Application of gallium-based chalcogenide scintillation crystal doped with rare earth elements in humidity measurement

By using gallium-based chalcogenide scintillation crystals doped with rare earth elements and utilizing their spontaneous absorption of water molecules, the problem of inaccurate measurement of existing humidity sensors in extreme environments is solved, and high-accuracy and high-sensitivity humidity detection is achieved. .

CN118731077APending Publication Date: 2024-10-01FUJIAN INST OF RES ON THE STRUCTURE OF MATTER CHINESE ACAD OF SCI +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410684444.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing humidity sensors are easily affected by environmental factors in extreme environments and long-term use, resulting in inaccurate measurement results and precision and accuracy challenges.

Method used

Gallium-based chalcogenide scintillation crystals doped with rare earth elements are used to replace AgGaS2 cations with alkali metal atoms Na to increase the band gap value of the compound, and adjust its radioluminescence properties with rare earth ions, taking advantage of its spontaneous absorption of water molecules. Humidity detection.

Benefits of technology

It achieves high-accuracy humidity measurement under extreme conditions. The material exhibits higher light yield and sensitivity than BGO materials. It can spontaneously absorb water molecules and conduct humidity detection through luminescence quenching, which significantly improves the accuracy of humidity measurement. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118731077A_ABST
    Figure CN118731077A_ABST
Patent Text Reader

Abstract

The invention discloses a gallium-based chalcogenide scintillation crystal doped with rare earth elements and application of the gallium-based chalcogenide scintillation crystal in humidity measurement, and belongs to the technical field of crystal materials. The chemical formula of the gallium-based chalcogenide scintillation crystal doped with the rare earth elements is Na < 1-x > GaS2: xEu, and x is 1%-9%. The crystal can well absorb X rays, the light yield of the series of crystals is higher than that of BGO, the performance of the series of crystals in the aspect of X-ray radiation is 2-3 times that of BGO material response, and the overall excellent performance shows important application value in X-ray detection. Moreover, the crystal shows the unique characteristic that water molecules can be spontaneously absorbed from air to enter structural layers, has good humidity response capability, and can play an important role in humidity measurement application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the application of a rare earth element-doped gallium-based sulfide compound scintillation crystal in humidity measurement, belonging to the technical field of crystal materials. Background Art

[0002] Based on the characteristic of converting high-energy rays such as X-rays and gamma rays into ultraviolet or visible light, scintillating materials have been widely used in many fields such as medical diagnosis, industrial inspection, nuclear physics, scientific research, etc.

[0003] Humidity detection plays an increasingly important role in various applications, from industrial automation to smart homes, from healthcare to environmental monitoring, among which humidity sensors are widely used. Although the existing humidity sensor technology is quite mature, there are still challenges in precision and accuracy. The measurement results of humidity sensors may be affected by the surrounding environmental conditions, such as chemicals, electromagnetic interference or mechanical vibration, etc. Especially under extreme conditions (such as high temperature, low temperature or high environment) and in long-term use, the sensor may drift or performance degrade, resulting in inaccurate measurement results.

[0004] Therefore, there is an urgent need to develop a humidity detection material with stable performance that is not affected by environmental factors and can be used in extreme conditions. Summary of the invention

[0005] In order to solve the problem in the prior art that the measurement results of humidity sensors are easily affected by the environment, sensor structure and circuit design, resulting in errors, the present application provides a new humidity measurement material and scheme, and applies gallium-based sulfide compound scintillation crystals doped with rare earth elements to humidity measurement, and replaces AgGaS2 cations with alkali metal atoms Na to effectively increase the band gap value of the compound, and adjusts its radioluminescence performance by doping rare earth ions. NaGaS2 crystals doped with different concentrations of rare earth elements are prepared by a high-temperature solid-phase method, and their x-ray radioluminescence is characterized. During the research process, it was found that NaGaS2 has the property of spontaneously absorbing water molecules from the atmosphere into its structure compared with other MGaS2 (M=Li, K, Rb) system compounds. Based on the regulating effect of this property on its radioluminescence degree, it is applied to the field of humidity detection.

