Laminate, polarizing plate and image display device
By using a combination of optically anisotropic layers X and Y with specific ratios and thicknesses in a liquid crystal display device, the polarizing plate was optimized, solving the problems of light leakage and color shift in the tilt direction in IPS-type liquid crystal displays, and achieving thin-film processing and thermal deformation suppression.
Patent Information
- Application Number
- CN202410353387.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-02-26
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-01
AI Technical Summary
In the prior art, IPS liquid crystal display devices suffer from light leakage and color shift when viewed in the tilt direction. Furthermore, with the increasing demands for lightweight image display devices and more demanding environmental requirements, the thinning of the phase retardation film and the suppression of thermal deformation have become challenges.
A stack of two optically anisotropic layers is used to optimize the in-plane and thickness direction phase difference by combining optically anisotropic layers X and Y in a specific ratio and thickness range, thereby forming a polarizing plate to reduce light leakage and color shift.
The thin-film laminate and polarizing plate effectively suppress light leakage and color shift in the tilt direction of the liquid crystal display device, and reduce thermal deformation.
Smart Images

Figure CN118732341A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a laminate including two types of optically anisotropic layers, a polarizing plate including the laminate, and an image display device. Background Art
[0002] Generally, in the case of an in-plane switching (IPS) liquid crystal display device, it is known that when visually recognized from an oblique direction at an angle of 45 degrees relative to the absorption axis of the polarizer, the black display has a large light leakage, which is prone to a decrease in contrast and color shift. This phenomenon is caused by the fact that the angle formed by the absorption axes of the polarizers arranged on the front and back sides of the liquid crystal unit does not apparently reach 90 degrees.
[0003] In order to reduce light leakage when visually recognized from the above-mentioned oblique direction, a method of configuring a phase difference film between a liquid crystal unit and a polarizer has been proposed. For example, Patent Document 1 describes a method of reducing light leakage in an IPS-type liquid crystal display device by configuring a stretched phase difference film with a refractive index anisotropy of nx>ny>nz and a stretched phase difference film with a refractive index anisotropy of nz>nx>ny.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2009-139747 Summary of the invention
[0007] Problems to be solved by the invention
[0008] The polarizing plate obtained by laminating a polarizer and a phase difference film as described in Patent Document 1 is preferably used to reduce light leakage of an IPS-type liquid crystal display device, but in the case of a liquid crystal display device having such a structure, when the screen is visually recognized from an oblique direction, there is a case where display unevenness is confirmed. In addition, with the lightening of image display devices and the harshening of the use environment, it is required to make these phase difference films thinner and further suppress deformation caused by heat.
[0009] The present invention aims to provide a new solution to the above problems, namely, a laminated body combining two optically anisotropic layers. In addition, the present invention aims to provide a laminated body that is thinner and less deformed by heat, a polarizing plate including the laminated body, and an image display device having the same.
[0010] Means for solving problems
[0011] The inventors of the present application have conducted intensive studies to solve the above-mentioned problems and have completed the present invention. That is, the present invention includes the following aspects.
[0012] [1] A laminate comprising an optically anisotropic layer X satisfying the following formula (1) and an optically anisotropic layer Y satisfying the following formula (2),
[0013] The laminate satisfies the following formula (3).
[0014] 0.960≤A≤1.040 (1)
[0015] 0.960≤B≤1.040 (2)
[0016] -0.070≤AB≤0.070 (3)
[0017] [In formulas (1) to (3), A represents the ratio (Re(450) / Re(550)) of the in-plane retardation value of the optical anisotropic layer X at a wavelength of 450 nm to the in-plane retardation value (Re(550)) at a wavelength of 550 nm, and B represents the ratio (Rth(450) / Rth(550)) of the retardation value in the thickness direction at a wavelength of 450 nm to the retardation value in the thickness direction (Rth(550)) of the optical anisotropic layer Y at a wavelength of 550 nm.]
[0018] [2] The laminate according to [1] above, wherein the optically anisotropic layer X has a thickness of 0.5 μm to 5 μm.
[0019] [3] The laminate according to [1] above, wherein the optically anisotropic layer Y has a thickness of 0.3 μm to 5 μm.
[0020] [4] A polarizing plate comprising, in order, a polarizing film, the optically anisotropic layer X described in [1] above, and the optically anisotropic layer Y described in [1] above.
[0021] [5] A polarizing plate comprising, in order, a polarizing film, the optically anisotropic layer Y described in [1] above, and the optically anisotropic layer X described in [1] above.
[0022] [6] The polarizing plate according to [4] above, wherein the angle formed by the absorption axis of the polarizing film and the slow axis of the optically anisotropic layer X is 90±5°.
[0023] [7] The polarizing plate according to [5] above, wherein the angle formed by the absorption axis of the polarizing film and the slow axis of the optically anisotropic layer X is 0±5°.
[0024] [8] An image display device comprising the polarizing plate according to any one of [4] to [7] above.
[0025] Effects of the Invention
[0026] According to the present invention, it is possible to provide a laminated body that is thinner and less deformed by heat, a polarizing plate including the laminated body, and an image display device including the laminated body. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] [ Figure 1 ] is a schematic cross-sectional view showing an example of the layer structure of the laminate of the present invention.
[0028] [ Figure 2 ] is a schematic cross-sectional view showing an example of the layer structure of the polarizing plate of the present invention.
[0029] [ Figure 3 ] is a schematic cross-sectional view showing an example of the layer structure of the polarizing plate of the present invention.
[0030] Description of Reference Numerals
[0031] 1: Optically anisotropic layer X
[0032] 2: Optically anisotropic layer Y
[0033] 3: Polarizing film
[0034] 10: Laminated body
[0035] 20: Polarizing plate
[0036] 21: Polarizing plate DETAILED DESCRIPTION
[0037] The laminate of the present invention comprises an optically anisotropic layer X (hereinafter, also referred to as "optically anisotropic layer X") satisfying the following formula (1) and an optically anisotropic layer Y (hereinafter, also referred to as "optically anisotropic layer Y") satisfying the following formula (2), and the laminate satisfies the following formula (3). Figure 1 An example of the layer structure of the laminate of the present invention is described. Figure 2 and Figure 3 An example of the layer structure of the polarizing plate of the present invention will be described, but the present invention is not limited to these aspects.
[0038] Figure 1 The laminate 10 shown comprises an optically anisotropic layer X ( Figure 1 Layer 1) and optically anisotropic layer Y ( Figure 1 Layer 2 in Figure 1 In the laminated body 10 shown, the optically anisotropic layer X satisfies the following formula (1), the optically anisotropic layer Y satisfies the following formula (2), and the laminated body 10 satisfies the following formula (3).
[0039] 0.960≤A≤1.040 (1)
[0040] 0.960≤B≤1.040 (2)
[0041] -0.070≤AB≤0.070 (3)
[0042] [In formulas (1) to (3), A represents the ratio (Re(450) / Re(550)) of the in-plane retardation value of the optical anisotropic layer X at a wavelength of 450 nm to the in-plane retardation value (Re(550)) at a wavelength of 550 nm, and B represents the ratio (Rth(450) / Rth(550)) of the retardation value in the thickness direction at a wavelength of 450 nm to the retardation value in the thickness direction (Rth(550)) of the optical anisotropic layer Y at a wavelength of 550 nm.]
[0043] In the present invention, the in-plane retardation value (Re(λ)) of the optical anisotropic layer X at a wavelength λnm is obtained by the formula: Re(λ) = (nx(λ) - ny(λ)) × d1. In the above formula, nx(λ) represents the principal refractive index at a wavelength λnm in the plane of the optical anisotropic layer X, ny(λ) represents the refractive index at a wavelength λnm in the same plane as nx and in a direction orthogonal to the direction of nx, and d1 represents the thickness of the optical anisotropic layer X.
[0044] When the optical anisotropic layer X satisfies formula (1), the optical anisotropic layer X shows that the in-plane phase difference value at a short wavelength is substantially equal to the in-plane phase difference value at a long wavelength. By combining such an optical anisotropic layer X with an optical anisotropic layer Y described later, when incorporated into a liquid crystal display device, a laminate having an excellent effect of preventing light leakage and color shift when visually recognized from an oblique direction during black display can be obtained. In addition, in formula (1), the value of A is preferably 0.970 or more, more preferably 0.975 or more, and preferably 1.030 or less, more preferably 1.025 or less. If the value of A is within the above range, a laminate having a more excellent effect of preventing light leakage and color shift when visually recognized from an oblique direction to a liquid crystal display device during black display can be obtained.
[0045] The above-mentioned in-plane phase difference value can be adjusted by the thickness (d1) of the optical anisotropic layer X. Since the in-plane phase difference value is determined by "Formula: Re (λ) = (nx (λ) - ny (λ)) × d1", in order to obtain the desired in-plane phase difference value, the three-dimensional refractive index and the film thickness (d1) can be adjusted. It should be noted that the three-dimensional refractive index depends on the molecular structure and orientation state of the compound constituting the optical anisotropic layer X.
[0046] In addition, the optically anisotropic layer X preferably satisfies the following formula (4).
[0047] 100nm≤Re(550)≤160nm (4)
[0048] [In formula (4), Re(λ) has the same meaning as above.]
[0049] If the in-plane retardation value (Re(550)) of the optically anisotropic layer X is within the range of formula (4), when a laminate including the optically anisotropic layer X and a polarizing plate including the laminate are applied to a liquid crystal display device, the effect of preventing light leakage and color shift when visually recognized from an oblique direction during black display becomes significant. A further preferred range of the in-plane retardation value (Re(550)) is 110 nm ≤ Re(550) ≤ 150 nm.
[0050] In the present invention, the phase difference value (Rth(λ)) in the thickness direction at a wavelength λnm of the optically anisotropic layer Y is obtained by the formula: Rth(λ)=((nx(λ)+ny(λ)) / 2-nz(λ))×d2. In the above formula, nx(λ) represents the in-plane principal refractive index of the optically anisotropic layer Y at a wavelength λnm, ny(λ) represents the refractive index in the direction orthogonal to nx(λ) in the plane at a wavelength λnm, nz(λ) represents the refractive index in the thickness direction of the optically anisotropic layer Y at a wavelength λnm, and when nx(λ)=ny(λ), nx(λ) can be set to the refractive index in any direction in the plane of the optically anisotropic layer Y, and d2 represents the thickness of the optically anisotropic layer Y.
[0051] When the optical anisotropic layer Y satisfies formula (2), the optical anisotropic layer Y shows a characteristic that the phase difference value in the thickness direction at the short wavelength is substantially the same as the phase difference value in the thickness direction at the long wavelength. By combining such an optical anisotropic layer Y with the above-mentioned optical anisotropic layer X, when a liquid crystal display device is incorporated, a laminate having an excellent effect of preventing light leakage and color shift when visually recognized from an oblique direction during black display can be obtained. In addition, in formula (2), the value of B is preferably 0.970 or more, more preferably 0.975 or more, and preferably 1.030 or less, more preferably 1.025 or less. If the value of B is within the above range, a laminate having a more excellent effect of preventing light leakage and color shift when visually recognized from an oblique direction to a liquid crystal display device during black display can be obtained.
[0052] The above-mentioned phase difference value in the thickness direction can be adjusted by the thickness (d2) of the optical anisotropic layer Y. Since the phase difference value in the thickness direction is determined by "Formula: Rth(λ)=((nx(λ)+ny(λ)) / 2-nz(λ))×d2", in order to obtain the desired phase difference value in the thickness direction (Rth(λ)), it is sufficient to adjust the three-dimensional refractive index and the film thickness (d2). It should be noted that the three-dimensional refractive index depends on the molecular structure and orientation state of the compound constituting the optical anisotropic layer Y.
[0053] Furthermore, as an index representing the degree of the effect of preventing light leakage and color shift when viewed from an oblique direction during black display, the optically anisotropic layer Y preferably satisfies the following formula (5).
[0054] -120nm≤Rth(550)≤60nm (5)
[0055] [In formula (5), Rth(550) has the same meaning as above.]
[0056] From the viewpoint of being able to further suppress light leakage and color shift when visually recognized from an oblique direction during black display, the phase difference value (Rth(550)) in the thickness direction of the optical anisotropic layer Y is more preferably greater than -115 nm, further preferably greater than -110 nm, and more preferably less than 55 nm, further preferably less than 50 nm.
[0057] In the present invention, the laminate including the optically anisotropic layer X satisfying the above formula (1) and the optically anisotropic layer Y satisfying the above formula (2) further satisfies the following formula (3).
[0058] -0.070≤AB≤0.070 (3)
[0059] [In formula (3), A and B have the same meanings as A and B in the above formula (1) and formula (2).]
[0060] When the laminate satisfies formula (3), it indicates that the value of A of the optically anisotropic layer X and the value of B of the optically anisotropic layer Y contained in the laminate are both close values. Generally, it is known that the value of A of the optically anisotropic layer X and the value of B of the optically anisotropic layer Y are less than 1, and the smaller the value and the closer to 0.82, the more the reverse wavelength dispersion characteristics are shown. As a result of the research by the inventors of the present application, it is found that it is not necessary to show the reverse wavelength dispersion characteristics that the value of A of the optically anisotropic layer X and the value of B of the optically anisotropic layer Y must be close to 0.82. By satisfying the above formula (3), the effect of preventing light leakage and color shift when visually recognized from an oblique direction when black display is displayed when incorporated in a liquid crystal display device can be obtained.
[0061] In the above formula (3), from the viewpoint of preventing light leakage and color shift when visually recognized from an oblique direction when black display is performed when the laminated body of the present invention is incorporated into a liquid crystal display device, the value of AB is preferably -0.064 or more, more preferably -0.060 or more, and particularly preferably -0.050 or more, and preferably 0.064 or less, more preferably 0.060 or less, and particularly preferably 0.050 or less. If the value of AB is within the above range, a laminated body having a more excellent effect of preventing light leakage and color shift when visually recognized from an oblique direction when a liquid crystal display device is displayed in black can be obtained.
[0062] Hereinafter, each structure of the laminated body of the present invention will be described in detail.
