Furfural molecular adsorption substrate, adsorption method, preparation method and application thereof
By evenly coating the adsorption base of silver nanowires on the filter paper, using the adsorption properties of the filter paper and the hot spot effect of the silver nanowires, the problem of unstable and inefficient adsorption of furfural molecules is solved, and the extremely low concentration of furfural in transformer oil is achieved. Efficient detection improves detection sensitivity and accuracy.
Patent Information
- Application Number
- CN202410717337.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing technology, the adsorption between furfural molecules and SERS substrate is unstable and inefficient, resulting in the inability to accurately detect extremely low concentrations of furfural, which limits the further promotion and application of the technology.
An efficient furfural molecule adsorption substrate is prepared using chemical synthesis and physical processing technology. Through the combination of silver nanowires and filter paper, the adsorption of filter paper and the hot spot effect of silver nanowires are used to achieve efficient adsorption and detection of furfural molecules.
It significantly improves the adsorption and aggregation capabilities of furfural molecules, improves detection sensitivity and accuracy, simplifies the detection process, and can accurately detect extremely low concentrations of furfural in transformer oil.
Smart Images

Figure CN118730995A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of energy and power technology, specifically to the field of detecting furfural molecules in transformer oil based on Raman spectroscopy, and particularly to a furfural molecule adsorption substrate, an adsorption method, a preparation method and applications thereof. Background Art
[0002] Transformer oil is a fractionation product of petroleum, and its main components are compounds such as alkanes, cycloalkanes, saturated aromatic hydrocarbons, and unsaturated aromatic hydrocarbons. It can also be regarded as a mineral oil obtained by distillation and refining of natural petroleum. It usually appears as a light yellow transparent liquid with a relative density of about 0.895 and a freezing point below -45°C.
[0003] Transformer oil has a higher dielectric strength than air, which can protect the insulating material from moisture erosion and improve the overall insulation performance. Due to its large specific heat capacity, transformer oil is often used as a coolant. The heat generated by the transformer during operation can be effectively dissipated through the up and down convection of the oil to ensure the normal operation of the transformer. In oil circuit breakers and transformer on-load tap changers, transformer oil can help improve arc extinguishing performance and extinguish the arc quickly due to its good thermal conductivity and the ability to decompose a large amount of gas at high arc temperatures.
[0004] Furfural is an organic compound that is a colorless, transparent, oily liquid at room temperature. In transformer oil, furfural mainly comes from the aging decomposition products of cotton insulation materials and wood insulation materials. With the long-term use of transformers, especially under the action of high temperature and high pressure, these insulation materials will decompose and produce pollutants such as furfural, which will then contaminate the transformer oil. Therefore, monitoring the furfural content in transformer oil can be used as an important indicator to evaluate the degree of aging of transformer insulation materials.
[0005] Raman spectroscopy is mainly based on the Raman scattering effect. When monochromatic light is irradiated to the transformer oil sample, the furfural molecules in the oil will inelastically scatter the photons. In this process, the frequency of the scattered light will change relative to the incident light, and this frequency shift just carries the vibration and rotation information of the furfural molecules. By carefully analyzing the frequency characteristics of these scattered lights, we can accurately determine the concentration of furfural in the transformer oil. Compared with other traditional methods, Raman spectroscopy detection does not require complex pretreatment of the sample, thus achieving true non-destructive testing. At the same time, due to its fast detection speed, it significantly improves work efficiency.
[0006] Although Raman spectroscopy has many advantages in detecting furfural, it still faces a technical problem: the adsorption problem between furfural molecules and SERS substrates. This adsorption is unstable and inefficient, which seriously affects the signal enhancement effect of the SERS substrate. Therefore, the current technology cannot meet the needs of accurate detection of extremely low concentrations of furfural, which undoubtedly restricts the further promotion and application of this technology.