[0006] This application adopts the following technical solutions:

[0007] According to one aspect of the present application, there is provided an application of a rare earth element-doped gallium-based chalcogenide scintillator crystal in humidity measurement, wherein the chemical formula of the rare earth element-doped gallium-based chalcogenide scintillator crystal is:

[0008] Na 1-x GaS2:xEu;

[0009] Here, x is 1% to 9%.

[0010] Optionally, the humidity measurement process includes:

[0011] The gallium-based chalcogenide scintillating crystal doped with a rare earth element is heated at 80 to 100° C. for 60 to 180 minutes to obtain an initial state crystal;

[0012] Then the initial state crystal is placed in an environment with the humidity to be tested for 300 to 600 seconds. After the crystal in the test state is obtained, an X-ray excitation spectrum test is performed on it and the humidity value is obtained by comparing it with the database.

[0013] In the present application, after being exposed to the atmosphere, the gallium-based chalcogenide scintillating crystal doped with rare earth elements will rapidly undergo a structural transformation after absorbing water, and importantly, this transformation is reversible.

[0014] Optionally, the database is a data set of X-ray excitation spectra of the initial state crystal at different temperatures after being kept in different humidity environments for different periods of time.

[0015] The present application aims to apply the prepared rare earth element-doped gallium-based sulfide compound scintillation crystals in the field of humidity detection based on the property that the prepared gallium-based sulfide compound scintillation crystals can spontaneously absorb water molecules from the air into the structural layers and cause the luminescence quenching of the material. The size of the database and the test conditions are not strictly limited in the present application. Those skilled in the art can use existing technologies to establish a database according to needs. The comparison method between the test results and the database can be a table lookup method or obtained by fitting a model. The fitting model can be obtained by model training based on the above database using the algorithm of the existing technology.

[0016] Optionally, the X-ray response of the rare earth element-doped gallium-based chalcogenide scintillating crystal is 2 to 3 times that of the BGO material.

[0017] Optionally, the light yield of the rare earth element-doped gallium-based chalcogenide scintillation crystal is greater than or equal to 8000 ph / MeV.

[0018] Optionally, a scintillation sensitivity ratio of the rare earth element-doped gallium-based chalcogenide scintillator crystal to the ZnS:Ag material is greater than or equal to 3.

[0019] Optionally, the method for preparing the rare earth element-doped gallium-based chalcogenide scintillation crystal comprises the following steps:

[0020] S1. Grind and mix the raw materials containing Na2S, Ga2S3 and EuS with I2 in an inactive atmosphere to obtain a mixture;

[0021] S2, placing the mixture in a vacuum sealed container and heating it in a temperature gradient zone to maintain a constant temperature, cooling it after the crystal grows, to obtain the rare earth element-doped gallium-based chalcogenide scintillation crystal;

[0022] The temperature gradient zone includes a high temperature zone and a low temperature zone connected to each other;

[0023] The mixture is located in a high temperature zone;

[0024] The rare earth element-doped gallium-based chalcogenide scintillation crystal is located in a low temperature region.

[0025] Optionally, in step S1, Na2S, Ga2S3 and EuS in the raw materials are weighed according to the chemical formula composition and stoichiometric ratio of the rare earth element-doped gallium-based chalcogenide scintillating crystal;

[0026] The amount of I2 used is 0.1 to 1 wt% of the raw material weight.

[0027] Optionally, the vacuum degree of the vacuum sealed container is 1×10 -4 1×10 -6 Entrust.

[0028] Optionally, the grinding time is 5 to 30 minutes.

[0029] Optionally, in step S2, the conditions for heating to a constant temperature include:

[0030] The preset temperature of the high temperature zone is 1000-1100°C;

[0031] The preset temperature of the low temperature zone is 750~850℃;

[0032] The high temperature zone and the low temperature zone are independently kept at a constant temperature for 90 to 120 hours;

[0033] Optionally, the heating and constant temperature conditions also include: heating the high temperature zone and the low temperature zone at a heating rate of 3 to 5° C. / h.

