perpendicular to the vertical line Q direction.
[0060] Although not shown in the figure, a plurality of recessed portions may be formed on the upper surface of the dielectric layer 20 , and the microstructures 30 may be provided in the recessed portions.
[0061] The microstructure 30 is conductive. The material of the microstructure 30 is, for example, a metal such as Al, Au, Ag, Cu, Pt, Pd, or Ni. The material of the microstructure 30 may also be an alloy thereof. The microstructure 30 may also be a metal particle. In addition, the material of the microstructure 30 is not particularly limited as long as it has a plasma frequency relative to the light from the light source, and may also be a transparent electrode such as ITO (Indium Tin Oxide) or a carbon nanotube.
[0062] The transparent layer 40 is provided on the microstructure 30 and the substrate 10. The transparent layer 40 covers the microstructure 30 and the substrate 10. The thickness of the transparent layer 40 is, for example, 10 nm to 2000 nm, preferably 20 nm to 1000 nm.
[0063] The transparent layer 40 is transparent to the light from the light source. The material of the transparent layer 40 is, for example, a dielectric such as Al2O3, TiO2, MgO, LiNbO3, HfO2, Ta2O5, SiON, Si3N4, etc. In addition, the material of the transparent layer 40 may also be polystyrene. The transparent layer 40 may also be composed of a plurality of layers. In this case, the materials of the plurality of layers may also be different. The refractive index of the transparent layer 40 may also be the same as the refractive index of the dielectric layer 20. If the refractive index of the transparent layer 40 is the same as the refractive index of the dielectric layer 20, the Rayleigh anomaly described later is likely to occur. The refractive index of the transparent layer 40 may be higher than the refractive index of the substrate 10.
[0064] The transparent layer 40 has an upper surface 42. The upper surface 42 constitutes, for example, an interface between the transparent layer 40 and an air layer. In the example shown in the figure, the upper surface 42 is a flat surface. The target substance to be detected is in contact with the upper surface 42, for example.
[0065] 1.2. Enhanced electric field
[0066] Figure 7 and Figure 8 It is a diagram for explaining plasmon resonance in the electric field enhancing element 100 . Fig. 9 1 is a diagram for explaining the enhanced electric field E generated by the plurality of fine structures 30 of the electric field enhancing element 100 .
[0067] exist Figure 7 and Figure 8 In the example shown, light enters the plurality of microstructures 30 from the substrate 10 side. The light entering the microstructures 30 has a wavelength capable of causing plasmon resonance in the plurality of microstructures 30. The wavelength of the light entering the microstructures 30 is, for example, 350 nm to 650 nm.
[0068] like Figure 7 As shown, when light from a light source enters the microstructure 30, LSPR is induced. Furthermore, 90° diffraction, namely Rayleigh anomaly, occurs due to the plurality of microstructures 30. By combining the Rayleigh anomaly with the LSPR, SLR (Surface Lattice Resonance) is induced.
[0069] Furthermore, if Figure 8 As shown, light is waveguided in the transparent layer 40. By combining the waveguide mode in the transparent layer 40 with the LSPR, a QGM (Quasi Guided Mode) is induced.
[0070] Furthermore, the SLR and the QGM cooperate to induce cooperative plasmons in the plurality of microstructures 30. By combining the SLR and the QGM, Fig. 9As shown, the enhanced electric field E generated by the multiple fine structures 30 not only has the first enhanced field Ea generated at the end of the fine structure 30 due to LSPR, but also has the second enhanced field Eb generated above the fine structure 30 due to SLR and QGM. The enhanced electric field E enhances the Raman scattered light and generates SERS. The enhanced electric field E has a maximum value at a position S1 on the opposite side of the multiple fine structures 30 to the substrate 10 and separated from the multiple fine structures 30 in the Z-axis direction through the second enhanced field Eb. The fact that the enhanced electric field E has a maximum value at the position S1 can be said to be a feature of the cooperative plasmon phenomenon. In the example shown in the figure, the position S1 is closer to the +Z axis direction than the multiple fine structures 30. The second enhanced field Eb can be separated from the first enhanced field Ea or continuous with the first enhanced field Ea.