[0007] To this end, the present invention proposes a furfural molecule adsorption substrate, an adsorption method, a preparation method and applications thereof. Summary of the invention
[0008] In view of this, the embodiments of the present invention hope to provide a furfural molecule adsorption substrate, an adsorption method, a preparation method and an application thereof, so as to solve or alleviate the technical problems existing in the prior art, that is, how to solve the technical problems of unstable and inefficient adsorption, and at least provide a beneficial option for this; the technical solution of the present invention is implemented as follows:
[0009] In the first aspect, the preparation method of furfural molecule adsorption substrate:
[0010] The preparation of the furfural molecule adsorption substrate is a key step to ensure efficient and sensitive detection of furfural content in transformer oil. The following is a detailed preparation method that combines chemical synthesis and physical treatment techniques to ensure the optimal performance of the substrate.
[0011] (I) Preparation of precursor solution:
[0012] Step S1: First, the ethylene glycol solution and the polyvinyl pyrrolidone powder are fully stirred and mixed until they are completely dissolved to form solution A. This step ensures the presence of the stabilizer and dispersant required in the subsequent reaction.
[0013] Step S2: Next, ethylene glycol and silver nitrate powder are stirred and mixed to obtain a B solution containing silver ions, which is the main silver source for the subsequent synthesis of silver nanowires.
[0014] Step S3: At the same time, ethylene glycol and ferric chloride powder are stirred and mixed to obtain solution C. Ferric chloride serves as a catalyst for the reaction, which helps to control the morphology and size of the silver nanowires.
[0015] (II) Preparation and synthesis of silver nanowires:
[0016] Step S4: Place solution A in a flask and heat it in an oil bath. During the heating process, slowly add solution B and solution C dropwise. This step is the key to the synthesis of silver nanowires and requires precise control of the solution drop rate and reaction temperature.
[0017] Step S5: Use a magnetic stirrer to continuously stir the mixed solution in the flask while keeping the temperature of the flask stable. This helps to ensure the uniformity and consistency of the reaction.
[0018] Step S6: After the reaction is completed, the flask is allowed to cool naturally. Subsequently, the reaction solution is drawn out for washing to obtain a pure silver nanowire sol. This step is mainly used to remove impurities and unreacted substances generated during the reaction.
[0019] (III) Preparation of adsorption substrate:
[0020] Step S7: Place the filter paper at the bottom of the cuvette and put it into a vacuum drying oven for drying. At the same time, the nanowires in the silver nanowire sol are dispersed to ensure that they can be evenly distributed on the filter paper.
[0021] Step S8: Add the silver nanowire sol dropwise onto the filter paper to ensure that the silver nanowires can evenly cover the surface of the filter paper. In this way, an efficient furfural molecule adsorption substrate is prepared.
[0022] (IV) Preparation of sample solution:
[0023] Step S9: In order to simulate the actual application scenario, the new transformer oil is placed in a vacuum drying oven for pretreatment to remove moisture and impurities therein.
[0024] Step S10: Add the pure furfural solution dropwise into the pretreated transformer oil to prepare a furfural-transformer oil sample solution. This step is to simulate the furfural content in the actual transformer oil for subsequent detection and analysis.
[0025] In one embodiment, in steps S1 to S3, the preparation amounts of solution A, solution B and solution C are 22 mL, 3 mL and 3 mL respectively. These precise solution amounts are optimized to ensure the stability and efficiency of subsequent silver nanowire synthesis.
[0026] In one embodiment, in step S4, the heating temperature is set to 150°C. This temperature is selected based on the optimal conditions for the synthesis of silver nanowires, which helps to obtain high-quality silver nanowires. At the same time, in this step, the dripping time of B and C solutions is not less than 15 minutes. This time control ensures that the reactants can be added to the reaction system evenly and slowly, thereby avoiding uneven reactions caused by excessive local concentrations.
[0027] In one embodiment, in step S5, the stirring time is not less than 1.5 hours. This time length is to ensure that the reactants can be fully mixed and reacted, so as to obtain silver nanowires with uniform morphology and stable performance.