[0063] [Optically anisotropic layer X]
[0064] Examples of the optically anisotropic layer X constituting the laminate of the present invention include a stretched film or a cured layer of a polymerizable liquid crystal composition obtained by curing a polymerizable liquid crystal compound in a state of being oriented in a horizontal direction with respect to a film plane.
[0065] As stretched films, for example, uniaxially stretched polycarbonate (PC) films, uniaxially stretched triacetyl cellulose (TAC) films, and uniaxially stretched cycloolefin polymer (COP) films can be cited. The in-plane phase difference value of these stretched films can be adjusted by controlling the composition of the resin constituting the stretched film, the stretching method, and the thickness of the stretched film.
[0066] As a polymerizable liquid crystal compound, the cured layer of the polymerizable liquid crystal composition obtained by curing in a state of being oriented in a horizontal direction relative to the film plane can be formed using a nematic liquid crystal or a discotic liquid crystal. The in-plane phase difference value of the cured layer of the polymerizable liquid crystal composition can be adjusted by controlling the type of the polymerizable liquid crystal compound, the orientation state of the cured product of the polymerizable liquid crystal compound, and the thickness of the cured layer.
[0067] The thickness of the optically anisotropic layer X is preferably 0.5 μm to 5 μm, more preferably 0.6 μm to 4.5 μm, and further preferably 0.7 μm to 4 μm. The thinner the thickness, the more preferred, so as described below, the optically anisotropic layer X is preferably a polymerizable liquid crystal compound solidified in a state oriented in a horizontal direction relative to the film plane and obtained by curing the polymerizable liquid crystal composition (hereinafter also referred to as "horizontally oriented liquid crystal cured film"), and more preferably a polymerizable liquid crystal compound having at least one free radical polymerizable group is solidified in a state horizontally oriented relative to the in-plane direction of the cured film. Liquid crystal cured film. By setting the thickness of the optically anisotropic layer X to a horizontally oriented liquid crystal cured film that satisfies the above range, it is possible to achieve lightweight image display devices, and a laminate with small deformation caused by heat as described later can be obtained.
[0068] In the present invention, the polymerizable liquid crystal compound contained in the polymerizable liquid crystal composition forming the horizontally aligned liquid crystal cured film refers to a liquid crystal compound having a polymerizable group, and particularly preferably a polymerizable liquid crystal compound having at least one radical polymerizable group.
[0069] The polymerizable group refers to a group that can participate in the polymerization reaction through an active free radical, acid, etc. generated by a polymerization initiator. As the polymerizable group, for example, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxacyclopropyl, and oxetanyl can be cited. Among them, free radical polymerizable groups are preferred, acryloyloxy, methacryloyloxy, vinyl, and vinyloxy are more preferred, and acryloyloxy and methacryloyloxy are further preferred.
[0070] The liquid crystal property exhibited by the polymerizable liquid crystal compound may be a thermotropic liquid crystal or a lyotropic liquid crystal. From the viewpoint of enabling precise film thickness control, a thermotropic liquid crystal is preferred.
[0071] As the polymerizable liquid crystal compound, there can be mentioned a polymerizable liquid crystal compound that generally exhibits positive wavelength dispersion and a polymerizable liquid crystal compound that exhibits reverse wavelength dispersion. Only one polymerizable liquid crystal compound can be used, or two polymerizable liquid crystal compounds can be mixed and used. From the perspective of preventing light leakage and color shift when visually recognized from an oblique direction during black display, it is preferred that the composition is adjusted in such a manner that the optically anisotropic layer X satisfies the above formula (1).
[0072] As the polymerizable liquid crystal compound showing reverse wavelength dispersion, a compound having the following characteristics (A) to (D) is preferred.
[0073] (A) is a compound that can form a nematic phase or a smectic phase.
[0074] (B) The polymerizable liquid crystal compound has π electrons in the long-axis direction (a).
[0075] (C) It has π electrons in a direction intersecting the long axis direction (a) (intersecting direction (b)).
[0076] (D) The π electron density in the long axis direction (a) of the polymerizable liquid crystal compound is defined by the following formula (i), where the total number of π electrons present in the long axis direction (a) is N(πa) and the total molecular weight present in the long axis direction is N(Aa):
[0077] D(πa)=N(πa) / N(Aa)(i), and,
[0078] The total number of π electrons present in the cross direction (b) is denoted as N(πb), and the total number of molecular weights present in the cross direction (b) is denoted as N(Ab), and the π electron density in the cross direction (b) of the polymerizable liquid crystal compound is defined by the following formula (ii):
[0079] D(πb)=N(πb) / N(Ab) (ii)
[0080] The relationship of existence (iii) is:
[0081] 0≤〔D(πa) / D(πb)〕<1 (iii)
[0082] [That is, the π electron density in the cross direction (b) is greater than the π electron density in the long axis direction (a)].
[0083] In addition, as described above, the polymerizable liquid crystal compound having π electrons in the long axis and in the direction intersecting therewith forms, for example, a T-shaped structure.
[0084] In the above-mentioned features (A) to (D), the major axis direction (a) and the number of π electrons N are defined as follows.
[0085] The major axis direction (a) refers to the major axis direction of the rod, for example, in the case of a compound having a rod-like structure.
[0086] The number of π electrons N(πa) present in the major axis direction (a) does not include π electrons that disappear due to the polymerization reaction.
[0087] The number of π electrons N(πa) present in the long axis direction (a) is the total number of π electrons on the long axis and π electrons conjugated thereto, for example, including the number of π electrons present in the ring that exists in the long axis direction (a) and satisfies the Huckel rule.
[0088] The number of π electrons N(πb) present in the crossing direction (b) does not include π electrons that disappear due to the polymerization reaction.
[0089] The polymerizable liquid crystal compound satisfying the above conditions has a mesostructure in the long-axis direction, and exhibits a liquid crystal phase (nematic phase, smectic phase) due to the mesostructure.
[0090] By applying a polymerizable liquid crystal compound satisfying the above (A) to (D) on a film (layer) forming a liquid crystal cured film and heating it to a temperature above the phase transition temperature, a liquid crystal phase such as a nematic phase or a smectic phase can be formed. The liquid crystal phase formed by the orientation of the polymerizable liquid crystal compound is usually oriented in a manner that the long axis directions of the polymerizable liquid crystal compound are parallel to each other, and the long axis direction becomes the orientation direction of the liquid crystal phase. If such a polymerizable liquid crystal compound is made into a film and polymerized in a liquid crystal phase, a polymer film formed by polymerizing in a state of orientation along the long axis direction (a) can be formed. The polymer film absorbs ultraviolet rays by π electrons in the long axis direction (a) and π electrons in the cross direction (b). Here, the absorption maximum wavelength of ultraviolet rays absorbed by the π electrons in the cross direction (b) is recorded as λbmax. λbmax is usually 300nm to 400nm. The density of π electrons satisfies the above formula (iii), and the density of π electrons in the cross direction (b) is greater than that in the long axis direction (a), so that the absorption of linearly polarized ultraviolet light (wavelength λbmax) having a vibration plane in the cross direction (b) is greater than that of linearly polarized ultraviolet light (wavelength λbmax) having a vibration plane in the long axis direction (a). The ratio (absorbance in the cross direction (b) of linearly polarized ultraviolet light / absorbance in the long axis direction (a)) is, for example, greater than 1.0, preferably greater than 1.2, and usually 30 or less, for example, 10 or less.
[0091] The polymerizable liquid crystal compound having the above-mentioned characteristics usually shows reverse wavelength dispersion. Specifically, for example, there can be mentioned a compound represented by the following formula (X) (hereinafter also referred to as a “polymerizable liquid crystal compound (X)”).
[0092] [Chemical formula 1]
[0093]
[0094] In formula (X), Ar represents a divalent group containing an aromatic group which may have a substituent. The aromatic group mentioned here refers to a group having a π electron number of [4n+2] in the ring structure according to the Huckel rule, for example, an Ar group such as (Ar-1) to (Ar-23) described later may have two or more Ar groups exemplified by divalent linking groups. Here, n represents an integer. In the case where a ring structure is formed by containing heteroatoms such as -N= and -S-, the case where the non-covalent bond electron pairs on these heteroatoms satisfy the Huckel rule and thus have aromaticity is also included. It is preferred that at least one of a nitrogen atom, an oxygen atom, and a sulfur atom is contained in the aromatic group. The aromatic group contained in the divalent group Ar may be one or more. In the case where the aromatic group is one, the divalent group Ar may be a divalent aromatic group which may have a substituent. When the divalent group Ar contains two or more aromatic groups, the two or more aromatic groups may be bonded to each other via a single bond, a divalent bonding group such as -CO-O-, or -O-.
[0095] G 1 and G 2 Each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group. Here, the hydrogen atoms contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted by a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group or a nitro group, and the carbon atoms constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted by an oxygen atom, a sulfur atom or a nitrogen atom.
[0096] L 1 , L 2 , B 1 and B 2 Each is independently a single bond or a divalent linking group.
[0097] k and l each independently represent an integer from 0 to 3, and satisfy the relationship 1≤k+1. Here, when 2≤k+1, B 1 and B 2 , G 1 and G 2 Each may be the same as or different from each other.
[0098] E 1 and E 2 Each independently represents an alkanediyl group having 1 to 17 carbon atoms, and more preferably an alkanediyl group having 4 to 12 carbon atoms. In addition, the hydrogen atoms contained in the alkanediyl group may be substituted with halogen atoms, and -CH2- contained in the alkanediyl group may be replaced with -O-, -S-, -SiH2-, or -C(=O)-.
[0099] P1 and P 2 Each independently represents a polymerizable group or a hydrogen atom, and at least one of them is a polymerizable group.
[0100] G 1 and G 2 Each independently preferably is a 1,4-phenylenediyl group which may be substituted with at least one substituent selected from the group consisting of a halogen atom and an alkyl group having 1 to 4 carbon atoms, or a 1,4-cyclohexanediyl group which may be substituted with at least one substituent selected from the group consisting of a halogen atom and an alkyl group having 1 to 4 carbon atoms. More preferably, it is a 1,4-phenylenediyl group substituted with a methyl group, an unsubstituted 1,4-phenylenediyl group, or an unsubstituted 1,4-trans-cyclohexanediyl group. Especially preferably, it is an unsubstituted 1,4-phenylenediyl group or an unsubstituted 1,4-trans-cyclohexanediyl group.
[0101] In addition, it is preferred that there are multiple G 1 and G 2 At least one of them is a divalent alicyclic hydrocarbon group, and more preferably 1 or L 2 Bonded G 1 and G 2 At least one of them is a divalent alicyclic hydrocarbon group.
[0102] L 1 and L 2 Each of them is independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a1 OR a2 -、-R a3 COOR a4 -、-R a5 OCOR a6 -、R a7 OC=OOR a8 -、-N=N-、-CR c =CR d -, or -C≡C-. Here, R a1 ~R a8 Each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms, and R c and R d represents an alkyl group having 1 to 4 carbon atoms or a hydrogen atom. 1 and L 2 Each independently is more preferably a single bond, -OR a2-1 -、-CH2-、-CH2CH2-、-COOR a4-1 -, or -OCOR a6-1 -. Here, R a2-1 , R a4-1 , Ra6-1 Each independently represents a single bond, -CH2-, or -CH2CH2-. 1 and L 2 Each independently is further preferably a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, or -OCO-.
[0103] B 1 and B 2 Each of them is independently preferably a single bond, an alkylene group having 1 to 4 carbon atoms, -O-, -S-, -R a9 OR a10 -、-R a11 COOR a12 -、-R a13 OCOR a14 -, or R a15 OC=OOR a16 -. Here, R a9 ~R a16 Each independently represents a single bond or an alkylene group having 1 to 4 carbon atoms. 1 and B 2 Each independently is more preferably a single bond, -OR a10-1 -、-CH2-、-CH2CH2-、-COOR a12 -1 -, or -OCOR a14-1 -. Here, R a10-1 , R a12-1 , R a14-1 Each independently represents a single bond, -CH2-, or -CH2CH2-. 1 and B 2 Each independently is further preferably a single bond, -O-, -CH2CH2-, -COO-, -COOCH2CH2-, -OCO-, or -OCOCH2CH2-.
[0104] From the viewpoint of exhibiting reverse wavelength dispersion, k and l are preferably in the range of 2≤k+l≤6, k+l=4 is preferred, and k=2 and l=2 are more preferred. k=2 and l=2 are preferred because a symmetrical structure is obtained.
[0105] As P 1 or P 2 The polymerizable group represented by , includes epoxy, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxirane, etc. Among them, acryloyloxy, methacryloyloxy, vinyl and vinyloxy are preferred, and acryloyloxy and methacryloyloxy are more preferred.
[0106] Ar preferably has at least one selected from an aromatic hydrocarbon ring that may have a substituent, an aromatic heterocycle that may have a substituent, and an electron-withdrawing group. As the aromatic hydrocarbon ring, for example, benzene ring, naphthalene ring, anthracene ring, etc. can be cited, preferably benzene ring, naphthalene ring. As the aromatic heterocycle, furan ring, benzofuran ring, pyrrole ring, indole ring, thiophene ring, benzothiophene ring, pyridine ring, pyrazine ring, pyrimidine ring, triazole ring, triazine ring, pyrroline ring, imidazole ring, pyrazole ring, thiazole ring, benzothiazole ring, thienothiazole ring, oxazole ring, benzoxazole ring, and phenanthroline ring, etc. can be cited. Among them, preferably have thiazole ring, benzothiazole ring or benzofuran ring, further preferably have benzothiazolyl. In addition, when Ar contains a nitrogen atom, the nitrogen atom preferably has π electrons.
[0107] In formula (X), the total number of π electrons contained in the divalent aromatic group represented by Ar is N π It is preferably 8 or more, more preferably 10 or more, further preferably 14 or more, and particularly preferably 16 or more. It is preferably 30 or less, more preferably 26 or less, and further preferably 24 or less.
[0108] Examples of the aromatic group represented by Ar include the following groups.