[0071] like Fig. 9 As shown, in the Z-axis direction, the second enhancement field Eb exists at the position S2 separated from the plurality of fine structures 30 by a distance L. The distance L may be 100 nm or 200 nm. In the example shown in the figure, in the Z-axis direction, the distance between the position S1 and the plurality of fine structures 30 is less than the distance L, but may be greater than the distance L. The second enhancement field Eb exists, for example, across the upper surface 42 of the transparent layer 40.
[0072] 1.3. Effects
[0073] The electric field enhancing element 100 includes a substrate 10, a plurality of conductive fine structures 30 disposed on the substrate 10, and a transparent layer 40 covering the plurality of fine structures 30 and the substrate 10. The enhanced electric field E generated by the plurality of fine structures 30 has a maximum value at a position S1 on the opposite side of the plurality of fine structures 30 from the substrate 10 and separated from the plurality of fine structures 30 in the direction of a perpendicular line Q to the substrate 10.
[0074] Therefore, in the electric field enhancement element 100, the detection sensitivity can be improved. For example, in the case where the enhanced electric field E is generated only at the end of the microstructure due to LSPR, if the target substance is not located near the pole of the microstructure, the electric field enhancement effect cannot be obtained. Usually, the probability of the target substance being located near the microstructure has a deviation, so when the enhanced electric field E is generated only at the end of the microstructure, the detection sensitivity is easily reduced. In addition, the reproducibility of the detection is also deteriorated. Furthermore, if the size of the target substance is large, the target substance cannot enter between adjacent microstructures, and it is sometimes difficult to locate the target substance near the microstructure.
[0075] As described above, in the electric field enhancement element 100, the enhanced electric field E generated by the plurality of fine structures 30 has a maximum value in the direction of the vertical line Q at the position S1 which is on the side of the plurality of fine structures 30 opposite to the substrate 10 and separated from the plurality of fine structures 30, so that even if the target substance is not located near the pole of the fine structure 30, the detection signal caused by the target substance can be enhanced. As a result, the detection sensitivity can be improved. In addition, the target substance such as virus and bacteria can be freely selected.
[0076] Furthermore, in the electric field enhancement element 100, as described above, the target substance need not be located near the pole of the microstructure 30, so that the transparent layer 40 covering the microstructure 30 can be provided. Therefore, chemical property changes such as oxidation and sulfurization of the microstructure 30 can be suppressed. In particular, Ag is prone to deterioration and deformation such as oxidation, sulfurization, migration, etc. In the electric field enhancement element 100, even if Ag is used as the microstructure 30, such deterioration and deformation can be suppressed. As a result, durability and reliability can be improved.
[0077] Furthermore, in the electric field enhancement element 100, the transparent layer 40 can alleviate the unevenness caused by the plurality of microstructures 30. Therefore, the flatness of the surface in contact with the target substance can be improved. Thus, the deviation of the detection signal caused by the target substance in the in-plane direction can be reduced.
[0078] In the electric field enhancing element 100, a transparent layer 40 is provided between adjacent fine structures 30 among the plurality of fine structures 30, and the refractive index of the transparent layer 40 is higher than that of the substrate 10. Therefore, in the electric field enhancing element 100, light is easily concentrated at the positions of the plurality of fine structures 30 in the direction of the perpendicular line Q, compared with, for example, a case where the refractive index of the transparent layer is lower than that of the substrate. Thus, QGM is easily induced.
[0079] In the electric field enhancing element 100, the enhanced electric field E exists at a position S2 separated by 100 nm from the plurality of fine structures 30 to the opposite side of the substrate 10 in the direction of the perpendicular line Q. Therefore, in the electric field enhancing element 100, even if the target substance is not located near the pole of the fine structure 30, the detection signal caused by the target substance can be enhanced.
[0080] In the electric field enhancing element 100, the enhanced electric field E exists at a position S2 separated by 200 nm from the plurality of fine structures 30 to the opposite side of the substrate 10 in the direction of the perpendicular line Q. Therefore, in the electric field enhancing element 100, even if the target substance is not located near the pole of the fine structure 30, the detection signal caused by the target substance can be enhanced.