[0028] In one embodiment, in step S6, the synthetic solution is repeatedly cleaned using a centrifuge tube and an ultrasonic cleaner. Alcohol is selected as the cleaning solution because alcohol can effectively remove impurities and unreacted substances generated during the reaction. The number of cleanings is no less than 5 times to ensure that the purity of the silver nanowires is the highest. The speed of the centrifuge is set to 3000 rpm, which can effectively separate the silver nanowires while avoiding damage to them.
[0029] In one embodiment, in step S7, the drying time of the filter paper is 10 minutes. This time length can ensure that the filter paper is completely dried, and its adsorption performance will not be affected by over-drying. At the same time, in this step, the silver nanowire sol is placed in an ultrasonic cleaning machine for 5 minutes to fully disperse the nanowires.
[0030] Second, furfural molecule adsorption method:
[0031] In the process of furfural molecule detection, in order to ensure the accuracy and sensitivity of the detection, the parameters of the detection system need to be accurately set and the operation should be carried out strictly according to the steps. The following is a detailed adsorption and detection method:
[0032] (I) Setting the parameters of the confocal Raman spectroscopy detection system:
[0033] The grating was set to 1200 l / mm to improve the resolution and accuracy of the spectrum.
[0034] The slit width was adjusted to 100 to optimize the optical path and ensure that more light signals could enter the detector, thus improving the signal-to-noise ratio.
[0035] Next, we follow the steps below to adsorb and detect furfural molecules:
[0036] (II) The first step, adsorption process:
[0037] The prepared surface enhanced Raman spectroscopy substrate is immersed in a sample solution containing furfural molecules.
[0038] Allow the substrate to stand in the sample solution for no less than 4 hours to ensure that the furfural molecules have enough time to adsorb on the substrate. This is a key step to ensure that the subsequent Raman spectroscopy detection can accurately capture the furfural molecular signal.
[0039] (III) Step 2: Preparation for testing:
[0040] Place the sample solution soaked with the substrate on the stage of the microscope to prevent the substrate from being damaged or moved. Adjust the focus and position of the microscope so that the furfural molecules on the substrate can be clearly observed.
[0041] (IV) Step 3: Spectral collection and analysis:
[0042] The Raman spectrum information on the substrate is collected using a confocal Raman spectroscopy detection system. During this process, the system emits a laser and collects light signals scattered back from the substrate. By analyzing these signals, vibration information about the furfural molecules can be obtained.
[0043] Import the collected Raman spectrum information into the origin drawing software and draw a spectrum. In the spectrum, we can observe different Raman characteristic peaks, which represent different vibration modes of furfural molecules.
[0044] 1703 is selected as the Raman characteristic peak of furfural in transformer oil. This characteristic peak is generated by the unique vibration frequency of furfural molecules, so it can be used as a sign to identify furfural molecules. By observing the presence and intensity of this characteristic peak, we can determine whether furfural exists in the sample and the concentration of furfural.
[0045] Thirdly, furfural molecule adsorption substrate:
[0046] The furfural molecule adsorption substrate is made through the above-mentioned detailed preparation technology process and is specially designed to implement the furfural molecule adsorption method described above. This substrate not only carries the key function of efficiently adsorbing furfural molecules, but also is the core component to ensure the accuracy and sensitivity of the entire detection process.
[0047] During the preparation process, various parameters and conditions were strictly controlled to ensure that the substrate had excellent adsorption performance and stability. By optimizing the synthesis conditions of silver nanowires and precisely controlling the composition and structure of the substrate, we successfully created this high-performance adsorption substrate.
[0048] When the furfural molecule adsorption method is performed, this substrate can quickly and effectively adsorb furfural molecules in the sample solution. Its unique surface structure and chemical properties enable furfural molecules to be tightly bound to the substrate, which facilitates subsequent Raman spectroscopy detection. The furfural molecule adsorption substrate is a key link in the entire detection scheme. It not only provides the possibility for efficient adsorption of furfural molecules, but also ensures the reliability and accuracy of the test results. Combined with the aforementioned adsorption method, this substrate provides a solid foundation for the accurate determination of furfural content in transformer oil.