[0109] [Chemical formula 2]
[0110]
[0111] In the formulas (Ar-1) to (Ar-23), the symbol * represents a connecting portion, and Z 0 , Z 1 and Z 2 Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, an alkylsulfinyl group having 1 to 12 carbon atoms, an alkylsulfonyl group having 1 to 12 carbon atoms, a carboxyl group, a fluoroalkyl group having 1 to 12 carbon atoms, an alkoxy group having 1 to 12 carbon atoms, an alkylthio group having 1 to 12 carbon atoms, an N-alkylamino group having 1 to 12 carbon atoms, an N,N-dialkylamino group having 2 to 12 carbon atoms, an N-alkylsulfamoyl group having 1 to 12 carbon atoms, or an N,N-dialkylsulfamoyl group having 2 to 12 carbon atoms. 0 , Z 1 and Z 2 A polymerizable group may be contained.
[0112] Q 1 and Q 2 Each independently represents -CR 2’ R 3’ -、-S-、-NH-、-NR 2’ -, -CO- or -O-, R 2’and R 3’ Each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0113] J 1 , and J 2 Each independently represents a carbon atom or a nitrogen atom.
[0114] Y 1 , Y 2 and Y 3 Each independently represents an aromatic hydrocarbon group or an aromatic heterocyclic group which may be substituted.
[0115] W 1 and W 2 Each independently represents a hydrogen atom, a cyano group, a methyl group or a halogen atom, and m represents an integer of 0-6.
[0116] As Y 1 , Y 2 and Y 3 The aromatic hydrocarbon group in the group includes aromatic hydrocarbon groups having 6 to 20 carbon atoms, such as phenyl, naphthyl, anthracenyl, phenanthrenyl, and biphenyl, preferably phenyl and naphthyl, and more preferably phenyl. The aromatic heterocyclic group includes aromatic heterocyclic groups having 4 to 20 carbon atoms, such as furanyl, pyrrolyl, thienyl, pyridyl, thiazolyl, and benzothiazolyl, which contain at least one hetero atom such as a nitrogen atom, an oxygen atom, or a sulfur atom, preferably furanyl, thienyl, pyridyl, thiazolyl, and benzothiazolyl.
[0117] Y 1 , Y 2 and Y 3 Each independently may be a substituted polycyclic aromatic hydrocarbon group or a polycyclic aromatic heterocyclic group. The polycyclic aromatic hydrocarbon group refers to a condensed polycyclic aromatic hydrocarbon group or a group derived from an aromatic ring collection. The polycyclic aromatic heterocyclic group refers to a condensed polycyclic aromatic heterocyclic group or a group derived from an aromatic ring collection.
[0118] Z 0 , Z 1 and Z 2 Each of Z is independently preferably a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, a cyano group, a nitro group, or an alkoxy group having 1 to 12 carbon atoms. 0 More preferably, a hydrogen atom, an alkyl group having 1 to 12 carbon atoms, or a cyano group. 1 and Z 2 More preferably, Z is a hydrogen atom, a fluorine atom, a chlorine atom, a methyl group, or a cyano group. 0 , Z 1 and Z 2 A polymerizable group may be contained.
[0119] Q 1 and Q2 Preferred are -NH-, -S-, -NR 2’ -、-O-,R 2’ A hydrogen atom is preferred, and -S-, -O-, and -NH- are particularly preferred.
[0120] Among formulae (Ar-1) to (Ar-23), formulae (Ar-6) and (Ar-7) are preferred from the viewpoint of molecular stability.
[0121] In the formulas (Ar-16) to (Ar-23), Y 1 The nitrogen atom and Z that can be bonded to it 0 Together, they form an aromatic heterocyclic group. Examples of the aromatic heterocyclic group include the aromatic heterocyclic rings that Ar may have and are described above, for example, a pyrrole ring, an imidazole ring, a pyrroline ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, an indole ring, a quinoline ring, an isoquinoline ring, a purine ring, a pyrrolidine ring, etc. The aromatic heterocyclic group may have a substituent. In addition, Y 1 The nitrogen atom and Z that can be bonded to it 0 Together, they form the above-mentioned optionally substituted polycyclic aromatic hydrocarbon group or polycyclic aromatic heterocyclic group, for example, a benzofuran ring, a benzothiazole ring, a benzoxazole ring, etc.
[0122] In addition, in the present invention, as a polymerizable liquid crystal compound for forming a horizontally aligned liquid crystal cured film, for example, a compound containing a group represented by the following formula (Y) (hereinafter also referred to as "polymerizable liquid crystal compound (Y)") can be used. Polymerizable liquid crystal compounds generally tend to show positive wavelength dispersion. The polymerizable liquid crystal compound can be used alone or in combination of two or more, and the polymerizable liquid crystal compound (X) can be used in combination with the polymerizable liquid crystal compound (Y).
[0123] P11-B11-E11-B12-A11-B13-(Y)
[0124] [In formula (Y), P11 represents a polymerizable group.
[0125] A11 represents a divalent alicyclic hydrocarbon group or a divalent aromatic hydrocarbon group. The hydrogen atoms contained in the divalent alicyclic hydrocarbon group and the divalent aromatic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cyano group or a nitro group, and the hydrogen atoms contained in the alkyl group having 1 to 6 carbon atoms and the alkoxy group having 1 to 6 carbon atoms may be substituted with a fluorine atom.
[0126] B11 represents -O-, -S-, -CO-O-, -O-CO-, -O-CO-O-, -CO-NR 16 -、-NR 16-CO-, -CO-, -CS- or a single bond. 16 It represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.
[0127] B12 and B13 each independently represent -C≡C-, -CH=CH-, -CH2-CH2-, -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -OC(=O)-O-, -CH=N-, -N=CH-, -N=N-, -C(=O)-NR 16 -、-NR 16 -C(=O)-, -OCH2-, -OCF2-, -CH2O-, -CF2O-, -CH=CH-C(=O)-O-, -OC(=O)-CH=CH- or a single bond.
[0128] E11 represents an alkanediyl group having 1 to 12 carbon atoms, wherein the hydrogen atoms contained in the alkanediyl group may be substituted by an alkoxy group having 1 to 5 carbon atoms, and the hydrogen atoms contained in the alkoxy group may be substituted by a halogen atom. In addition, -CH2- constituting the alkanediyl group may be replaced by -O- or -CO-.]
[0129] The number of carbon atoms of the aromatic hydrocarbon group and alicyclic hydrocarbon group of A11 is preferably in the range of 3 to 18, more preferably in the range of 5 to 12, and particularly preferably 5 or 6. A11 is preferably cyclohexane-1,4-diyl or 1,4-phenylene.
[0130] E11 is preferably a linear alkanediyl group having 1 to 12 carbon atoms. -CH2- constituting the alkanediyl group may be replaced by -O-.
[0131] Specifically, there can be mentioned straight-chain alkanediyl groups having 1 to 12 carbon atoms, such as methylene, ethylene, propane-1,3-diyl, butane-1,4-diyl, pentane-1,5-diyl, hexane-1,6-diyl, heptane-1,7-diyl, octane-1,8-diyl, nonane-1,9-diyl, decane-1,10-diyl, undecane-1,11-diyl and dodecane-1,12-diyl; -CH2-CH2-O-CH2-CH2-, -CH2-CH2-O-CH2-CH2-O-CH2-CH2- and -CH2-CH2-O-CH2-CH2-O-CH2-CH2-O-CH2-CH2-, etc.
[0132] B11 is preferably -O-, -S-, -CO-O-, or -O-CO-, and among them, -CO-O- is more preferred.
[0133] B12 and B13 are each independently preferably -O-, -S-, -C(=O)-, -C(=O)-O-, -OC(=O)-, or -OC(=O)-O-, and among them, -O- or -OC(=O)-O- is more preferable.
[0134] As the polymerizable group represented by P11, from the perspective of high polymerization reactivity, especially photopolymerization reactivity, it is preferably a free radical polymerizable group or a cationic polymerizable group. From the perspective of easy operation and easy manufacture of the liquid crystal compound itself, the polymerizable group is preferably a group represented by the following formula (P-11) to (P-15).
[0135] [Chemical formula 3]
[0136]
[0137] [In formulas (P-11) to (P-15), R 17 ~R 21 Each independently represents an alkyl group having 1 to 6 carbon atoms or a hydrogen atom.]
[0138] Specific examples of the groups represented by formula (P-11) to formula (P-15) include groups represented by the following formula (P-16) to formula (P-20).
[0139] [Chemical formula 4]
[0140]
[0141] P11 is preferably a group represented by formula (P-14) to formula (P-20), and more preferably a vinyl group, a p-stilbene group, an epoxy group, or an oxetanyl group.
[0142] The group represented by P11-B11- is more preferably an acryloyloxy group or a methacryloyloxy group.
[0143] Examples of the polymerizable liquid crystal compound (Y) include compounds represented by formula (I), formula (II), formula (III), formula (IV), formula (V) or formula (VI).
[0144] P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-A14-B16-E12-B17-P12(I)
[0145] P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-A14-F11(II)
[0146] P11-B11-E11-B12-A11-B13-A12-B14-A13-B15-E12-B17-P12(III)
[0147] P11-B11-E11-B12-A11-B13-A12-B14-A13-F11(IV)
[0148] P11-B11-E11-B12-A11-B13-A12-B14-E12-B17-P12(V)
[0149] P11-B11-E11-B12-A11-B13-A12-F11(VI)
[0150] (Where,
[0151] A12 to A14 each independently have the same meaning as A11, B14 to B16 each independently have the same meaning as B12, B17 has the same meaning as B11, and E12 has the same meaning as E11.
[0152] F11 represents a hydrogen atom, an alkyl group having 1 to 13 carbon atoms, an alkoxy group having 1 to 13 carbon atoms, a cyano group, a nitro group, a trifluoromethyl group, a dimethylamino group, a hydroxyl group, a hydroxymethyl group, a formyl group, a sulfo group (-SO3H), a carboxyl group, an alkoxycarbonyl group having 1 to 10 carbon atoms, or a halogen atom, and the -CH2- constituting the alkyl group and the alkoxy group may be replaced by -O-.)
[0153] Specific examples of polymerizable liquid crystal compounds (Y) include compounds having polymerizable groups recorded in "3.8.6 Network (Completely Cross-linked Type)" and "6.5.1 Liquid Crystal Materials b. Polymerizable Nematic Liquid Crystal Materials" of Liquid Crystal Handbook (edited by Liquid Crystal Handbook Editorial Committee, published by Maruzen Co., Ltd. on October 30, 2013), and polymerizable liquid crystals recorded in Japanese Patent Publication No. 2010-31223, Japanese Patent Publication No. 2010-270108, Japanese Patent Publication No. 2011-6360 and Japanese Patent Publication No. 2011-207765.
[0154] As specific examples of polymerizable liquid crystal compounds (Y), compounds represented by the following formulas (I-1) to (I-4), (II-1) to (II-4), (III-1) to (III-26), (IV-1) to (IV-26), (V-1) to (V-2) and (VI-1) to (VI-6) can be cited. It should be noted that in the following formula, k1 and k2 each independently represent an integer of 2 to 12. These polymerizable liquid crystal compounds (Y) are preferred from the perspective of ease of synthesis or ease of availability.
[0155] [Chemical formula 5]
[0156]
[0157] [Chemical formula 6]
[0158]
[0159] [Chemical formula 7]
[0160]
[0161] [Chemical formula 8]
[0162]
[0163] [Chemical formula 9]
[0164]
[0165] [Chemical formula 10]
[0166]
[0167] [Chemical formula 11]
[0168]
[0169] [Chemical formula 12]
[0170]
[0171] [Chemical formula 13]
[0172]
[0173] In the present invention, the horizontally aligned liquid crystal cured film preferably has at least one maximum absorption between wavelengths of 300 and 400 nm, and the polymerizable liquid crystal composition forming the horizontally aligned liquid crystal cured film preferably contains at least one polymerizable liquid crystal compound having a maximum absorption wavelength between wavelengths of 300 and 400 nm. When a photopolymerization initiator is included in the polymerizable liquid crystal composition, the polymerization reaction and gelation of the polymerizable liquid crystal compound may proceed during long-term storage. However, if the maximum absorption wavelength of the polymerizable liquid crystal compound is 300 to 400 nm, even if it is exposed to ultraviolet light during storage, the generation of reactive species from the photopolymerization initiator and the polymerization reaction and gelation of the polymerizable liquid crystal compound caused by the reactive species can be effectively suppressed. Therefore, it is advantageous in terms of the long-term stability of the polymerizable liquid crystal composition, and the orientation and uniformity of the film thickness of the obtained liquid crystal cured film can be improved. It should be noted that the maximum absorption wavelength of the polymerizable liquid crystal compound can be measured in a solvent using an ultraviolet-visible spectrophotometer. The solvent is a solvent that can dissolve the polymerizable liquid crystal compound, and chloroform and the like can be cited as examples.
[0174] Regarding the content of the polymerizable liquid crystal compound in the polymerizable liquid crystal composition that forms the horizontally oriented liquid crystal cured film, relative to 100 parts by mass of the solid content of the polymerizable liquid crystal composition, for example, 70 to 99.5 parts by mass, preferably 80 to 99 parts by mass, more preferably 85 to 98 parts by mass, and further preferably 90 to 95 parts by mass. When the content of the polymerizable liquid crystal compound is within the above range, it is advantageous from the perspective of the orientation of the obtained liquid crystal cured film. It should be noted that in the present invention, the solid content of the polymerizable liquid crystal composition refers to all components after removing volatile components such as organic solvents from the polymerizable liquid crystal composition.
[0175] The polymerizable liquid crystal composition used in the formation of the horizontally aligned liquid crystal cured film may contain, in addition to the polymerizable liquid crystal compound, additives such as a solvent, a polymerization initiator, a leveling agent, an antioxidant, and a photosensitizer. These components may be used alone or in combination of two or more.
[0176] The polymerizable liquid crystal composition used in the formation of the horizontal alignment liquid crystal cured film is usually applied to a substrate, a horizontal alignment film, etc. in a state dissolved in a solvent, and therefore preferably contains a solvent. As the solvent, it is preferably a solvent that can dissolve the polymerizable liquid crystal compound, and it is preferably a solvent that is inactive for the polymerization reaction of the polymerizable liquid crystal compound. Examples of the solvent include alcohol solvents such as water, methanol, ethanol, ethylene glycol, isopropanol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, 1-methoxy-2-propanol, 2-butoxyethanol, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; alicyclic hydrocarbon solvents such as ethylcyclohexane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorinated solvents such as chloroform and chlorobenzene; amide solvents such as dimethylacetamide, dimethylformamide, N-methyl-2-pyrrolidone (NMP), and 1,3-dimethyl-2-imidazolidinone; and the like. These solvents may be used alone or in combination of two or more. Among them, alcohol solvents, ester solvents, ketone solvents, chlorine-containing solvents, amide solvents, and aromatic hydrocarbon solvents are preferred.