[0081] In the electric field enhancement element 100, a plurality of fine structures 30 are arranged periodically. Therefore, in the electric field enhancement element 100, it is possible to reduce the intensity deviation of the enhanced electric field E in the in-plane direction. In the case where a plurality of fine structures are randomly arranged, only the fine structures with a pitch and a diameter consistent with the wavelength of the light from the light source induce LSPR, so that the intensity of the enhanced electric field E is deviated in the in-plane direction. In addition, in the electric field enhancement element 100, a plurality of fine structures 30 are arranged periodically, so it is easy to induce SLR.
[0082] 2. Method for manufacturing electric field enhancement element
[0083] Next, a method for manufacturing the electric field enhancing element 100 according to the present embodiment will be described with reference to the drawings.
[0084] like Figure 1 As shown, a dielectric layer 20 is formed on a substrate 10. The dielectric layer 20 is formed by, for example, vapor deposition, sputtering, CVD (Chemical Vapor Deposition) or ALD (Atomic Layer Deposition).
[0085] Next, a plurality of microstructures 30 are formed on the dielectric layer 20. The microstructures 30 are formed by forming a thin film by vacuum deposition or sputtering, for example, and then patterning the thin film. Examples of patterning include photolithography and etching, microcontact printing, and nanoimprinting.
[0086] Next, the transparent layer 40 is formed on the dielectric layer 20 and the microstructure 30. The transparent layer 40 is formed by, for example, vapor deposition, sputtering, CVD, or ALD.
[0087] Through the above steps, the electric field enhancing element 100 can be manufactured.
[0088] 3. Modification of the electric field enhancement element
[0089] Next, an electric field enhancing element according to a modification of the present embodiment will be described with reference to the drawings. Fig.10 2 is a cross-sectional view schematically showing an electric field enhancing element 200 according to a modification of the present embodiment. In the electric field enhancing element 200 according to the modification of the present embodiment, components having the same functions as those of the components of the electric field enhancing element 100 according to the present embodiment are denoted by the same reference numerals, and detailed description thereof is omitted.
[0090] like Fig.10 As shown, the electric field enhancing element 200 is different from the above-mentioned electric field enhancing element 100 in that it has a molecule trapping layer 50 .
[0091] The molecular capture layer 50 is disposed on the transparent layer 40. The molecular capture layer 50 is in contact with the transparent layer 40. The molecular capture layer 50 is an organic molecular film. The molecular capture layer 50 is, for example, a SAM (Self-Assembled Monolayers). The thickness of the molecular capture layer 50 is, for example, greater than 0.1 nm and less than 1 nm, preferably less than 0.4 nm. The molecular capture layer 50 has a function of capturing a target substance. The molecular capture layer 50 can be appropriately selected according to the type of the target substance, for example, an alkanethiol film, a silane coupling agent can be cited. The molecular capture layer 50 is formed, for example, by a liquid bubble method, a vacuum evaporation method, an MVD (Molecular Vapor Deposition: molecular vapor deposition) method, or a CVD method.
[0092] In the electric field enhancement element 200, since the molecule capture layer 50 is provided on the transparent layer 40, it is possible to alleviate uneven film formation of the molecule capture layer 50. For example, when the molecule capture layer is directly formed on the microstructure and the substrate without providing a transparent layer, since the surface of the microstructure and the surface of the substrate have different physical and chemical states, uneven film formation of the molecule capture layer may occur.
[0093] Furthermore, in the electric field enhancement element 200, as described above, the target substance need not be located near the pole of the microstructure 30, so the selectivity of the molecular chain length of the molecule capture layer 50 is increased. Although not shown, a primer layer may be provided between the transparent layer 40 and the molecule capture layer 50 to improve the adhesion between the two.
[0094] In the example shown in the figure, the shape of the microstructure 30 is a semicircle. In addition, the cross-sectional shape of the microstructure 30 is not particularly limited, and may be, for example, a trapezoid, a circle, an inverted cone, a spherical end, etc. The shape of the microstructure 30 may be a quadrangular pyramid or a cone.