[0034] Optionally, the heating and constant temperature conditions also include: when heating the high temperature zone and the low temperature zone, independently keeping the temperatures at 300° C., 500° C. and 700° C. for 180 to 300 minutes respectively.

[0035] The beneficial effects of this application include:

[0036] The present application proposes an application of a novel rare earth element-doped gallium-based sulfide compound scintillation crystal in humidity measurement. The crystal is grown by a high-temperature solid phase method, wherein the introduction of alkali metal increases the band gap of the compound and increases the atomic number of the compound, and can absorb X-rays well. This series of crystals can show a light yield higher than that of BGO, and the performance in X-ray radiation is 2 to 3 times that of the BGO material response. The crystal exhibits a unique ability to spontaneously absorb water molecules from the air into the interlayer of the structure, and by combining the luminescence quenching effect of water on the material, it can be applied to the field of precise measurement of humidity, giving full play to the scintillation performance of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 For different proportions of Eu 2+ XEL spectrum of ion-activated NaGaS2 matrix material.

[0038] Figure 2 This is a comparison of the light yield of this application with commercial BGO and other crystals.

[0039] Figure 3 For this application Eu 2+ The hydrated and anhydrous phases of ion-activated NaGaS2 and the comparative sample BGO at different X-ray doses (from 0.686 to 42.293 mGy air / s) sensitivity and detection limit under radiation stimulation;

[0040] Figure 4 For this application Eu 2+ The hydrated and anhydrous phases of ion-activated NaGaS2 are (2.81×10 -5 to 4.34×10 -3 mxD air / s) radiation stimulation. DETAILED DESCRIPTION

[0041] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0042] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0043] Unless otherwise specified, conventional methods were used for testing and instrument settings were those recommended by the manufacturer.

[0044] The XEL spectra and light yield were obtained by testing and collecting photon counting and spectrum acquisition equipment equipped with a (W-target, 5W) X-ray source, and the PL spectra were tested using an Edinburgh FLS1000 fluorescence spectrometer.

[0045] According to an implementation method of the present application

[0046] The chemical formula of the rare earth element doped gallium-based chalcogenide scintillating crystal provided in the present application is Na 1-x GaS2:xEu, where x=1~9%.

[0047] The present invention provides Na 1-x The method of preparing GaS2:xEu raw materials and growing crystals is as follows:

[0048] The raw material preparation is as follows:

[0049] In the glove box environment, high-purity Na2S and Ga2S3 were accurately weighed according to the stoichiometric ratio. For doped samples, in addition to the above-mentioned main materials, a corresponding proportion of EuS was also added. After these raw materials were evenly mixed, they were put into an agate mortar and fully ground to obtain fully mixed raw materials.

[0050] Raw material packaging, as follows:

[0051] The obtained Na 1-x The GaS2:xEu raw materials were placed in a numbered quartz tube (about 15 cm in length and 9 mm in diameter) in a glove box. The top of the quartz tube was plugged tightly with a rubber stopper. After being taken out of the glove box, the numbered quartz tube was sealed with a self-assembled vacuum tube sealing system under vacuum using an oxyhydrogen flame. After sealing the tube, Na 1-x GaS2:xEu crystal growth.

[0052] Crystal growth, as follows:

[0053] Transfer the well-sealed quartz tube to a dual-temperature zone tubular furnace, and raise the temperature of the high-temperature zone and the low-temperature zone under the program setting of the temperature controller. Keep the constant temperature for a certain period of time, and the I2 vapor carries the reactants from the high-temperature side to the low-temperature side for cooling and crystallization. Finally, turn off the power of the equipment after the temperature slowly drops to 300°C, carefully take out the quartz tube after the temperature cools to room temperature, collect the synthesized product, and grind it evenly for further testing and analysis. Among them, since the melting point of sulfur is 115°C and the boiling point is 445°C, the sealed quartz tube will not be able to withstand the high sulfur vapor pressure and explode, so keep the temperature slowly during the heating stage, and set the temperature gradient at the same time, and keep it warm at 300°C, 500°C and 700°C for a while.