[0049] Fourthly, the application of furfural molecular adsorption substrate in the detection of furfural in transformer oil:
[0050] The furfural molecule adsorption substrate can quickly capture furfural molecules in transformer oil through its efficient adsorption capacity. Combined with the confocal Raman spectroscopy detection system, the furfural content in transformer oil can be accurately identified and quantitatively measured. This application not only improves the sensitivity and accuracy of detection, but also greatly shortens the detection time, providing a strong guarantee for the safe operation of the power system.
[0051] In actual operation, the furfural molecule adsorption substrate is first immersed in the transformer oil sample to be tested, allowing the substrate to fully adsorb the furfural molecules in the oil. Subsequently, the substrate adsorbed with furfural molecules is placed on the microscope stage, and the spectral information is collected by the confocal Raman spectroscopy detection system. The characteristic peaks of furfural molecules can be easily identified using professional analysis software, and the furfural content in the transformer oil can be accurately calculated based on this.
[0052] Compared with the prior art, the present invention has the following beneficial effects:
[0053] 1. Solve the problem of unstable adsorption and low efficiency: The present invention contacts the treated filter paper with the furfural solution in the transformer oil, and uses the adsorption property of the filter paper to effectively adsorb and deposit the furfural molecules on the paper surface. In this process, silver nanowires play a key role, and the hot spot areas formed by them significantly increase the aggregation density of furfural molecules. Then, strong electric and electromagnetic fields are formed on the filter paper through the silver nanowires, like "magnetic field traps", which greatly enhance the adsorption and aggregation ability of furfural molecules. This hot spot effect makes the furfural molecules highly concentrated around the silver nanowires, thereby significantly improving the sensitivity of detection. At the same time, the tiny size and wide surface area of the silver nanowires also provide abundant adsorption sites for furfural molecules, further optimizing the adsorption efficiency.
[0054] Second, the detection process is simplified: The present invention achieves efficient and low-concentration detection of furfural molecules in transformer oil by cleverly combining the adsorption of filter paper and the hotspot effect of silver nanowires. By combining the adsorption of filter paper and the hotspot effect of silver nanowires, this solution achieves efficient adsorption and detection of furfural molecules, significantly improving the sensitivity of detection. Not only does it simplify the detection process, but it also raises the detection sensitivity to a new level, providing a strong guarantee for the safe and stable operation of the power system. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or technical descriptions will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0056] Figure 1It is a schematic flow chart of the preparation method of the furfural molecule adsorption substrate of the present invention;
[0057] Figure 2 Schematic diagram of the implementation steps of the furfural molecule adsorption method of the present invention;
[0058] Figure 3 The paper-based SERS substrate image of the present invention;
[0059] Figure 4 This is an electron microscope image of the SERS substrate of the present invention;
[0060] Figure 5 This is a Raman spectrum diagram for detecting furfural in transformer oil in the solution of the present invention. DETAILED DESCRIPTION
[0061] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below;
[0062] It should be noted that the various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments, and the same or similar parts between the various embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part description.
[0063] Example 1: Please refer to Figure 1 , this embodiment discloses a method for preparing a furfural molecule adsorption substrate:
[0064] The method of this embodiment combines chemical synthesis technology and physical treatment technology, aiming to optimize the adsorption performance of the substrate, thereby improving the detection sensitivity and efficiency of furfural content in transformer oil. Through precise preparation steps, we successfully synthesized silver nanowires and evenly coated them on filter paper, thereby forming an efficient furfural molecule adsorption substrate. Including:
[0065] (I) Preparation of precursor solution:
[0066] 1.1 Preparation of stabilizer and dispersant solution (Solution A):
[0067] Mix a certain amount of ethylene glycol solution with polyvinyl pyrrolidone powder.