[0177] Relative to 100 parts by mass of polymerizable liquid crystal composition, the content of the solvent in the polymerizable liquid crystal composition is preferably 50 to 98 parts by mass, more preferably 70 to 95 parts by weight. Therefore, the solid component preferably accounts for 2 to 50 parts by mass in 100 parts by mass of the polymerizable liquid crystal composition. When the solid component is less than 50 parts by mass, the viscosity of the polymerizable liquid crystal composition decreases, so the thickness of the film becomes roughly uniform, and there is a tendency that it is not easy to produce unevenness. The above-mentioned solid component can be appropriately determined considering the thickness of the liquid crystal cured film to be manufactured.
[0178] The polymerization initiator is a compound that generates reactive species by the contribution of heat or light and can initiate a polymerization reaction of a polymerizable liquid crystal compound or the like. As reactive species, there can be mentioned active species such as free radicals, cations or anions. Among them, from the viewpoint of easy control of the reaction, a photopolymerization initiator that generates free radicals by light irradiation is preferred.
[0179] Examples of the photopolymerization initiator include benzoin compounds, benzophenone compounds, benzyl ketal compounds, α-hydroxyketone compounds, α-aminoketone compounds, oxime compounds, triazine compounds, iodonium salts, and sulfonium salts. Specific examples include Irgacure (registered trademark) 907, Irgacure 184, Irgacure 651, Irgacure 819, Irgacure 250, Irgacure 369, Irgacure 379, Irgacure 127, Irgacure 2959, Irgacure 754, and Irgacure 379EG (all manufactured by BASF Japan Co., Ltd.), SEIKUOL BZ, SEIKUOL Z, and SEIKUOL BEE (all manufactured by Seiko Chemical Industries, Ltd.), kayacure BP100 (manufactured by Nippon Kayaku Co., Ltd.), kayacure UVI-6992 (manufactured by DOW), and ADEKA OPTOMER. SP-152, ADEKA OPTOMER SP-170, ADEKA OPTOMER N-1717, ADEKA OPTOMER N-1919, ADEKA ARKLS NCI-831, ADEKA ARKLSNCI-930 (the above are made by ADEKA Co., Ltd.), TAZ-A, TAZ-PP (the above are made by Japan Siber Hegner Co., Ltd.) and TAZ-104 (the above are made by Sanwa Chemical Co., Ltd.).
[0180] The photopolymerization initiator preferably has a maximum absorption wavelength of 300 nm to 400 nm, more preferably 300 nm to 380 nm, in order to fully utilize the energy emitted from the light source and achieve excellent productivity. Among them, α-acetophenone-based polymerization initiators and oxime-based photopolymerization initiators are preferred.
[0181] Examples of the α-acetophenone compound include 2-methyl-2-morpholino-1-(4-methylthiophenyl)-1-propanone, 2-dimethylamino-1-(4-morpholinophenyl)-2-benzyl-1-butanone, and 2-dimethylamino-1-(4-morpholinophenyl)-2-(4-methylphenylmethyl)-1-butanone. More preferred examples include 2-methyl-2-morpholino-1-(4-methylthiophenyl)-1-propanone and 2-dimethylamino-1-(4-morpholinophenyl)-2-benzyl-1-butanone. Examples of commercially available α-acetophenone compounds include Irgacure 369, 379EG, and 907 (all manufactured by BASF Japan Co., Ltd.) and SEIKUOL BEE (manufactured by Seiko Chemical Co., Ltd.).
[0182] Oxime-based photopolymerization initiators generate free radicals such as phenyl radicals and methyl radicals by irradiating light. The polymerization of polymerizable liquid crystal compounds is suitably carried out by the free radicals, wherein the oxime-based photopolymerization initiator that can generate methyl radicals is preferred from the perspective of high initiation efficiency of the polymerization reaction. In addition, from the perspective of making the polymerization reaction more efficient, it is preferred to use a photopolymerization initiator that can efficiently utilize ultraviolet rays of more than 350nm. As a photopolymerization initiator that can efficiently utilize ultraviolet rays of more than 350nm, it is preferably a triazine compound or a carbazole compound containing an oxime structure, and from the perspective of sensitivity, it is more preferably a carbazole compound containing an oxime ester structure. As a carbazole compound containing an oxime ester structure, 1-[4-(phenylthio)]-1,2-octanedione 2-(O-benzoyl oxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-ethanone 1-(O-acetyl oxime) and the like can be cited. Examples of commercially available products of oxime ester photopolymerization initiators include Irgacure OXE-01, Irgacure OXE-02, and Irgacure OXE-03 (all manufactured by BASF Japan Co., Ltd.), ADEKA OPTOMER N-1919, and ADEKA ARKLS NCI-831 (all manufactured by ADEKA Corporation).
[0183] The content of the photopolymerization initiator is usually 0.1 to 30 parts by mass, preferably 1 to 20 parts by mass, and more preferably 1 to 15 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound. Within the above range, the reaction of the polymerizable group proceeds sufficiently and the alignment of the polymerizable liquid crystal compound is less likely to be disturbed.
[0184] The leveling agent refers to an additive having the function of adjusting the fluidity of the polymerizable liquid crystal composition and making the coating film obtained by applying the composition flatter, and examples thereof include silicone-based, polyacrylate-based, and perfluoroalkyl-based leveling agents.As the leveling agent, commercially available products can be used, and specific examples thereof include DC3PA, SH7PA, DC11PA, SH28PA, SH29PA, SH30PA, ST80PA, ST86PA, SH8400, SH8700, and FZ2123 (all manufactured by Dow Corning Toray Co., Ltd.), KP321, KP323, KP324, KP326, KP340, KP341, X22-161A, and KF6001 (all manufactured by Shin-Etsu Chemical Co., Ltd.), TSF400, TSF401, TSF410, TSF4300, TSF4440, TSF4445, TSF-4446, TSF4452, and TSF4460 (all manufactured by Momentive Performance Materials Japan LLC), fluorinert (registered trademark) FC-72, fluorinert FC-40, fluorinert FC-43, fluorinert FC-3283 (all manufactured by Sumitomo 3M Co., Ltd.), MEGAFACE (registered trademark) R-08, MEGAFACE R-30, MEGAFACE R-90, MEGAFACE F-410, MEGAFACE F-411, MEGAFACE F-443, MEGAFACE F-445, MEGAFACE F-470, MEGAFACE F-477, MEGAFACE F-479, MEGAFACE F-482, MEGAFACE F-483, MEGAFACE F-556 (all manufactured by DIC Corporation), EFTOP (trade name) EF301, EFTOP EF303, EFTOP EF351, EFTOP EF352 (all of the above are manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd.), Surflon (registered trademark) S-381, Surflon S-382, Surflon S-383, Surflon S-393, Surflon SC-101, Surflon SC-105, KH-40, SA-100 (all of the above are manufactured by AGC Seimi Chemical Co., Ltd.), trade name E1830, trade name E5844 (manufactured by Daikin Fine Chemical Kenkyusho, KK), BM-1000, BM-1100, BYK-352, BYK-353 and BYK-361N (all trade names: manufactured by BM Chemie), etc.The leveling agent can be used alone or in combination of two or more.
[0185] The content of the leveling agent is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the leveling agent is within the above range, it is easy to align the polymerizable liquid crystal compound and the resulting liquid crystal cured film tends to be smoother, so it is preferred.
[0186] By combining an antioxidant, the polymerization reaction of the polymerizable liquid crystal compound can be controlled. As an antioxidant, it can be a primary antioxidant selected from phenolic antioxidants, amine antioxidants, quinone antioxidants, and nitroso antioxidants, or it can be a secondary antioxidant selected from phosphorus antioxidants and sulfur antioxidants. In order to polymerize the polymerizable liquid crystal compound without disturbing the orientation of the polymerizable liquid crystal compound, the content of the antioxidant is usually 0.01 to 10 parts by mass, preferably 0.1 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound. The antioxidant can be used alone or in combination of two or more.
[0187] In addition, by using a photosensitizer, the photopolymerization initiator can be highly sensitive. As a photosensitizer, for example, xanthone such as xanthone and thioxanthone; anthracenes with substituents such as anthracene and alkyl ether; thiophenazine; rubrene. The photosensitizer can be used alone or in combination of two or more. The content of the photosensitizer is usually 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound.
[0188] The polymerizable liquid crystal composition used for forming the horizontally aligned liquid crystal cured film can be obtained by stirring a polymerizable liquid crystal compound, a solvent, a photopolymerization initiator, and components other than the polymerizable liquid crystal compound at a predetermined temperature.
[0189] [Optically anisotropic layer Y]
[0190] As the optically anisotropic layer Y constituting the laminate of the present invention, for example, a cured product of a polymerizable liquid crystal composition obtained by curing a polymerizable liquid crystal compound in a state of being oriented in a vertical direction relative to the film plane (hereinafter also referred to as "vertical alignment liquid crystal cured film") can be cited. In the present invention, the vertical alignment liquid crystal cured film preferably includes a vertical alignment promoter. That is, in the present invention, the polymerizable liquid crystal composition forming the vertical alignment liquid crystal cured film preferably includes a vertical alignment promoter. In the present invention, the so-called vertical alignment promoter refers to a material that promotes the liquid crystal orientation of the polymerizable liquid crystal compound in a direction perpendicular to the film plane. By forming the vertical alignment liquid crystal cured film by a polymerizable liquid crystal composition including a vertical alignment promoter, a vertical alignment liquid crystal cured film can be formed without a vertical alignment film. Thus, in the laminate of the present invention, there is no need to form a vertical alignment film, the manufacturing process of the laminate is simplified, and the laminate can be manufactured with good productivity.
[0191] As a vertical alignment promoter that promotes the alignment of the polymerizable liquid crystal compound in the vertical direction, ionic compounds formed by non-metal atoms and non-ionic silane compounds can be cited. The vertically aligned liquid crystal cured film preferably contains at least one of a non-ionic silane compound and an ionic compound formed by a non-metal atom, and more preferably contains both a non-ionic silane compound and an ionic compound formed by a non-metal atom.
[0192] When the polymerizable liquid crystal composition forming the vertically oriented liquid crystal cured film contains a nonionic silane compound, the nonionic silane compound reduces the surface tension of the polymerizable liquid crystal composition. In the dried coating formed by the polymerizable liquid crystal composition, the nonionic silane compound tends to be biased at the interface between the dried coating and the air, thereby improving the vertical orientation control force for the polymerizable liquid crystal compound, and tends to orient the polymerizable liquid crystal compound in the dried coating in a vertical direction relative to the film plane. Thus, the liquid crystal cured film can be formed while maintaining the vertical orientation state of the polymerizable liquid crystal compound.
[0193] Nonionic silane compounds are nonionic compounds containing Si element. Examples of nonionic silane compounds include silicone polymers such as polysilane, silicone resins such as silicone oil and silicone resin, and organosilicon oligomers, organic inorganic silane compounds such as silsesquioxane and alkoxysilane (more specifically, silane coupling agents, etc.).
[0194] The nonionic silane compound may be a silicone monomer type or a silicone oligomer (polymer) type. In addition, the nonionic silane compound may be used alone or in combination of two or more.
[0195] Silane coupling agent is a compound containing Si element with at least one functional group selected from the group consisting of vinyl, epoxy, styryl, methacryloyl, acryl, amino, isocyanurate, urea, sulfydryl, isocyanate, carboxyl and hydroxyl at the end, and at least one alkoxysilyl or silanol group. By appropriately selecting these functional groups, it is possible to give the improvement of the mechanical strength of the vertically oriented liquid crystal curing film, the surface modification of the vertically oriented liquid crystal curing film, and the improvement of the adhesion of the layer adjacent to the vertically oriented liquid crystal curing film. From the viewpoint of adhesion, silane coupling agent is preferably a silane coupling agent with an alkoxysilyl and another different reactive group (for example, the above-mentioned functional group). Silane coupling agent is further preferably a silane coupling agent with an alkoxysilyl and a polar group. When the silane coupling agent has at least one alkoxysilyl and at least one polar group in its molecule, the vertical orientation of the polymerizable liquid crystal compound is easily further improved, and there is a trend that can significantly obtain a vertical orientation promotion effect. Examples of the polar group include an epoxy group, an amino group, an isocyanurate group, a mercapto group, a carboxyl group, and a hydroxyl group. In addition, the polar group may have a substituent or a protective group as appropriate in order to control the reactivity of the silane coupling agent.
[0196] Examples of commercially available silane coupling agents include KP321, KP323, KP324, KP326, KP340, KP341, X22-161A, KF6001, KBM-1003, KBE-1003, KBM-303, KBM-402, KBM-403, KBE-402, KBE-403, KBM-1403, KBM-502, KBM-503, Silane coupling agents manufactured by Shin-Etsu Chemical Co., Ltd. such as KBE-502, KBE-503, KBM-5103, KBM-602, KBM-603, KBM-903, KBE-903, KBE-9103, KBM-573, KBM-575, KBM-9659, KBE-585, KBM-802, KBM-803, KBE-846, and KBE-9007.
[0197] When the polymerizable liquid crystal composition forming the vertically aligned liquid crystal cured film includes a nonionic silane compound, the content thereof is generally preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and further preferably 0.1 to 3 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound contained in the polymerizable liquid crystal composition. When the content of the nonionic silane compound is within the above range, the vertical alignment of the polymerizable liquid crystal compound can be effectively promoted while maintaining the good coating properties of the polymerizable liquid crystal composition.