[0095] 4. Raman spectroscopy device
[0096] 4.1. Structure
[0097] Next, the Raman spectroscopic apparatus according to the present embodiment will be described with reference to the drawings. Fig.11 Schematic diagram of a Raman spectroscopic apparatus 300 according to the present embodiment.
[0098] like Fig.11 As shown, the Raman spectroscopic device 300 includes, for example, an electric field enhancement element 100, a light source 310, a collimating lens 320, a polarization control element 330, a dichroic mirror 340, an objective lens 350, a condenser lens 360, and a detector 370. Fig.11 In FIG. 1 , the electric field enhancing element 100 is shown in a simplified manner.
[0099] The target substance is carried into the Raman spectrometer 300 from the C1 direction and carried out from the C2 direction. For example, by controlling the driving of a fan (not shown), the target substance is introduced into the conveying unit from the carrying inlet and discharged from the discharge outlet.
[0100] The light source 310 irradiates light to the electric field enhancement element 100. The light emitted from the light source 310 has a wavelength that causes the electric field enhancement element 100 to induce SLR and QGM. As the light source 310, for example, a laser or an LED (Light Emitting Diode) is used. As the laser, for example, VCSEL (Vertical Cavity Surface Emitting Laser) and PCSEL (Photonic Crystal Surface Emitting Laser) can be cited.
[0101] The light emitted from the light source 310 is converted into parallel light by, for example, a collimating lens 320, passes through a polarization control element 330, and is guided toward the electric field enhancement element 100 by a dichroic mirror 340. The light toward the electric field enhancement element 100 is converged by an objective lens 350 and enters the electric field enhancement element 100. At this time, the target substance is in contact with the transparent layer 40 of the electric field enhancement element 100.
[0102] When light is incident on the electric field enhancement element 100, an enhanced electric field E is generated through the plurality of fine structures 30. If the target substance is located in the enhanced electric field E, SERS light is generated therefrom. The SERS light passes through the objective lens 350 and is guided by the dichroic mirror 340 toward the detector 370. The SERS light toward the detector 370 is converged by the condenser lens 360 and incident on the detector 370.
[0103] The detector 370 detects the SERS light from the electric field enhancement element 100. The detector 370 is, for example, a diffraction grating spectrometer. In addition, in the Raman spectroscopic device 300, the SERS light is spectrally decomposed by the detector 370 to obtain spectral information. The detector 370 may also be a Fabry-Perot etalon spectrometer.
[0104] 4.2 Principle
[0105] Fig.12 This is a diagram for explaining the principle of Raman scattering spectroscopy.
[0106] like Fig.12As shown in FIG. 1 , for example, when a light of wavelength Lin is irradiated to a target substance X, in addition to Rayleigh scattered light Ray of wavelength λ1 which is the same as the wavelength λin of the incident light Lin, Raman scattered light Ram of wavelength λ2 which is different from wavelength λ1 is generated in the scattered light. The energy difference between the Raman scattered light Ram and the incident light Lin corresponds to the energy of the vibrational energy level, rotational energy level, and electronic energy level of the target substance X. The target substance X has a unique vibrational energy corresponding to its structure, so the target substance X can be identified by using the light of wavelength Lin.
[0107] Fig.13 is a schematic diagram showing an example of a Raman spectrum obtained by Raman scattering spectroscopy. Fig.13 In FIG. 1 , the horizontal axis represents the Raman frequency shift. The Raman frequency shift is the difference between the wave number (vibration number) of the Raman scattered light Ram and the wave number of the incident light Lin, and has a value specific to the molecular bonding state of the target substance X.
[0108] like Fig.13 As shown, when the scattering intensity of the Raman scattered light Ram shown by K1 is compared with the scattering intensity of the Rayleigh scattered light Ray shown by K2, it can be seen that the Raman scattered light Ram is weaker. Thus, the Raman scattering spectroscopy method is a measurement method that has excellent recognition capability for the target substance X, but has low sensitivity itself for detecting the target substance X. Therefore, in the Raman spectroscopic apparatus 300, SERS is used to achieve high sensitivity.