[0068] Continue stirring until polyvinyl pyrrolidone is completely dissolved in ethylene glycol to form a stable and uniform solution A. This step ensures the effective supply of stabilizer and dispersant during the reaction.
[0069] 1.2 Prepare silver source solution (Solution B):
[0070] Mix ethylene glycol and silver nitrate powder and stir thoroughly.
[0071] Until the silver nitrate is completely dissolved, a solution B containing silver ions is obtained, which provides a silver source for the subsequent synthesis of silver nanowires.
[0072] 1.3 Preparation of catalyst solution (C solution):
[0073] Mix ethylene glycol and ferric chloride powder.
[0074] until the ferric chloride is dissolved to obtain solution C. Ferric chloride acts as a catalyst in the reaction and plays a key role in controlling the morphology and size of the silver nanowires.
[0075] Specifically, the preparation amounts of solution A, solution B, and solution C are 22 mL, 3 mL, and 3 mL, respectively. These precise solution amounts are optimized ratios to ensure the stability and efficiency of subsequent silver nanowire synthesis.
[0076] (II) Synthesis of silver nanowires:
[0077] 2.1 Heating and adding precursor solution:
[0078] Place solution A in a flask and heat it in an oil bath at a preset temperature.
[0079] While heating, slowly and dropwise add solution B and solution C. The dropwise addition speed and reaction temperature must be precisely controlled to ensure the quality of the silver nanowires.
[0080] 2.2 Stirring and reaction control:
[0081] The mixed solution in the flask was stirred continuously and evenly using a magnetic stirrer.
[0082] Keep the temperature in the flask stable to ensure the smooth progress of the reaction and the uniformity of the product.
[0083] 2.3 Post-reaction treatment:
[0084] After the reaction was completed, the flask was allowed to cool naturally to room temperature.
[0085] The solution after the reaction is taken out for multiple washings to remove impurities and unreacted substances, and finally a pure silver nanowire sol is obtained.
[0086] Specifically, the heating temperature is set to 150°C. This temperature is selected based on the optimal conditions for the synthesis of silver nanowires, which helps to obtain high-quality silver nanowires. At the same time, in this step, the dripping time of B and C solutions is not less than 15 minutes. This time control ensures that the reactants can be added to the reaction system evenly and slowly, thereby avoiding uneven reactions caused by excessive local concentrations.
[0087] Specifically, the stirring time is not less than 1.5 hours, which is to ensure that the reactants can be fully mixed and reacted, so as to obtain silver nanowires with uniform morphology and stable performance.
[0088] Specifically, the synthetic solution is repeatedly cleaned using a centrifuge tube and an ultrasonic cleaner. Alcohol is selected as the cleaning solution because it can effectively remove impurities and unreacted substances generated during the reaction. The number of cleanings is no less than 5 times to ensure that the purity of the silver nanowires is as high as possible. The speed of the centrifuge is set to 3000 rpm, which can effectively separate the silver nanowires while avoiding damage to them.
[0089] (III) Preparation of adsorption substrate:
[0090] 3.1 Filter paper pretreatment and silver nanowire dispersion:
[0091] Lay the filter paper flat on the bottom of the cuvette and dry it in a vacuum oven.
[0092] At the same time, the silver nanowire sol is dispersed to ensure that the silver nanowires can be evenly coated on the filter paper.
[0093] 3.4 Coating of silver nanowire sol:
[0094] The dispersed silver nanowire sol was added drop by drop onto the dried filter paper.
[0095] Ensure that the silver nanowires evenly cover the entire filter paper surface, thereby completing the preparation of an efficient furfural molecule adsorption substrate. Figures 3-4 shown.
[0096] (IV) Preparation of sample solution:
[0097] 4.1 Pretreatment of transformer oil:
[0098] Place the new transformer oil in a vacuum drying oven for pretreatment to remove moisture and impurities in the oil to ensure the accuracy of subsequent testing.