[0198] When the polymerizable liquid crystal composition forming the vertically aligned liquid crystal cured film contains an ionic compound formed by non-metallic atoms, in the dried coating formed by the polymerizable liquid crystal composition, a vertical alignment control force for the polymerizable liquid crystal compound is presented by means of electrostatic interaction, and there is a tendency to align the polymerizable liquid crystal compound in the dried coating in a vertical direction relative to the film plane. Thus, the liquid crystal cured film can be formed while maintaining the vertically aligned state of the polymerizable liquid crystal compound.
[0199] As the ionic compound formed by non-metallic atoms, for example, onium salts (more specifically, quaternary ammonium salts, tertiary sulfonium salts, and quaternary phosphonium salts with positive charges on nitrogen atoms, etc.) can be cited. Among these onium salts, from the viewpoint of being able to further improve the vertical orientation of polymerizable liquid crystal compounds, quaternary onium salts are preferred, and from the viewpoint of improving availability and mass production, quaternary phosphonium salts or quaternary ammonium salts are more preferred. Onium salts can have more than two quaternary onium salt sites in the molecule, or can be oligomers or polymers.
[0200] The molecular weight of the ionic compound formed by the non-metallic atom is preferably 100 to 10,000. When the molecular weight is within the above range, it is easy to improve the vertical alignment of the polymerizable liquid crystal compound while ensuring the coating property of the polymerizable composition. The molecular weight of the ionic compound is more preferably 5000 or less, and further preferably 3000 or less.
[0201] As the cationic component of the ionic compound formed by the non-metal atom, for example, inorganic cations and organic cations can be cited. Among them, organic cations are preferred from the aspect of not being easy to produce the orientation defects of the polymerizable liquid crystal compound. As the organic cation, for example, imidazolium cations, pyridinium cations, ammonium cations, sulfonium cations and phosphonium cations can be cited.
[0202] The ionic compound formed by the non-metallic atom usually has a counter anion. As the anion component that becomes the counter ion of the above-mentioned cationic component, for example, inorganic anions and organic anions can be cited. Among them, from the aspect of not being easy to produce the orientation defect of the polymerizable liquid crystal compound, organic anions are preferred. It should be noted that the cation and the anion do not necessarily correspond one to one.
[0203] Specific examples of the anion component include the following anions.
[0204] Chloride anion 〔Cl-〕,
[0205] Bromide anion - 〕、
[0206] Iodide anion 〔I-〕,
[0207] Tetrachloroaluminate anion 〔AlCl4- 〕、
[0208] Heptachlorodialuminate anion 〔Al2Cl7 - 〕、
[0209] Tetrafluoroborate anion 〔BF4 - 〕、
[0210] Hexafluorophosphate anion 〔PF6 - 〕、
[0211] Perchlorate anion 〔ClO4 - 〕、
[0212] Nitrate anion 〔NO3 - 〕、
[0213] Acetate anion 〔CH3COO - 〕、
[0214] trifluoroacetate anion 〔CF3COO - 〕、
[0215] Fluorosulfonate anion 〔FSO3 - 〕、
[0216] Methanesulfonate anion 〔CH3SO3 - 〕、
[0217] trifluoromethanesulfonate anion 〔CF3SO3 - 〕、
[0218] p-Toluenesulfonate anion 〔p-CH3C6H4SO3 - 〕、
[0219] Bis(fluorosulfonyl)imide anion〔(FSO2)2N-〕,
[0220] Bis(trifluoromethanesulfonyl)imide anion〔(CF3SO2)2N - 〕、
[0221] Tris(trifluoromethanesulfonyl)methane anion〔(CF3SO2)3C-〕,
[0222] Hexafluoroarsenate anion 〔AsF6 - 〕、
[0223] Hexafluoroantimonate anion 〔SbF6 - 〕、
[0224] Hexafluoroniobate anion〔NbF6 - 〕、
[0225] Hexafluorotantalate anion 〔TaF6 -〕、
[0226] Dimethylphosphinate anion〔(CH3)2POO - 〕、
[0227] (poly)hydrofluorofluoride anion〔F(HF) n - 〕(for example, n represents an integer from 1 to 3),
[0228] Dicyanamide anion〔(CN)2N - 〕、
[0229] SCN - 〕、
[0230] Perfluorobutanesulfonate anion 〔C4F9SO3 - 〕、
[0231] Bis(pentafluoroethanesulfonyl)imide anion〔(C2F5SO2)2N - 〕、
[0232] Perfluorobutyrate anion 〔C3F7COO - 〕,and
[0233] (Trifluoromethanesulfonyl)(trifluoromethanecarbonyl)imide anion〔(CF3SO2)(CF3CO)N - 〕.
[0234] Specific examples of the ionic compound formed of non-metal atoms can be appropriately selected from the above-mentioned combinations of cation components and anion components. Specific examples of the compound of the combination of cation components and anion components include the following compounds.
[0235] (Pyridinium salt)
[0236] N-hexylpyridinium hexafluorophosphate,
[0237] N-octylpyridinium hexafluorophosphate,
[0238] N-methyl-4-hexylpyridinium hexafluorophosphate,
[0239] N-butyl-4-methylpyridinium hexafluorophosphate,
[0240] N-octyl-4-methylpyridinium hexafluorophosphate,
[0241] Bis(fluorosulfonyl)imide N-hexylpyridinium,
[0242] Bis(fluorosulfonyl)imide N-octylpyridinium,
[0243] N-methyl-4-hexylpyridinium bis(fluorosulfonyl)imide,
[0244] N-butyl-4-methylpyridinium bis(fluorosulfonyl)imide,
[0245] Bis(fluorosulfonyl)imide N-octyl-4-methylpyridinium,
[0246] N-hexylpyridinium bis(trifluoromethanesulfonyl)imide,
[0247] N-octylpyridinium bis(trifluoromethanesulfonyl)imide,
[0248] N-methyl-4-hexylpyridinium bis(trifluoromethanesulfonyl)imide,
[0249] N-butyl-4-methylpyridinium bis(trifluoromethanesulfonyl)imide,
[0250] Bis(trifluoromethanesulfonyl)imide N-octyl-4-methylpyridinium,
[0251] N-hexylpyridinium p-toluenesulfonate,
[0252] N-Octylpyridinium p-toluenesulfonate,
[0253] N-methyl-4-hexylpyridinium p-toluenesulfonate,
[0254] N-butyl-4-methylpyridinium p-toluenesulfonate, and
[0255] N-Octyl-4-methylpyridinium p-toluenesulfonate.
[0256] (Imidazolium salt)
[0257] 1-Ethyl-3-methylimidazolium hexafluorophosphate,
[0258] 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide,
[0259] 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide,
[0260] 1-Ethyl-3-methylimidazolium p-toluenesulfonate,
[0261] 1-Butyl-3-methylimidazolium methanesulfonate, etc.
[0262] (Pyrrolidinium salt)
[0263] N-butyl-N-methylpyrrolidinium hexafluorophosphate,
[0264] Bis(fluorosulfonyl)imide N-butyl-N-methylpyrrolidinium,
[0265] N-butyl-N-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide,
[0266] N-butyl-N-methylpyrrolidinium p-toluenesulfonate, etc.
[0267] (Ammonium salt)
[0268] Tetrabutylammonium hexafluorophosphate,
[0269] Tetrabutylammonium bis(fluorosulfonyl)imide,
[0270] Tetrahexyl ammonium bis(fluorosulfonyl)imide,
[0271] Bis(fluorosulfonyl)imide trioctylmethylammonium,
[0272] Bis(fluorosulfonyl)imide (2-hydroxyethyl)trimethylammonium,
[0273] Tetrabutylammonium bis(trifluoromethanesulfonyl)imide,
[0274] Tetrahexylammonium bis(trifluoromethanesulfonyl)imide,
[0275] Bis(trifluoromethanesulfonyl)imide trioctylmethylammonium,
[0276] Bis(trifluoromethanesulfonyl)imide (2-hydroxyethyl)trimethylammonium,
[0277] Tetrabutylammonium p-toluenesulfonate,
[0278] Tetrahexyl ammonium p-toluenesulfonate,
[0279] Trioctylmethylammonium p-toluenesulfonate,
[0280] (2-Hydroxyethyl)trimethylammonium p-toluenesulfonate,
[0281] (2-Hydroxyethyl)trimethylammonium dimethylphosphinate,
[0282] Bis(trifluoromethanesulfonyl)imide 1-(3-trimethoxysilylpropyl)-1,1,1-tributylammonium,
[0283] 1-(3-trimethoxysilylpropyl)-1,1,1-trimethylammonium bis(trifluoromethanesulfonyl)imide,
[0284] Bis(trifluoromethanesulfonyl)imide 1-(3-trimethoxysilylbutyl)-1,1,1-tributylammonium,
[0285] 1-(3-trimethoxysilylbutyl)-1,1,1-trimethylammonium bis(trifluoromethanesulfonyl)imide,
[0286] Bis(trifluoromethanesulfonyl)imide N-{(3-triethoxysilylpropyl)carbamoyloxyethyl)}-N,N,N-trimethylammonium, and
[0287] Bis(trifluoromethanesulfonyl)imide N-[2-{3-(3-trimethoxysilylpropylamino)-1-oxopropoxy}ethyl]-N,N,N-trimethylammonium.
[0288] (Phosphonium salt)
[0289] Bis(trifluoromethanesulfonyl)imide tributyl(2-methoxyethyl)phosphonium,
[0290] Bis(trifluoromethanesulfonyl)imide tributylmethylphosphonium,
[0291] 1,1,1-trimethyl-1-[(trimethoxysilyl)methyl]phosphonium bis(trifluoromethanesulfonyl)imide,
[0292] 1,1,1-trimethyl-1-[2-(trimethoxysilyl)ethyl]phosphonium bis(trifluoromethanesulfonyl)imide,
[0293] 1,1,1-trimethyl-1-[3-(trimethoxysilyl)propyl]phosphonium bis(trifluoromethanesulfonyl)imide,
[0294] 1,1,1-trimethyl-1-[4-(trimethoxysilyl)butyl]phosphonium bis(trifluoromethanesulfonyl)imide,
[0295] 1,1,1-tributyl-1-[(trimethoxysilyl)methyl]phosphonium bis(trifluoromethanesulfonyl)imide,
[0296] 1,1,1-tributyl-1-[2-(trimethoxysilyl)ethyl]phosphonium bis(trifluoromethanesulfonyl)imide, and
[0297] 1,1,1-tributyl-1-[3-(trimethoxysilyl)propyl]phosphonium bis(trifluoromethanesulfonyl)imide.
[0298] The above-mentioned ionic compounds may be used alone or in combination of two or more. Among them, ionic compounds composed of phosphonium salts or ammonium salts are preferred.
[0299] From the viewpoint of being able to further improve the vertical alignment of the polymerizable liquid crystal compound, the ionic compound preferably has Si element and / or F element in the molecular structure of the cationic part. When the ionic compound has Si element and / or F element in the molecular structure of the cationic part, it is easy to segregate the ionic compound on the surface of the vertically aligned liquid crystal cured film. Among them, as ionic compounds whose constituent elements are all non-metallic elements, the following ionic compounds (i) to (iii) are preferred.
[0300] (Ionic compound (i))
[0301] [Chemical formula 14]
[0302]
[0303] (Ionic compound (ii))
[0304] [Chemical formula 15]
[0305]
[0306] (Ionic compound (iii))
[0307] [Chemical formula 16]
[0308]
[0309] For example, a method of improving the orientation of liquid crystal by treating the surface of the substrate with a surfactant having a long alkyl group of a certain chain length (for example, see Chapter 2 of "Liquid Crystal Handbook: Orientation and Physical Properties of Liquid Crystals" (published by Maruzen Co., Ltd.) etc.) can be applied to further improve the vertical orientation of the polymerizable liquid crystal compound. That is, by treating the surface of the substrate with an ionic compound having a long alkyl group of a certain chain length, the vertical orientation of the polymerizable liquid crystal compound can be effectively improved.
[0310] Specifically, the ionic compound formed from non-metal atoms preferably satisfies the following formula (10).
[0311] 5 <M<16 (10)
[0312] In formula (10), M is represented by the following formula (11).
[0313] M = (the number of covalent bonds from the positively charged atom to the molecular chain terminal of the substituent with the largest number of covalent bonds to the molecular chain terminal among the substituents directly bonded to the positively charged atom) ÷ (the number of positively charged atoms) (11)
[0314] When the ionic compound composed of non-metal atoms satisfies the above-mentioned (10), the vertical alignment property of the polymerizable liquid crystal compound can be effectively improved.
[0315] It should be noted that, when there are two or more atoms with positive charge in the molecule of the ionic compound formed by non-metallic atoms, for a substituent having two or more atoms with positive charge, the number of covalent bonds from the atom with positive charge regarded as the base point to the closest another atom with positive charge is taken as the "number of covalent bonds from the atom with positive charge to the end of the molecular chain" described in the above definition of M. In addition, when the ionic compound formed by non-metallic atoms is an oligomer or polymer having two or more repeating units, the constituent unit is regarded as one molecule and the above M is calculated. When the atom with positive charge is incorporated in a ring structure, the number of covalent bonds from the ring structure to the atom with positive charge or the number of covalent bonds to the end of the substituent bonded to the ring structure, whichever has more covalent bonds, is taken as the "number of covalent bonds from the atom with positive charge to the end of the molecular chain" described in the above definition of M.
[0316] When the polymerizable liquid crystal composition forming the vertically aligned liquid crystal cured film includes an ionic compound formed by non-metallic atoms, the content thereof is generally preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and further preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound contained in the polymerizable liquid crystal composition. When the content of the ionic compound is within the above range, the vertical alignment of the polymerizable liquid crystal compound can be effectively promoted while maintaining the good coating properties of the polymerizable liquid crystal composition.
[0317] The polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film contains both a nonionic silane compound and an ionic compound formed by non-metallic atoms, so that in the dried coating formed by the polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film, the vertical alignment of the polymerizable liquid crystal compound is further promoted by means of the electrostatic interaction derived from the ionic compound and the surface tension reduction effect derived from the nonionic silane compound. Thus, the liquid crystal cured film can be formed while maintaining the state in which the polymerizable liquid crystal compound is further accurately aligned vertically.