[0054] In addition, since the prepared rare earth element-doped gallium-based chalcogenide scintillating crystal has water absorption characteristics, in order to accurately measure its performance, it is further prepared into an organic-inorganic composite film for measurement during the test. This method can effectively avoid the luminescence quenching caused by NaGaS2:Eu spontaneously absorbing water molecules from the air into the interlayer of the structure. The details are as follows:

[0055] In a glove box environment, accurately weigh the NaGaS2:Eu sample and mix it with epoxy resin. After sufficient stirring to eliminate large bubbles on the surface, place the mixed sample in a vacuum deoxidation tank to eliminate small bubbles. Then, the mixture is coated on polyethylene terephthalate (PET) by blade coating and then cured by heating. Finally, a composite film of NaGaS2:Eu and epoxy resin is formed on the PET plastic substrate.

[0056] Preparation Example 1 NaGaS2:Eu Single Crystal Growth

[0057] First, weigh the corresponding raw materials 0.1193g NaS, 0.1193g Ga2S3 and a trace amount of EuS (the amount added is 7wt% based on the total weight of the raw materials) according to the stoichiometric ratio, and add a small amount of I2 as a vapor transmission medium. Then, grind in an agate mortar under the protection of an inert atmosphere for about 20 minutes to fully mix them. Thereafter, the mixed reaction raw materials are loaded into numbered quartz tubes (about 15cm in length and about 9mm in diameter). Next, vacuumize the quartz tubes one by one (1×10 -4 Then, the treated quartz tube was transferred to a tube furnace with two heating zones, and the two heating zones were set to 1050°C as a high temperature zone and 800°C as a low temperature zone and maintained for 100h and 120h respectively, and then the power was turned off.

[0058] Among them, the temperature is slowly increased at 4°C per hour during the heating stage to prevent the reaction from being too intense and causing the tube to explode. Since the melting point of sulfur is 115°C and the boiling point is 445°C, the sealed quartz tube will not be able to withstand the high sulfur vapor pressure and will explode. Therefore, the temperature is slowly increased during the heating stage, and the temperature gradient is set at 300°C, 500°C and 700°C for 300 minutes to allow the reactants to react fully and prevent the reaction from being too intense and causing the tube to explode. During the entire reaction process, the quartz tube is placed under the protection of flowing nitrogen for heating. Finally, after the temperature slowly drops to 300°C, turn off the power of the equipment. When the temperature drops to room temperature, some high-quality NaGaS2:Eu single crystals will be collected from the quartz tube.

[0059] Preparation Examples 2 to 9 Growth of NaGaS2:Eu Single Crystals with Different Eu Doping Amounts

[0060] The preparation methods are the same as those in Example 1, except that the amounts of EuS added are different, which are 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 8wt% and 9wt% respectively based on the Eu element in the total weight of the raw materials.

[0061] Preparation Example 10 NaGaS2:Eu composite thin film

[0062] In a glove box environment, accurately weigh 1g of the newly prepared NaGaS2:Eu single crystal sample of Example 1, and mix it with 1.125g of epoxy resin and 0.375g of curing agent after sufficient grinding. After standing for 10 minutes to eliminate large bubbles on the surface, place it in a vacuum deoxidation tank to eliminate small bubbles. Then use a scraper coating method to coat it on polyethylene terephthalate (PET). By using scrapers of different sizes to control the film thickness, 50μm, 100μm, and 150μm scrapers are used for three-layer coating to ensure the uniformity of the film. Then cure at 80°C for 8h. Finally, a composite film of NaGaS2:Eu and epoxy resin is formed on the PET plastic substrate, that is, the NaGaS2:Eu in the composite film is anhydrous.

[0063] Application Test Example 1

[0064] Examples 1 to 9 Different ratios of Eu 2+ XEL spectra of ion-activated NaGaS2 matrix materials are shown in Figure 2. Figure 1 As shown, with Eu 2+ With the increase of ion doping ratio, the XEL intensity first increases and then decreases, and the highest intensity appears at 7% Eu 2+ Ion doping.