[0099] 4.2 Preparation of furfural-transformer oil sample solution:
[0100] A certain amount of pure furfural solution is added dropwise to the pretreated transformer oil. After thorough mixing, a sample solution simulating the furfural content in the actual transformer oil is prepared for subsequent detection and analysis.
[0101] Specifically, the drying time of the filter paper is 10 minutes. This time length can ensure that the filter paper is completely dry, and will not affect its adsorption performance due to over-drying. At the same time, in this step, the silver nanowire sol is placed in an ultrasonic cleaning machine for 5 minutes to fully disperse the nanowires.
[0102] Example 2: Please refer to Figure 2 Based on the furfural molecule adsorption substrate prepared in Example 1, this example further discloses a method for adsorbing furfural molecules:
[0103] In order to ensure high accuracy and sensitivity in the detection of furfural molecules, this embodiment proposes a detailed adsorption and detection method on a prepared furfural molecule adsorption substrate. By accurately setting the parameters of the confocal Raman spectroscopy detection system and strictly following the operating steps, we can effectively capture the characteristic spectral signals of furfural molecules, thereby achieving qualitative and quantitative analysis of them.
[0104] (I) Confocal Raman spectroscopy detection system parameter settings:
[0105] Before detecting furfural molecules, it is necessary to first accurately set the key parameters of the confocal Raman spectroscopy detection system to ensure that the system is in the best working state. The specific parameters are as follows:
[0106] 1.1 Grating settings:
[0107] A grating of 1200l / mm was selected to improve the resolution of the spectrum and ensure that different chemical bond vibration modes can be clearly distinguished, thereby improving the accuracy of detection.
[0108] 1.2 Slit width adjustment:
[0109] The slit width is set to 100 to optimize the optical path configuration of the system. This setting helps more light signals enter the detector, thereby improving the signal-to-noise ratio, so that weak signals can also be effectively captured.
[0110] (II) Adsorption and detection steps of furfural molecules:
[0111] 2.1 Base immersion:
[0112] The previously prepared surface-enhanced Raman spectroscopy substrate was immersed in a sample solution containing furfural molecules.
[0113] 2.2 Static adsorption:
[0114] Keep the substrate in the sample solution for at least 4 hours to ensure that the furfural molecules have sufficient time to adsorb to the substrate surface.
[0115] (III) Preparation for testing:
[0116] 3.1 Sample placement:
[0117] Place the sample solution soaked with the substrate on the stage of the microscope, making sure that the substrate is not damaged and is fixed in position.
[0118] 3.2 Microscope adjustment:
[0119] Finely adjust the focus and field position of the microscope to obtain a clear image of the furfural molecules on the substrate.
[0120] (IV) Spectral collection and analysis:
[0121] Spectral acquisition:
[0122] 4.1 Use the confocal Raman spectroscopy detection system to collect spectral information of the substrate. The system obtains the vibration information of furfural molecules by emitting lasers and capturing the light signals scattered back from the substrate.
[0123] 4.2 Spectral processing:
[0124] Import the collected Raman spectrum data into the professional origin drawing software to generate a spectrum diagram such as Figure 5 In the spectrum, different Raman characteristic peaks can be clearly identified, which correspond to the specific vibration modes of furfural molecules.
[0125] 4.4 Characteristic peak analysis:
[0126] like Figure 5 As shown, 1703 is identified as the characteristic Raman peak of furfural in transformer oil. This characteristic peak is generated by the unique vibration frequency of furfural molecules and can therefore be used as a reliable marker for identifying furfural. By observing the presence and intensity of this characteristic peak, we can accurately determine the presence and concentration of furfural in the sample.