[0318] The vertically aligned liquid crystal cured film is preferably a cured product of a polymerizable liquid crystal composition comprising the above-mentioned alignment promoter and at least one polymerizable liquid crystal compound, and more preferably a liquid crystal cured film formed by curing a polymerizable liquid crystal compound having at least one free radical polymerizable group in a state of being oriented vertically relative to the in-plane direction of the liquid crystal cured film. In the present invention, the polymerizable liquid crystal compound contained in the polymerizable liquid crystal composition forming the vertically aligned liquid crystal cured film refers to a liquid crystal compound having a polymerizable group in the same manner as the compound shown in the horizontally aligned liquid crystal cured film, and a liquid crystal compound having at least one free radical polymerizable group is particularly preferred. The polymerizable liquid crystal compound is not particularly limited, and for example, a polymerizable liquid crystal compound previously known in the field of phase difference films can be used.
[0319] As the optically anisotropic layer Y of the present invention, the vertically aligned liquid crystal cured film is preferably formed on a layer having no vertical alignment control force without interposing the vertically aligned film. In the laminate of the present invention, the vertically aligned liquid crystal cured film can be formed without the vertically aligned film, so the number of manufacturing steps of the laminate is reduced, and the laminate can be manufactured with good productivity.
[0320] The polymerizable liquid crystal compound constituting the vertically aligned liquid crystal curing film is not particularly limited, and for example, a polymerizable liquid crystal compound previously known in the field of phase difference film can be used. Specifically, a polymerizable liquid crystal compound (X) or a polymerizable liquid crystal compound (Y) exemplified as a polymerizable liquid crystal compound that can be used in the formation of a horizontally aligned liquid crystal curing film can be used, wherein it is preferred to include at least one polymerizable liquid crystal compound showing so-called reverse wavelength dispersion, for example, a polymerizable liquid crystal compound (X) can be preferably used. In the polymerizable liquid crystal composition for forming a vertically aligned liquid crystal curing film, the polymerizable liquid crystal compound can be used alone or in combination of two or more, and the polymerizable liquid crystal compound (X) can also be used in combination with the polymerizable liquid crystal compound (Y).
[0321] The thickness of the optically anisotropic layer Y is preferably 0.3 μm to 5 μm, more preferably 0.4 μm to 4.5 μm, and further preferably 0.5 μm to 4 μm. The horizontally aligned liquid crystal cured film having the thickness of the optically anisotropic layer Y satisfying the above range can achieve a lightweight image display device.
[0322] The content of the polymerizable liquid crystal compound in the polymerizable liquid crystal composition used in the formation of the vertically aligned liquid crystal cured film is, for example, 70 to 99.5 parts by mass, preferably 80 to 99 parts by mass, more preferably 85 to 98 parts by mass, and further preferably 90 to 95 parts by mass, relative to 100 parts by mass of the solid content of the polymerizable liquid crystal composition. When the content of the polymerizable liquid crystal compound is within the above range, it is advantageous from the viewpoint of the orientation of the obtained liquid crystal cured film.
[0323] The polymerizable liquid crystal composition used in the formation of the vertical alignment liquid crystal cured film may contain additives such as a solvent, a polymerization initiator, a leveling agent, an antioxidant, and a photosensitizer in addition to the polymerizable liquid crystal compound or the polymerizable liquid crystal compound and the vertical alignment promoter. As these components, the same components as those exemplified above as components that can be used in the horizontal alignment liquid crystal cured film can be cited, and only one of each can be used, or two or more can be used in combination.
[0324] The polymerizable liquid crystal composition used for forming the vertically aligned liquid crystal cured film can be obtained by stirring a polymerizable liquid crystal compound, a solvent, a photopolymerization initiator and other components other than the polymerizable liquid crystal compound at a predetermined temperature.
[0325] [Method for producing laminate]
[0326] The laminate of the present invention comprises an optical anisotropic layer X and an optical anisotropic layer Y. As the optical anisotropic layer X, as described above, for example, a stretched film or a polymerizable liquid crystal compound can be used, and a cured product layer of a polymerizable liquid crystal composition obtained by curing in a state where the polymerizable liquid crystal compound is oriented in a horizontal direction relative to the film plane (horizontally oriented liquid crystal cured film). In addition, as the optical anisotropic layer Y, for example, a cured product of a polymerizable liquid crystal composition obtained by curing in a state where the polymerizable liquid crystal compound is oriented in a vertical direction relative to the film plane (vertically oriented liquid crystal cured film) can be used.
[0327] With regard to the laminate of the present invention, for example, a laminate having an optically anisotropic layer Y directly on an optically anisotropic layer X can be manufactured by the following process, wherein a coating film of a polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film containing a polymerizable liquid crystal compound is formed on a stretched film, and a vertically aligned liquid crystal cured film is formed from the coating film (hereinafter also referred to as a “vertically aligned liquid crystal cured film forming process”).
[0328] With regard to the laminate of the present invention, for example, a laminate having an optically anisotropic layer Y directly on an optically anisotropic layer X can be manufactured by the following method, which sequentially comprises: forming a coating film of a polymerizable liquid crystal composition for forming a horizontally aligned liquid crystal cured film containing a polymerizable liquid crystal compound, a step of forming a horizontally aligned liquid crystal cured film from the coating film (hereinafter also referred to as a “horizontally aligned liquid crystal cured film forming step”); and a vertically aligned liquid crystal cured film forming step.
[0329] In the laminate of the present invention, when the optically anisotropic layer X is formed of a horizontally aligned liquid crystal cured film, it is preferred that a step of forming a coating film of a horizontally aligned film-forming composition and forming a horizontally aligned film from the coating film (hereinafter also referred to as a "horizontal aligned film forming step") is included before forming the horizontally aligned liquid crystal cured film. It is preferred that the horizontally aligned film forming step and the horizontally aligned liquid crystal cured film forming step are performed sequentially. The optically anisotropic layer X composed of a horizontally aligned liquid crystal cured film formed on the horizontally aligned film is obtained by a manufacturing method including a horizontally aligned film forming step.
[0330] In the horizontal alignment liquid crystal cured film forming step, the horizontal alignment liquid crystal cured film can be produced, for example, by the following method, which includes:
[0331] A step of applying a polymerizable liquid crystal composition for forming a horizontally aligned liquid crystal cured film onto a substrate or an alignment film to obtain a coating film;
[0332] A step of drying the coating to form a dried coating; and
[0333] A step of irradiating the dried coating film with active energy rays to form a horizontally aligned liquid crystal cured film.
[0334] The coating film of the polymerizable liquid crystal composition can be formed by, for example, applying the polymerizable liquid crystal composition for forming a horizontally aligned liquid crystal cured film on a substrate, an alignment film described later, or the like.
[0335] As the substrate, for example, a glass substrate, a film substrate, etc. can be cited, but from the viewpoint of processability, a resin film substrate is preferred. As the resin constituting the film substrate, for example, polyolefins such as polyethylene, polypropylene, and norbornene polymers; cyclic olefin resins; polyvinyl alcohol; polyethylene terephthalate; polymethacrylate; polyacrylate; cellulose esters such as cellulose triacetate, cellulose diacetate, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyethersulfone; polyetherketone; plastics such as polyphenylene sulfide and polyphenylene ether. Such resins can be made into substrates by known means such as solvent casting and melt extrusion. The surface of the substrate can have a protective layer formed by acrylic resin, methacrylic resin, epoxy resin, oxetane resin, polyurethane resin, melamine resin, etc., and surface treatments such as mold release treatment, corona treatment, and plasma treatment such as silicone treatment can also be implemented.
[0336] As the substrate, commercially available products can be used. Examples of commercially available cellulose ester substrates include cellulose ester substrates manufactured by Fuji Photo Film Co., Ltd. such as Fujitack Film; cellulose ester substrates manufactured by Konica Minolta Opto Co., Ltd. such as "KC8UX2M", "KC8UY", and "KC4UY", etc. Examples of commercially available cyclic olefin resins include cyclic olefin resins manufactured by Ticona (Germany) such as "Topas (registered trademark)"; cyclic olefin resins manufactured by JSR Corporation such as "ARTON (registered trademark)"; cyclic olefin resins manufactured by Zeon Co., Ltd. such as "ZEONOR (Registered Trademark)" and "ZEONEX (Registered Trademark)"; and cyclic olefin resins manufactured by Mitsui Chemicals, Inc. such as "Apel (Registered Trademark). Commercially available cyclic olefin resin substrates may also be used. Examples of commercially available cyclic olefin resin substrates include cyclic olefin resin substrates such as "Escena (registered trademark)" and "SCA40 (registered trademark)" manufactured by Sekisui Chemical Co., Ltd.; cyclic olefin resin substrates such as "ZEONORFILM (registered trademark)" manufactured by OPTES Co., Ltd.; and cyclic olefin resin substrates such as "ARTONFILM (registered trademark)" manufactured by JSR Co., Ltd.
[0337] From the viewpoints of thinning the laminate, ease of peeling of the substrate, and operability of the substrate, the thickness of the substrate is usually 5 to 300 μm, preferably 10 to 150 μm. In addition, when the substrate is arranged in the laminate of the present invention, from the viewpoint of optical compensation described later, the substrate is preferably optically isotropic. In the present invention, the so-called optical isotropy means that the in-plane phase difference value of the substrate is 3 nm or less.
[0338] Examples of a method for applying the polymerizable liquid crystal composition to a substrate include known methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and coater coating, and printing methods such as flexographic printing.
[0339] Then, the solvent is removed by drying, etc. to form a dry coating. As a drying method, natural drying, ventilation drying, heating drying and reduced pressure drying methods, etc. can be cited. At this time, by heating the coating obtained by the polymerizable liquid crystal composition, the polymerizable liquid crystal compound can be oriented in the horizontal direction relative to the coating plane while the solvent is dried and removed from the coating. The heating temperature of the coating can be appropriately determined by considering the materials of the polymerizable liquid crystal compound used and the substrate to be formed, but in order to make the polymerizable liquid crystal compound phase change to a liquid crystal phase state, it is usually necessary to be a temperature above the liquid crystal phase transition temperature. In order to remove the solvent contained in the polymerizable liquid crystal composition and make the polymerizable liquid crystal compound become a horizontal orientation state, for example, it can be heated to a temperature above the liquid crystal phase transition temperature (smectic phase transition temperature or nematic phase transition temperature) of the polymerizable liquid crystal compound contained in the above-mentioned polymerizable liquid crystal composition.
[0340] It should be noted that the liquid crystal phase transition temperature can be measured using, for example, a polarizing microscope, a differential scanning calorimeter (DSC), a thermogravimetric differential thermal analyzer (TG-DTA), etc., which are equipped with a temperature regulating station. In addition, when two or more kinds are used in combination as polymerizable liquid crystal compounds, the above-mentioned phase transition temperature refers to: a mixture of polymerizable liquid crystal compounds obtained by mixing all polymerizable liquid crystal compounds constituting the polymerizable liquid crystal composition in the same ratio as the composition in the polymerizable liquid crystal composition, and the temperature measured by operating in the same manner as when using one polymerizable liquid crystal compound. It should be noted that it is known that the following situation usually exists: the liquid crystal phase transition temperature of the polymerizable liquid crystal compound in the aforementioned polymerizable liquid crystal composition is lower than the liquid crystal phase transition temperature of the polymerizable liquid crystal compound monomer.
[0341] The heating time can be appropriately determined depending on the heating temperature, the type of polymerizable liquid crystal compound used, the type of solvent, its boiling point and its amount, etc., and is usually 15 seconds to 10 minutes, preferably 0.5 to 5 minutes.
[0342] The removal of the solvent from the coating can be carried out simultaneously with the heating reaching the liquid crystal phase transition temperature of the polymerizable liquid crystal compound, or it can be carried out independently, but from the viewpoint of improving productivity, it is preferably carried out simultaneously. Before the heating reaching the liquid crystal phase transition temperature of the polymerizable liquid crystal compound, a pre-drying process for appropriately removing the solvent in the coating under the condition that the polymerizable liquid crystal compound contained in the coating obtained by the polymerizable liquid crystal composition is not polymerized can be provided. As the drying method in the pre-drying process, natural drying method, ventilation drying method, heating drying and reduced pressure drying method, etc. can be cited, and the drying temperature (heating temperature) in the drying process can be appropriately determined according to the type of polymerizable liquid crystal compound used, the type of solvent, its boiling point and its amount, etc.
[0343] Next, in the obtained dry coating, in the state of maintaining the horizontal orientation state of the polymerizable liquid crystal compound, the polymerizable liquid crystal compound is polymerized to form a horizontally oriented liquid crystal cured film. As a polymerization method, thermal polymerization and photopolymerization can be cited, but from the viewpoint of easy control of polymerization reaction, photopolymerization is preferred. In photopolymerization, as the light irradiated to the dry coating, it can be appropriately selected according to the type of polymerization initiator contained in the dry coating, the type of polymerizable liquid crystal compound (especially the type of polymerizable group possessed by the polymerizable liquid crystal compound) and its amount. As a specific example, one or more light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α rays, β rays and γ rays, and active electron beams can be cited. Among them, from the aspect of easy control of the progress of the polymerization reaction, it can be used as a photopolymerization device and the device widely used in the art is considered, preferably ultraviolet light, preferably in a way that ultraviolet light can be used for photopolymerization The type of polymerizable liquid crystal compound and polymerization initiator contained in the polymerizable liquid crystal composition is pre-selected. In addition, during polymerization, it is also possible to control the polymerization temperature by irradiating light while cooling the dried coating using appropriate cooling means. If the polymerization of the polymerizable liquid crystal compound is implemented at a lower temperature by adopting such cooling means, even if a substrate with lower heat resistance is used, a horizontally oriented liquid crystal cured film can be appropriately formed. In addition, within the range of the unfavorable conditions (deformation of the substrate due to heat, etc.) caused by the heat during light irradiation, it is also possible to promote the polymerization reaction by increasing the polymerization temperature. During photopolymerization, by shielding, developing, etc., a patterned cured film can also be obtained.
[0344] As the light source of the aforementioned active energy rays, for example, there can be mentioned a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting light in the wavelength range of 380 to 440 nm, a chemical lamp, a black light lamp, a microwave-excited mercury lamp, a metal halide lamp, and the like.