[0109] 4.3. Effects
[0110] The Raman spectroscopic device 300 includes the electric field enhancing element 100, the light source 310 for irradiating light to the electric field enhancing element 100, and the detector 370 for detecting light from the electric field enhancing element 100. As described above, the electric field enhancing element 100 can improve detection sensitivity. Therefore, the Raman spectroscopic device 300 has high detection sensitivity.
[0111] 5. Experimental Examples
[0112] Model
[0113] <Example 1>
[0114] Fig.14 1 is an XZ cross-sectional view schematically showing a model M used for simulation. Fig.15 1 is an XY cross-sectional view schematically showing a model M used for simulation.
[0115] In model M, if Fig.14 As shown, the material of the substrate is set to SiO2. Light is made incident from the substrate side to the model M. The wavelength of the incident light is set to 578nm.
[0116] The material of the dielectric layer was set to Al2O3, and the thickness A of the dielectric layer was set to 20 nm.
[0117] The material of the microstructure is Al. Fig.15 As shown, the arrangement of the microstructures is a square lattice. The shape of the microstructures is a cylinder. The pitch P of the microstructures is 391 nm, the diameter D is 156 nm, and the thickness H is 20 nm.
[0118] The material of the transparent layer was set to Al2O3. The thickness B of the transparent layer was set to 360 nm. An air layer was arranged on the transparent layer.
[0119] <Example 2>
[0120] In Example 2, the same procedures as in Example 1 were performed except that the thickness H of the microstructure was set to 200 nm and the wavelength of the incident light was set to 432 nm.
[0121] <Example 3>
[0122] In Example 3, the same procedures as in Example 1 were performed except that the diameter D of the microstructure was set to 39 nm, the thickness H of the microstructure was set to 60 nm, and the wavelength of the incident light was set to 410 nm.
[0123] <Example 4>
[0124] In Example 4, the same procedures as in Example 1 were performed except that the diameter D of the microstructure was set to 352 nm, the thickness H of the microstructure was set to 60 nm, and the wavelength of the incident light was set to 571 nm.
[0125] <Example 5>
[0126] In Example 5, the thickness A of the dielectric layer is set to zero, that is, no dielectric layer is provided, the diameter D of the microstructure is set to 39 nm, the thickness H of the microstructure is set to 60 nm, and the wavelength of the incident light is set to 408 nm. The above is the same as Example 1.
[0127] <Example 6>
[0128] In Example 6, the process is the same as that of Example 1 except that the thickness A of the dielectric layer is set to 1000 nm, the diameter D of the microstructure is set to 39 nm, the thickness H of the microstructure is set to 60 nm, and the wavelength of the incident light is set to 576 nm.
[0129] <Example 7>
[0130] In Example 7, the same procedures as in Example 1 were followed except that the thickness H of the microstructure was set to 19 nm, the thickness B of the transparent layer was set to 20 nm, and the wavelength of the incident light was set to 412 nm.
[0131] <Example 8>
[0132] In Example 8, the process was the same as that of Example 1 except that the thickness H of the microstructure was set to 19 nm, the thickness B of the transparent layer was set to 1000 nm, and the wavelength of the incident light was set to 404 nm.
[0133] <Example 9>
[0134] In Example 9, the pitch P of the fine structure is set to 278nm, the material of the dielectric layer is set to TiO2, the diameter D of the fine structure is set to 111nm, the thickness H of the fine structure is set to 60nm, and the wavelength of the incident light is set to 426nm. Other than this, it is the same as Example 1.
[0135] <Example 10>
[0136] In Example 10, the pitch P of the fine structure is set to 365nm, the material of the dielectric layer is set to MgO, the diameter D of the fine structure is set to 146nm, the thickness H of the fine structure is set to 60nm, and the wavelength of the incident light is set to 568nm. Except for this, it is the same as Example 1.
[0137] <Example 11>
[0138] Example 11 is the same as Example 1 except that the material of the microstructure is Au, the diameter D of the microstructure is 196 nm, the thickness H of the microstructure is 60 nm, and the wavelength of the incident light is 583 nm.