[0127] It is understandable that, for the technical solution of this embodiment, the core of this solution is to combine the adsorption of filter paper with the hot spot effect of silver nanowires. With its strong adsorption capacity, filter paper can effectively adsorb and fix furfural molecules in transformer oil on the paper surface. The silver nanowires coated on the filter paper significantly increase the aggregation density of furfural molecules by forming hot spot areas, thereby greatly improving the sensitivity of detection. Therefore, this technical solution successfully solves the problems of low sensitivity and complicated operation of furfural molecule detection in transformer oil by cleverly combining the adsorption characteristics of filter paper and the hot spot effect of silver nanowires. This solution is efficient, simple, sensitive and widely applicable, and provides strong technical support for status monitoring and fault diagnosis of power system equipment.
[0128] All the above embodiments only express the implementation methods of the relevant practical applications of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.
Claims
1. A method for adsorbing furfural molecules, comprising using a confocal Raman spectroscopy detection system for detection, characterized in that: The steps include: S1, immersing the prepared surface enhanced Raman spectroscopy substrate in a sample solution and allowing it to stand; S2, placing the sample solution soaked with the surface enhanced Raman spectroscopy substrate on the microscope stage; S3, collecting spectra, obtaining Raman spectrum information, and obtaining Raman characteristic peaks of furfural in transformer oil.
2. The adsorption method according to claim 1, characterized in that: The confocal Raman spectroscopy detection system uses a 1200 l / mm grating, and the slit width is adjusted to 100.
3. The adsorption method according to claim 1, characterized in that: In S1, the standing time is not less than 4 hours.
4. A method for preparing a furfural molecule adsorption substrate, characterized in that: The substrate as claimed in any one of claims 1 to 3 is prepared by the following method: S1, stirring and mixing the ethylene glycol solution and the polyvinyl pyrrolidone powder to dissolve to obtain a solution A; S2, stirring and mixing the ethylene glycol solution and the silver nitrate powder to dissolve, to obtain a solution B; S3, stirring and mixing the ethylene glycol solution and the ferric chloride powder to dissolve, to obtain a C solution; S4, pouring solution A into a flask, and then placing the flask in an oil bath to heat it, during which time solutions B and C are added dropwise into the flask; S5, using magnetic stirring to maintain the flask temperature; S6, after the reaction is completed and the flask is cooled naturally, the reaction solution is sucked out to obtain a synthetic solution; then the synthetic solution is washed to obtain a silver nanowire sol; S7, placing the filter paper at the bottom of the cuvette and placing it in a vacuum drying oven to dry; at the same time, the nanowires of the silver nanowire sol are dispersed; S8, adding the silver nanowire solution dropwise onto the filter paper to ensure that the silver nanowires are evenly distributed on the surface of the filter paper to obtain the substrate.
5. The preparation method according to claim 4, characterized in that: In S1 to S3, the A solution, the B solution and the C solution are 22 mL, 3 mL and 3 mL respectively; In S4, the heating temperature is 150° C., and the dropping time is not less than 15 minutes; In S5, the stirring time is not less than 1.5 h.
6. The preparation method according to claim 4, characterized in that: In S6, the synthetic solution is repeatedly cleaned by using a centrifuge tube and an ultrasonic cleaner for no less than 5 times, and the speed of the centrifuge is set to 3000 rpm to obtain the silver nanowire sol.
7. The preparation method according to claim 4, characterized in that: In S7, the drying time is 10 minutes; the silver nanowire sol is placed in an ultrasonic cleaning machine for 5 minutes to disperse the nanowires.
8. The preparation method according to claim 4, characterized in that: It is also necessary to configure a furfural-transformer oil sample to cooperate with the base to implement the adsorption method according to any one of claims 1 to 3; comprising the following steps: S9, placing the new transformer oil in a vacuum drying oven for drying pretreatment; S10, the absorbed pure furfural solution is added dropwise into the transformer oil to obtain a furfural-transformer oil sample solution.
9. Furfural molecule adsorption substrate, characterized in that: The invention is prepared by the preparation method according to any one of claims 4 to 8.
10. Use of the adsorption substrate as claimed in claim 9 in detecting furfural in transformer oil.