[0345] UV radiation intensity is usually 10 to 3,000 mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in the wavelength region effective for activating the photopolymerization initiator. The irradiation time is usually 0.1 second to 10 minutes, preferably 0.1 second to 5 minutes, more preferably 0.1 second to 3 minutes, and further preferably 0.1 second to 1 minute. When irradiation is performed once or more times with such an ultraviolet irradiation intensity, the cumulative light amount is 10 to 3,000 mJ / cm 2 , preferably 50 to 2,000 mJ / cm 2 , more preferably 100 to 1,000 mJ / cm 2 .
[0346] Since the alignment order of the horizontally aligned liquid crystal cured film can be improved, it is preferred in the present invention that the coating film of the polymerizable liquid crystal composition for forming the horizontally aligned liquid crystal cured film is formed on the horizontally aligned film having an alignment control force in the horizontal direction relative to the plane of the obtained liquid crystal cured film. Therefore, in the laminate of the present invention, it is preferred that the optically anisotropic layer X is formed on the horizontally aligned film, and the horizontally aligned liquid crystal cured film is sequentially included.
[0347] The alignment control force of the alignment film can be arbitrarily adjusted by the type of the alignment film, the surface state, the rubbing conditions, etc., and when the alignment film is formed of a photo-aligning polymer, it can be arbitrarily adjusted by the polarized light irradiation conditions, etc.
[0348] As a horizontal alignment film, it is preferred to have solvent resistance that does not dissolve due to the coating of the polymerizable liquid crystal composition, etc., and heat resistance in the heating treatment for the removal of the solvent and the orientation of the polymerizable liquid crystal compound described later. As alignment films, alignment films including alignment polymers, photoalignment films, groove alignment films having a concave-convex pattern and multiple grooves on the surface, and stretched films stretched along the alignment direction can be cited. From the perspective of the accuracy and quality of the orientation angle, photoalignment films are preferred.
[0349] As the oriented polymer, for example, polyamides having amide bonds in the molecule, gelatins, polyimides having imide bonds in the molecule and polyamic acid, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinyl pyrrolidone, polyacrylic acid and polyacrylates can be cited. Among them, polyvinyl alcohol is preferred. The oriented polymer can be used alone or in combination of two or more.
[0350] An oriented film containing an oriented polymer can be generally obtained by applying a composition obtained by dissolving an oriented polymer in a solvent (hereinafter, sometimes referred to as an "oriented polymer composition") on a substrate and removing the solvent; or by applying the oriented polymer composition on a substrate, removing the solvent, and rubbing (rubbing method). As the solvent, the same solvent as the solvent exemplified above as a solvent that can be used for the polymerizable liquid crystal composition can be cited.
[0351] The concentration of the oriented polymer in the oriented polymer composition may be within a range in which the oriented polymer material can be completely dissolved in the solvent, and is preferably about 0.1 to 20%, more preferably about 0.1 to 10%, in terms of solid content relative to the solution.
[0352] As the oriented polymer composition, a commercially available oriented film material may be used as it is. Examples of commercially available oriented film materials include SUNEVER (registered trademark, manufactured by Nissan Chemical Industries, Ltd.) and Optomer (registered trademark, manufactured by JSR Corporation).
[0353] As a method for applying the oriented polymer composition to the substrate, the same method as the method exemplified above as the method for applying the polymerizable liquid crystal composition to the substrate can be mentioned.
[0354] Examples of a method for removing the solvent contained in the oriented polymer composition include a natural drying method, a ventilation drying method, a heat drying method, and a reduced pressure drying method.
[0355] In order to impart an orientation control force to the oriented film, a rubbing treatment (rubbing method) may be performed as required. As a method of imparting an orientation control force by rubbing method, the following method may be cited: a film of an oriented polymer formed on the surface of a substrate by coating an oriented polymer composition on a substrate and annealing the oriented polymer composition is brought into contact with a rubbing roller wound with a rubbing cloth and rotating. During the rubbing treatment, if shielding is performed, multiple regions (patterns) with different orientation directions can also be formed on the oriented film.
[0356] As a preferred embodiment of the present invention, the horizontal alignment film is a photoalignment film formed of a polymer having a (meth)acryloyl group. When the horizontal alignment film has a polymerizable group similar to or the same as the polymerizable liquid crystal compound constituting the horizontal alignment liquid crystal cured film, there is a tendency that the adhesion between the horizontal alignment film and the horizontal alignment liquid crystal cured film is further improved, so it is preferred that the horizontal alignment film is formed of a polymer having a (meth)acryloyl group, and the horizontal alignment liquid crystal cured film is formed of a polymerizable liquid crystal composition containing a polymerizable liquid crystal compound having a (meth)acryloyl group.
[0357] The photo-alignment film can be generally obtained by applying a composition containing a polymer or monomer having a photoreactive group and a solvent (hereinafter also referred to as a "photo-alignment film-forming composition") to a substrate, removing the solvent, and then irradiating the substrate with polarized light (preferably polarized UV light). The photo-alignment film is advantageous in that the direction of the orientation control force can be arbitrarily controlled by selecting the polarization direction of the irradiated polarized light.
[0358] The so-called photoreactive group refers to a group that generates liquid crystal orientation ability by light irradiation. Specifically, groups that participate in the photoreaction of the orientation induction or isomerization reaction, dimerization reaction, photocrosslinking reaction or photodecomposition reaction of molecules that occur by light irradiation, which become the source of liquid crystal orientation ability, can be cited. Among them, the group participating in the dimerization reaction or the photocrosslinking reaction is preferred from the aspect of excellent orientation. As a photoreactive group, it is preferably a group having an unsaturated bond, especially a double bond, and it is particularly preferred to have at least one group selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond) and a carbon-oxygen double bond (C=O bond).
[0359] As photoreactive groups having C=C bonds, vinyl, polyene, stilbene, stilbazole, stilbazolium, chalcone, and cinnamoyl groups can be cited. As photoreactive groups having C=N bonds, groups having structures such as aromatic Schiff bases and aromatic hydrazones can be cited. As photoreactive groups having N=N bonds, azophenyl, azonaphthyl, aromatic heterocyclic azo, bisazo, formazan, and groups having an oxidized azobenzene structure can be cited. As photoreactive groups having C=O bonds, benzophenone, coumarin, anthraquinone, and maleimide groups can be cited. These groups can have substituents such as alkyl, alkoxy, aryl, allyloxy, cyano, alkoxycarbonyl, hydroxyl, sulfonic acid, and halogenated alkyl.
[0360] Among them, photoreactive groups that participate in the photodimerization reaction are preferred, and azo, cinnamoyl and chalcone groups are preferred from the viewpoint that the amount of polarized light irradiation required for photo-alignment is small and a photo-alignment film with excellent thermal stability and temporal stability can be easily obtained. As the polymer having a photoreactive group, a polymer having an azo or cinnamoyl group is preferred, and from the viewpoint of improving the adhesion between the horizontal alignment film and the horizontal alignment liquid crystal cured film, a polymer having a cinnamoyl group such that the terminal of the polymer side chain is a cinnamic acid structure is particularly preferred.
[0361] By applying the photo-alignment film-forming composition on a substrate, a photo-alignment inducing layer can be formed on the substrate. The solvent contained in the composition may be the same solvent as the solvent previously exemplified as a solvent that can be used in the polymerizable liquid crystal composition, and may be appropriately selected according to the solubility of the polymer or monomer having a photoreactive group.
[0362] The content of the polymer or monomer having a photoreactive group in the composition for forming a photo-alignment film can be appropriately adjusted according to the type of the polymer or monomer and the thickness of the target photo-alignment film, and is preferably set to at least 0.2% by mass, more preferably in the range of 0.3 to 10% by mass, relative to the mass of the composition for forming a photo-alignment film. The composition for forming a photo-alignment film may also contain a polymer material such as polyvinyl alcohol and polyimide, and a photosensitizer within a range that does not significantly impair the properties of the photo-alignment film.
[0363] As a method for applying the photo-alignment film-forming composition to a substrate, the same method as the method for applying the oriented polymer composition to a substrate can be cited. As a method for removing the solvent from the applied photo-alignment film-forming composition, for example, natural drying, ventilation drying, heating drying, and reduced pressure drying can be cited.
[0364] When irradiating polarized light, it can be a method of directly irradiating polarized UV light to the product obtained after removing the solvent from the composition for forming a photo-alignment film applied on the substrate, or it can be a method of irradiating polarized light from the substrate side and transmitting the polarized light. In addition, it is particularly preferred that the polarized light is substantially parallel light. The wavelength of the irradiated polarized light is preferably a wavelength in the wavelength region where the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) in the range of 250 to 400 nm is particularly preferred. As the light source used in the polarized light irradiation, xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, ultraviolet lasers such as KrF and ArF can be cited, and high-pressure mercury lamps, ultra-high-pressure mercury lamps and metal halide lamps are more preferred. Among them, high-pressure mercury lamps, ultra-high-pressure mercury lamps and metal halide lamps are preferred because of the large luminous intensity of ultraviolet rays with a wavelength of 313 nm. Polarized UV light can be irradiated by passing light from the aforementioned light source through an appropriate polarizer. As the polarizer, a polarizing filter, a polarizing prism such as Glan-Thompson or Glan-Taylor, or a wire grid type polarizer can be used.
[0365] It should be noted that, by shielding during rubbing or polarized light irradiation, a plurality of regions (patterns) in which the directions of liquid crystal alignment are different can be formed.
[0366] The groove oriented film is a film having a concavo-convex pattern or multiple grooves (grooves) on the film surface. When a polymerizable liquid crystal compound is applied to a film having multiple linear grooves arranged at equal intervals, the liquid crystal molecules will be oriented in the direction along the grooves.
[0367] As methods for obtaining a grooved oriented film, there are: a method of exposing the surface of a photosensitive polyimide film through an exposure mask having a slit in a pattern shape, and then developing and rinsing to form a concave-convex pattern; a method of forming a layer of a UV-curable resin before curing on a plate-like original plate having grooves on its surface, transferring the formed resin layer to a substrate, and then curing it; and a method of pressing a roll-shaped original plate having a plurality of grooves against a film of a UV-curable resin before curing formed on a substrate to form convex-concave and concave, and then curing it; and the like.
[0368] The thickness of the alignment film (alignment film or photoalignment film containing an aligning polymer) is usually 100 to 5000 nm, preferably 100 to 1000 nm, more preferably 100 to 500 nm, further preferably 100 to 300 nm, and particularly preferably 100 to 250 nm. When the thickness of the alignment film is within the above range, the alignment film has sufficient horizontal alignment control power, and cohesive failure is not likely to occur at the alignment film in the laminate.
[0369] When the optically anisotropic layer Y in the laminate of the present invention is formed of a vertically aligned liquid crystal cured film, the laminate having the optically anisotropic layer Y directly on the optically anisotropic layer X can be produced by, for example, a method including the following steps in the vertically aligned liquid crystal cured film forming step:
[0370] A step of applying a polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film onto a stretched film (optically anisotropic layer X) to obtain a coating film;
[0371] A step of drying the coating to form a dried coating; and
[0372] A step of irradiating the dried coating film with active energy rays to form a vertically aligned liquid crystal cured film.
[0373] The formation of the coating film of the polymerizable liquid crystal composition can be carried out, for example, by coating the polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film on a stretched film. As a coating method of the polymerizable liquid crystal composition, the same method as that used in the method for producing a horizontally aligned liquid crystal cured film can be cited.
[0374] The vertically aligned liquid crystal cured film can be produced by, for example, a method including the following steps in the vertically aligned liquid crystal cured film forming step, wherein the laminate having the optically anisotropic layer Y directly on the optically anisotropic layer X can be produced:
[0375] A step of applying a polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film onto the horizontally aligned liquid crystal cured film to obtain a coating film;
[0376] A step of drying the coating to form a dried coating; and
[0377] A step of irradiating the dried coating film with active energy rays to form a vertically aligned liquid crystal cured film.
[0378] The formation of the coating film of the polymerizable liquid crystal composition can be carried out, for example, by coating the polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film on the horizontally aligned liquid crystal cured film. As a coating method of the polymerizable liquid crystal composition, the same method as that used in the method for manufacturing the horizontally aligned liquid crystal cured film can be cited.
[0379] In addition, the formation of the coating of the polymerizable liquid crystal composition can be carried out, for example, by applying a polymerizable liquid crystal composition for forming a vertically oriented liquid crystal cured film on the above-mentioned substrate. As a substrate, a substrate exemplified in the method for manufacturing a horizontally oriented liquid crystal cured film can be used. In addition, when the substrate is configured in the laminate of the present invention, from the viewpoint of optical compensation described later, the substrate is preferably optically isotropic. In the present invention, optical isotropy refers to an in-plane phase difference value of the substrate of less than 3nm.
[0380] As for the laminate of the present invention, as long as the effect of the present invention is not affected, the horizontally aligned liquid crystal cured film and the vertically aligned liquid crystal cured film can be laminated via other layers. As such other layers, for example, a pressure-sensitive adhesive layer can be cited. When the laminate of the present invention includes a pressure-sensitive adhesive layer, the thickness of the pressure-sensitive adhesive layer is preferably 0.1 to 30 μm, more preferably 0.5 to 20 μm.
[0381] Examples of the adhesive layer include pressure-sensitive adhesives and energy-ray curing adhesives, and acrylic adhesives, epoxy adhesives, and urethane adhesives are preferred because of their high transparency and excellent heat resistance.
[0382] In addition, the laminate of the present invention may include a cured resin layer, a hard coating layer, etc. for the purpose of improving or enhancing the mechanical strength of the liquid crystal curing film as the above-mentioned other layer. When the laminate of the present invention includes such other layers between the horizontally aligned liquid crystal curing film and the vertically aligned liquid crystal curing film, the thickness of the above-mentioned other layers is preferably 0.1 to 4 μm, and more preferably 0.5 to 3 μm. When the laminate of the present invention includes such other layers between the horizontally aligned liquid crystal curing film and the vertically aligned liquid crystal curing film, the other layers can be formed after the horizontally aligned liquid crystal curing film is formed, and then a coating film of a polymerizable liquid crystal composition for forming a vertically aligned liquid crystal curing film is formed on the above-mentioned other layers.