[0139] <Example 12>
[0140] In Example 12, the material of the microstructure is ITO, the diameter D of the microstructure is 235 nm, the thickness H of the microstructure is 60 nm, and the wavelength of the incident light is 413 nm. The above is the same as in Example 1.
[0141] <Example 13>
[0142] In Example 13, the same procedures as in Example 1 were performed except that the pitch P of the microstructures was set to 246 nm, the diameter D of the microstructures was set to 98 nm, the thickness H of the microstructures was set to 60 nm, and the wavelength of the incident light was set to 386 nm.
[0143] <Example 14>
[0144] In Example 14, the same procedures as in Example 1 were performed except that the pitch P of the microstructures was set to 829 nm, the diameter D of the microstructures was set to 332 nm, the thickness H of the microstructures was set to 60 nm, and the wavelength of the incident light was set to 638 nm.
[0145] <Example 15>
[0146] In Example 15, Fig.16 As shown, the arrangement of the microstructures was set to a triangular lattice, the thickness H of the microstructures was set to 60 nm, and the wavelength of the incident light was set to 505 nm. The above was the same as in Example 1.
[0147] <Example 16>
[0148] In Example 16, Fig.17 As shown, the same procedures as in Example 1 are performed except that the shape of the microstructure is set to a cone, the thickness H of the microstructure is set to 60 nm, and the wavelength of the incident light is set to 576 nm.
[0149] <Comparative Example 1>
[0150] In Comparative Example 1, except that the thickness A of the dielectric layer is zero (i.e., no dielectric layer is provided), the thickness B of the transparent layer is zero (i.e., no transparent layer is provided), the material of the fine structure is Ag, the pitch P of the fine structure is 250nm, the diameter D of the fine structure is 50nm, the thickness H of the fine structure is 25nm, and the wavelength of the incident light is 464nm, it is the same as Example 1.
[0151] Fig.18 This is a table showing dimensions and main parameters of changes in the above-mentioned Examples 1 to 16 and Comparative Example 1.
[0152] 5.2. Simulation results
[0153] In the above-mentioned Examples 1 to 16 and Comparative Example 1, simulations were performed on the distribution of the enhanced electric field. The simulations used the FDTD (Finite Difference Time Domain) method.
[0154] Figure 19 to Figure 35 They are the simulation results of Examples 1 to 16 and Comparative Example 1. Figure 19 to Figure 35 In , the distribution of the normalized enhanced electric field is shown.
[0155] exist Figure 19 to Figure 35 In the figure, α represents the distribution of the enhanced electric field in the XZ section. Specifically, α represents (Ex 2 +Ez 2 ), that is, √(Ex2 +Ez 2 ).exist Figures 19 to 34 In the text, "air interface" refers to the interface between the transparent layer and the air layer. Fig.35 In the figure, "substrate / air interface" refers to the interface between the substrate and the air layer.
[0156] exist Figure 19 to Figure 35 In the figure, β represents the distribution of the enhanced electric field in the XY cross section. Specifically, β represents (Ex 2 +Ez 2 ), that is, √(Ex 2 +Ez 2 ).exist Figures 19 to 34 In the figure, β represents the XY cross section at a position 1 nm closer to the +Z axis direction than the "air interface" represented by α. Fig.35 β1 represents an XY cross section at a position 1 nm closer to the +Z axis direction than the “air interface” represented by α, and β2 represents an XY cross section at a position 100 nm closer to the +Z axis direction than the “substrate / air interface” represented by α.
[0157] like Figures 19 to 34 As shown in β, in Examples 1 to 16, the specified pattern was confirmed at a position 1 nm above the air interface. This is because the SLR and QGM induced by the microstructure enhance the electric field above the air interface. Figures 19 to 34 As shown, it can be seen that an enhanced electric field exists also at a position separated 100 nm upward from the microstructure and further at a position separated 200 nm upward from the microstructure.
[0158] On the other hand, Fig.35 As shown in β2, in Comparative Example 1, no pattern was confirmed at a position 100 nm above the substrate / air interface, and no enhanced electric field existed.
[0159] The above-mentioned embodiment and modification examples are examples and are not limiting. For example, each embodiment and each modification example can be combined as appropriate.