[0065] The light yield of the newly prepared NaGaS2:Eu single crystal in Example 1 of the present application is compared with that of commercial BGO, BaF2, and PbWO4 crystals. Figure 2 As shown, NaGaS2:Eu single crystals exhibit light yield values ​​comparable to commercial BGO and much higher than BaF2 and PbWO4 crystals.

[0066] The newly prepared NaGaS2:Eu single crystal in Example 1 of the present application was stored in a 40% humidity environment for 600s (i.e., a NaGaS2:Eu hydrate phase was formed), and the NaGaS2:Eu composite film prepared in Example 10 (the NaGaS2:Eu in the composite film is anhydrous) and the comparative sample BGO were exposed to different X-ray doses (from 0.686 to 42.293 mGy air / s) radiation stimulation RL spectrum is as follows Figure 3 As shown in the figure, it can be seen that the removal of water molecules in the material structure improves the material's response sensitivity to X-rays, and the sensitivity of the hydrated phase and the anhydrous phase are both higher than that of BGO.

[0067] The newly prepared NaGaS2:Eu single crystal in Example 1 of the present application was stored in a 40% humidity environment for 600s (i.e., a NaGaS2:Eu hydrate phase was formed), and the NaGaS2:Eu composite film prepared in Example 10 (the NaGaS2:Eu in the composite film was anhydrous) was compared with the NaGaS2:Eu composite film prepared in Example 10 at (2.81×10 -5to 4.34×10 -3 mxD air / s) radiation stimulation detection limit is as follows Figure 4 As shown in the figure, the removal of water molecules in the material structure also significantly improved the detection limit performance (from 356nGy air / s to 250nGy air / s).

[0068] Application Test Example 2 Humidity Response Capability Test

[0069] Six 1 g NaGaS2:Eu single crystal samples prepared in Example 1 were accurately weighed, and each was fully ground and heated at 100°C for 180 min to remove bound water to obtain an initial state crystal;

[0070] Then, the six initial state crystals were placed in a 40% humidity environment for 600 seconds to obtain the crystals in the test state, and then X-ray excitation spectroscopy (XEL) was performed on them at different temperatures;

[0071] The results are shown in Table 1. After the NaGaS2:Eu with bound water removed is kept in a 40% humidity environment for a certain period of time, the intensity of its X-ray excitation spectrum (XEL) has a trend of first rising and then falling in the range of 300K to 450K. The increase in intensity is the process of bound water (structural water) removal, and the decrease in intensity is the process of thermal quenching caused by temperature, indicating that NaGaS2:Eu has good humidity-temperature response characteristics, which makes it possible to establish a database and perform model training through a large number of parameters such as the humidity of the environment to be tested, the holding time in the environment to be tested, and the X-ray excitation spectrum test temperature as variables, and use the X-ray excitation spectrum (XEL) intensity and variable temperature spectrum as results, so as to give the value of the environmental humidity through the X-ray excitation spectrum (XEL) detection data of NaGaS2:Eu.

[0072] The humidity testing process includes: heating the NaGaS2:Eu scintillation crystal prepared in the present application for a set time and temperature to remove bound water and obtain an initial state crystal as a humidity sensing test material; then placing the initial state crystal in an environment with a humidity to be detected for a set time, and after obtaining the test state crystal, performing an X-ray excitation spectrum detection on it at a set temperature, and then comparing it with a database to obtain a humidity value (the comparison method can be a table lookup method or obtained by fitting a model, and the fitting model can be obtained by model training based on the above database using an algorithm of the prior art).

[0073] Furthermore, the humidity test process uses multiple NaGaS2:Eu scintillation crystals prepared in the present application, and heats them for a set time and temperature to remove bound water, thereby obtaining multiple initial state crystals as humidity sensing test materials; then the multiple initial state crystals are placed in an environment with a humidity to be detected and maintained for a set time. After obtaining multiple crystals in the state to be tested, X-ray excitation spectrum detection is performed on the multiple crystals in the state to be tested at different set temperatures to obtain XEL intensity results at different temperatures, and then the humidity value is obtained by comparing the spectrum formed by temperature-XEL intensity in the database (the comparison method can be a table lookup method or obtained by fitting a model, and the fitting model can be obtained by model training based on the above-mentioned database using an algorithm of the prior art).