[0160] The present invention includes structures that are substantially the same as the structures described in the embodiments (for example, structures with the same functions, methods and results, or structures with the same purposes and effects). In addition, the present invention includes structures after replacing non-essential parts of the structures described in the embodiments. In addition, the present invention includes structures that can play the same role and effect as the structures described in the embodiments or structures that achieve the same purpose. In addition, the present invention includes structures after adding known technologies to the structures described in the embodiments.
[0161] The following contents are derived from the above-mentioned embodiment and modification examples.
[0162] One method of an electric field enhancing element comprises: a substrate; a plurality of fine structures which are arranged on the substrate and have conductivity; and a transparent layer which covers the plurality of fine structures and the substrate, wherein the enhanced electric field generated by the plurality of fine structures has a maximum value in a perpendicular direction of the substrate at a position on the side of the plurality of fine structures opposite to the substrate and separated from the plurality of fine structures.
[0163] According to this electric field enhancing element, the detection sensitivity can be improved.
[0164] In one embodiment of the electric field enhancing element, the transparent layer is provided between adjacent microstructures among the plurality of microstructures, and a refractive index of the transparent layer is higher than a refractive index of the substrate.
[0165] According to this electric field enhancing element, light can be easily concentrated at the positions of a plurality of fine structures in the perpendicular direction of the substrate.
[0166] In one embodiment of the electric field enhancing element, the enhanced electric field may exist at a position separated from the plurality of fine structures by 100 nm or more in the perpendicular direction.
[0167] According to this electric field enhancement element, even if the target substance is not located in the very vicinity of the microstructure, the detection signal derived from the target substance can be enhanced.
[0168] In one embodiment of the electric field enhancing element, the enhanced electric field may exist at a position separated from the plurality of fine structures by 200 nm or more in the perpendicular direction.
[0169] According to this electric field enhancement element, even if the target substance is not located in the very vicinity of the microstructure, the detection signal derived from the target substance can be enhanced.
[0170] In one embodiment of the electric field enhancing element, the plurality of fine structures may be periodically arranged.
[0171] According to this electric field enhancing element, it is possible to reduce the variation in the intensity of the enhanced electric field in the in-plane direction perpendicular to the perpendicular direction of the substrate.
[0172] In one embodiment of the electric field enhancing element, each of the plurality of microstructures may be made of metal.
[0173] In one embodiment of the electric field enhancement element, the material of the transparent layer may be a dielectric.
[0174] One embodiment of a Raman spectroscopic device includes: one embodiment of the electric field enhancing element; a light source for irradiating light to the electric field enhancing element; and a detector for detecting the light from the electric field enhancing element.
[0175] According to this Raman spectroscopic apparatus, detection sensitivity is high.
Claims
1. An electric field enhancement element, wherein: The electric field enhancement element has: substrate; a plurality of microstructures disposed on the substrate and having conductivity; and a transparent layer covering the plurality of microstructures and the substrate, The enhanced electric field generated by the plurality of fine structures has a local maximum in a perpendicular direction to the substrate at a position on a side of the plurality of fine structures opposite to the substrate and separated from the plurality of fine structures.
2. The electric field enhancement element according to claim 1, wherein: The transparent layer is provided between adjacent microstructures among the plurality of microstructures, The refractive index of the transparent layer is higher than that of the substrate.
3. The electric field enhancement element according to claim 1, wherein: The enhanced electric field exists at a position separated from the plurality of fine structures by 100 nm or more in the vertical direction.
4. The electric field enhancement element according to claim 1, wherein: The enhanced electric field exists at a position separated from the plurality of fine structures by 200 nm or more in the vertical direction.
5. The electric field enhancement element according to claim 1, wherein: The plurality of fine structures are arranged periodically.
6. The electric field enhancement element according to claim 1, wherein: The material of each of the plurality of microstructures is metal.
7. The electric field enhancing element according to claim 1, wherein: The material of the transparent layer is dielectric.
8. A Raman spectroscopy device, wherein: The Raman spectroscopy device has: The electric field enhancement element according to any one of claims 1 to 7; a light source that irradiates light toward the electric field enhancing element; and A detector detects light from the electric field enhancing element.