[0074] Table 1 Results of XEL intensity at different temperatures

[0075] temperature XEL Strength 300K <![CDATA[2.08×10 7 ]]> 330K <![CDATA[2.38×10 7 ]]> 360K <![CDATA[5.02×10 7 ]]> 390K <![CDATA[3.11×10 7 <!-- 5 -->]]> 420K <![CDATA[1.79×10 7 ]]> 450K <![CDATA[8.51×10 6 ]]>

[0076] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. Application of a rare earth element-doped gallium-based chalcogenide scintillation crystal in humidity measurement, characterized in that: The chemical formula of the rare earth element-doped gallium-based chalcogenide scintillating crystal is: Is 1-x GaS2:xEu; Here, x is 1% to 9%.

2. The use according to claim 1, characterized in that: The humidity measurement process includes: The gallium-based chalcogenide scintillating crystal doped with a rare earth element is heated at 80 to 100° C. for 60 to 180 minutes to obtain an initial state crystal; Then the initial state crystal is placed in an environment with the humidity to be tested for 300 to 600 seconds. After the crystal in the test state is obtained, an X-ray excitation spectrum test is performed on it and the humidity value is obtained by comparing it with the database.

3. The use according to claim 2, characterized in that: The database is a data set of X-ray excitation spectra of the initial state crystals at different temperatures after being kept in different humidity environments for different periods of time.

4. The use according to claim 1, characterized in that: The X-ray response of the rare earth element-doped gallium-based chalcogenide scintillation crystal is 2 to 3 times that of the BGO material.

5. The use according to claim 1, characterized in that: The light output of the rare earth element-doped gallium-based chalcogenide scintillation crystal is greater than or equal to 8000 ph / MeV.

6. The use according to claim 1, characterized in that: The method for preparing the rare earth element-doped gallium-based chalcogenide scintillation crystal comprises the following steps: S1. Grind and mix the raw materials containing Na2S, Ga2S3 and EuS with I2 in an inactive atmosphere to obtain a mixture; S2, placing the mixture in a vacuum sealed container and heating it in a temperature gradient zone to maintain a constant temperature, cooling it after the crystal grows, to obtain the rare earth element-doped gallium-based chalcogenide scintillation crystal; The temperature gradient zone includes a high temperature zone and a low temperature zone connected to each other; The mixture is located in a high temperature zone; The rare earth element-doped gallium-based chalcogenide scintillation crystal is located in a low temperature region.

7. The use according to claim 6, characterized in that: In step S1, Na2S, Ga2S3 and EuS in the raw materials are weighed according to the chemical formula composition and stoichiometric ratio of the rare earth element-doped gallium-based chalcogenide scintillating crystal; The amount of I2 used is 0.1 to 1 wt% of the raw material weight.

8. The use according to claim 6, characterized in that: In step S2, the conditions for heating and maintaining a constant temperature include: The preset temperature of the high temperature zone is 1000-1100°C; The preset temperature of the low temperature zone is 750~850℃; The high temperature zone and the low temperature zone are independently kept at a constant temperature for 90 to 120 hours.

9. The use according to claim 6, characterized in that: In step S2, the heating and constant temperature conditions also include: heating the high temperature zone and the low temperature zone at a heating rate of 3-5°C / h.

10. The use according to claim 6, characterized in that: In step S2, the heating and constant temperature conditions also include: when heating the high temperature zone and the low temperature zone, they are kept warm at 300°C, 500°C and 700°C for 180 to 300 minutes respectively.

Citation Information

Patent Citations

  • Large-bulk high-quality scintillation crystal and preparation method and application thereof

    CN113512757A

  • Alkaline-earth metal gallium sulfenyl scintillation crystal as well as preparation method and application thereof

    CN115652434A