[0383] The above-mentioned cured resin layer can be formed of, for example, acrylic resin, methacrylic resin, epoxy resin, oxetane resin, polyurethane resin, melamine resin, etc. By providing the cured resin layer, even if the liquid crystal cured film formed adjacent to the cured resin layer is a thin film, the cured resin layer can fully compensate for the strength of the liquid crystal cured film as a protective layer or a reinforcing layer.
[0384] After forming the coating of polymerizable liquid crystal composition, the solvent is removed by drying, etc., thereby forming a dry coating. As a drying method, natural drying method, ventilation drying method, heating drying and reduced pressure drying method, etc. can be cited. From the aspect of productivity, it is preferably heated and dried, and for the heating temperature in this case, the solvent can be preferably removed, and it is above the phase transition temperature of the polymerizable liquid crystal compound. About the steps and conditions in the process, the steps and conditions that can be adopted in the manufacture method of the horizontally oriented liquid crystal cured film can be cited.
[0385] The obtained dried coating film is irradiated with active energy rays (more specifically, ultraviolet rays, etc.), and the polymerizable liquid crystal compound is polymerized while maintaining the state of being oriented in a vertical direction relative to the coating film plane, thereby forming a vertically oriented liquid crystal cured film. As a polymerization method, the same method as that used in the method for producing a horizontally oriented liquid crystal cured film can be cited.
[0386] The laminate of the present invention may be a laminate in which the optically anisotropic layer X is arranged on the optically anisotropic layer Y.
[0387] The laminated body in which the optically anisotropic layer X is arranged on the optically anisotropic layer Y can be produced by the following method, which sequentially comprises:
[0388] A step of applying a polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film to a substrate to obtain a coating film;
[0389] A step of drying the coating to form a dried coating;
[0390] The step of irradiating the dried coating film with active energy rays to form a vertically aligned liquid crystal cured film;
[0391] A step of applying a polymerizable liquid crystal composition for forming a horizontally aligned liquid crystal cured film on the vertically aligned liquid crystal cured film to obtain a coating film;
[0392] A step of drying the coating to form a dried coating; and
[0393] A step of irradiating the dried coating film with active energy rays to form a horizontally aligned liquid crystal cured film.
[0394] In the laminate of the present invention, when the optically anisotropic layer X is formed on the optically anisotropic layer Y, it is preferred that a step of forming a horizontal alignment film by a horizontal alignment film forming step is included before forming a horizontal alignment liquid crystal cured film. Here, the horizontal alignment film forming step can be the same step as the method exemplified in the above-mentioned horizontal alignment liquid crystal cured film forming step.
[0395] 〔Polarizing plate〕
[0396] The present invention includes a polarizing plate including the laminate of the present invention and a polarizing film.
[0397] The polarizing film is a film having a polarizing function, and examples thereof include a stretched film adsorbed with a dye having absorption anisotropy, a film coated with a dye having absorption anisotropy as a polarizer, etc. As the dye having absorption anisotropy, for example, a dichroic dye can be mentioned.
[0398] For a film that includes a stretched film adsorbed with a dye having absorption anisotropy as a polarizer, it is usually produced by clamping a transparent protective film on at least one side of the following polarizer via an adhesive, and the polarizer is manufactured through the following steps: a step of uniaxially stretching a polyvinyl alcohol resin film; a step of dyeing the polyvinyl alcohol resin film with a dichroic dye so that it adsorbs the dichroic dye; a step of treating the polyvinyl alcohol resin film adsorbed with the dichroic dye with an aqueous boric acid solution; and a step of washing with water after the treatment with the aqueous boric acid solution.
[0399] The polyvinyl alcohol resin is obtained by saponifying a polyvinyl acetate resin. As the polyvinyl acetate resin, in addition to polyvinyl acetate which is a homopolymer of vinyl acetate, copolymers of vinyl acetate and other monomers copolymerizable therewith can be used. Examples of other monomers copolymerizable with vinyl acetate include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfonic acids, and acrylamides having an ammonium group.
[0400] The saponification degree of the polyvinyl alcohol resin is usually about 85 to 100 mol%, preferably 98 mol% or more. The polyvinyl alcohol resin may be modified, for example, polyvinyl formal or polyvinyl acetal modified with aldehydes may be used. The degree of polymerization of the polyvinyl alcohol resin is usually about 1,000 to 10,000, preferably in the range of 1,500 to 5,000.
[0401] The film made of such a polyvinyl alcohol resin can be used as a raw film of a polarizing film. The method of making a polyvinyl alcohol resin into a film is not particularly limited, and the film can be made by a known method. The film thickness of the polyvinyl alcohol raw film can be, for example, about 10 to 150 μm.
[0402] The uniaxial stretching of the polyvinyl alcohol resin film can be performed before, at the same time as, or after dyeing based on a dichroic pigment. In the case of uniaxial stretching after dyeing, the uniaxial stretching can be performed before or during the boric acid treatment. In addition, the uniaxial stretching can be performed in multiple stages thereof. When the uniaxial stretching is performed, the uniaxial stretching can be performed between rollers having different peripheral speeds, or the uniaxial stretching can be performed using a hot roller. In addition, the uniaxial stretching can be dry stretching performed in the atmosphere, or wet stretching performed in a state where the polyvinyl alcohol resin film is swollen with a solvent. The stretching ratio is usually about 3 to 8 times.
[0403] The polyvinyl alcohol-based resin film can be dyed with a dichroic dye by, for example, a method of immersing the polyvinyl alcohol-based resin film in an aqueous solution containing a dichroic dye.
[0404] As the dichroic pigment, specifically, iodine and dichroic organic dyes can be used. As the dichroic organic dyes, dichroic direct dyes formed by disazo compounds such as CI Direct Red (DIRECT RED) 39, and dichroic direct dyes formed by compounds such as triazo and tetrakis azo can be cited. For the polyvinyl alcohol-based resin film, it is preferably immersed in water before dyeing.
[0405] When iodine is used as a dichroic pigment, a method of dyeing a polyvinyl alcohol-based resin film by immersing it in an aqueous solution containing iodine and potassium iodide can generally be adopted. The content of iodine in the aqueous solution is generally about 0.01 to 1 part by mass relative to 100 parts by mass of water. In addition, the content of potassium iodide is generally about 0.5 to 20 parts by mass relative to 100 parts by mass of water. The temperature of the aqueous solution used for dyeing is generally about 20 to 40°C. In addition, the immersion time (dyeing time) in the aqueous solution is generally about 20 to 1,800 seconds.
[0406] On the other hand, when a dichroic organic dye is used as the dichroic pigment, a method of dyeing the polyvinyl alcohol-based resin film by immersing the film in an aqueous solution containing a water-soluble dichroic dye can be generally adopted. The content of the dichroic organic dye in the aqueous solution is generally 1×10 -4 ~10 parts by mass, preferably 1×10 -3 ~1 mass part, more preferably 1×10 -3 ~1×10 -2 The aqueous solution may contain an inorganic salt such as sodium sulfate as a dyeing auxiliary. The temperature of the dichroic dye aqueous solution used for dyeing is usually about 20 to 80° C. In addition, the immersion time (dyeing time) in the aqueous solution is usually about 10 to 1,800 seconds.
[0407] Boric acid treatment after dyeing based on dichroic pigments can usually be carried out by immersing the dyed polyvinyl alcohol-based resin film in an aqueous solution of boric acid. The content of boric acid in the aqueous solution of boric acid is usually about 2 to 15 parts by mass, preferably 5 to 12 parts by mass, relative to 100 parts by mass of water. When iodine is used as a dichroic pigment, the aqueous solution of boric acid preferably contains potassium iodide, and the content of potassium iodide at this time is usually about 0.1 to 15 parts by mass, preferably 5 to 12 parts by mass, relative to 100 parts by mass of water. The immersion time in the aqueous solution of boric acid is usually about 60 to 1,200 seconds, preferably 150 to 600 seconds, and more preferably 200 to 400 seconds. The temperature of the boric acid treatment is usually above 50°C, preferably 50 to 85°C, and more preferably 60 to 80°C.
[0408] Generally, the polyvinyl alcohol-based resin film treated with boric acid can be subjected to a water washing treatment. The water washing treatment can be performed, for example, by immersing the polyvinyl alcohol-based resin film treated with boric acid in water. The temperature of water in the water washing treatment is generally about 5 to 40° C. In addition, the immersion time is generally about 1 to 120 seconds.
[0409] A drying treatment can be performed after washing to obtain a polarizer. The drying treatment can be performed, for example, using a hot air dryer or a far-infrared heater. The temperature of the drying treatment is usually about 30 to 100°C, preferably 50 to 80°C. The time of the drying treatment is usually about 60 to 600 seconds, preferably 120 to 600 seconds. By drying, the moisture content of the polarizer can be reduced to a practical level. The moisture content is usually about 5 to 20% by mass, preferably 8 to 15% by mass. When the moisture content is less than 5% by mass, the flexibility of the polarizer is lost, and the polarizer is sometimes damaged or broken after it is dried. In addition, when the moisture content is higher than 20% by mass, there is a possibility that the thermal stability of the polarizer will deteriorate.
[0410] The thickness of the polarizer obtained by uniaxially stretching the polyvinyl alcohol-based resin film, dyeing it with a dichroic dye, treating it with boric acid, washing it with water, and drying it as described above is preferably 5 to 40 μm.
[0411] As a film formed by coating a pigment having absorption anisotropy, a film obtained by coating a composition containing a dichroic pigment having liquid crystal properties or a composition containing a dichroic pigment and polymerizable liquid crystal, etc. can be cited. The film preferably has a protective film on one or both sides. As the protective film, a film identical to the resin film exemplified in the above text as a base material that can be used in the manufacture of a horizontally oriented liquid crystal cured film can be cited.
[0412] The film formed by coating the dye having absorption anisotropy is preferably as thin as possible, but if it is too thin, the strength decreases and the processability tends to be poor. The thickness of the film is usually 20 μm or less, preferably 5 μm or less, and more preferably 0.5 to 3 μm.
[0413] Specific examples of the film formed by coating a dye having absorption anisotropy include films described in JP-A-2012-33249 and the like.
[0414] A transparent protective film may be laminated on at least one side of the polarizer obtained as described above via, for example, an adhesive layer. As the transparent protective film, the same transparent film as the resin film exemplified above as a base material that can be used in the production of a liquid crystal cured film can be used.
[0415] The polarizing plate of the present invention comprises the laminate of the present invention and a polarizing film, and can be obtained by laminating the laminate of the present invention and the polarizing film with an adhesive layer or the like interposed therebetween, for example.
[0416] In one embodiment of the present invention, when the laminate of the present invention is laminated with a polarizing film, Figure 2 As an example, a polarizing film 3, an optical anisotropic layer X ( Figure 2 layer 1 in the embodiment of the present invention), and an optically anisotropic layer Y ( Figure 2 In this case, the polarizing plate of the present invention can be obtained by laminating the laminated body including the optically anisotropic layer X and the optically anisotropic layer Y to the polarizing film 3 via an adhesive layer. In the present invention, when the polarizing film, the optically anisotropic layer X, and the optically anisotropic layer Y are laminated in sequence, it is preferred that the laminated body is laminated in such a manner that the angle formed by the slow axis (optical axis) of the optically anisotropic layer X constituting the laminated body and the absorption axis of the polarizing film becomes 90±5°.
[0417] In one embodiment of the present invention, when the laminate of the present invention is laminated with a polarizing film, Figure 3As an example, a polarizing film 3, an optical anisotropic layer Y ( Figure 3 layer 2 in the embodiment), and an optically anisotropic layer X ( Figure 3 In this case, the polarizing plate of the present invention can be obtained by laminating the laminated body including the optically anisotropic layer Y and the optically anisotropic layer X to the polarizing film 3 via an adhesive layer. In the present invention, when the polarizing film, the optically anisotropic layer Y, and the optically anisotropic layer X are laminated in sequence, it is preferred that the laminated body is laminated in such a way that the angle formed by the slow axis (optical axis) of the optically anisotropic layer X constituting the laminated body and the absorption axis of the polarizing film becomes 0±5°.
[0418] As the adhesive layer for bonding the polarizing film and the optically anisotropic layer X or the optically anisotropic layer Y, the same layer as exemplified as the other layer for bonding the horizontally aligned liquid crystal cured film and the vertically aligned liquid crystal cured film can be used.
[0419] The polarizing plate of the present invention may have a structure as that of a conventional polarizing plate, or a polarizing film and a phase difference film. Such a structure may include, for example, an adhesive layer (sheet) for attaching the polarizing plate to a display element such as a liquid crystal display device, a protective film used to protect the surface of the polarizing film and the liquid crystal curing film from damage or contamination, and the like.
[0420] The laminate and polarizing plate of the present invention can be used in various display devices.
[0421] The so-called display device is a device having a display element, including a light-emitting element or a light-emitting device as a light source. As the display device, there can be cited a liquid crystal display device, an organic electroluminescent (EL) display device, an inorganic electroluminescent (EL) display device, a touch panel display device, an electron emission display device (such as a field emission display device (FED), a surface field emission display device (SED)), an electronic paper (a display device using electronic ink, an electrophoretic element, a plasma display device, a projection type display device (such as a grating light valve (GLV) display device, a display device with a digital micromirror device (DMD)) and a piezoelectric ceramic display, etc. The liquid crystal display device includes any one of a transmissive liquid crystal display device, a semi-transmissive liquid crystal display device, a reflective liquid crystal display device, a direct-view liquid crystal display device and a projection type liquid crystal display device. In particular, with respect to the laminate and the polarizing plate of the present invention, from the aspect of being easy to significantly exert their effects, they can be suitably used in liquid crystal display devices, and are particularly preferably used as IPS (in-plane By using the laminate or polarizing plate of the present invention, it is easy to realize a thinner display device, and a display device that can exhibit the following characteristics can be obtained, which is a characteristic of preventing light leakage and color shift when the liquid crystal display device is visually recognized from an oblique direction when black is displayed.
[0422] Example
[0423] Hereinafter, the present invention will be described in more detail using Examples. It should be noted that, unless otherwise specified, "%" and "parts" in the examples refer to mass % and mass parts, respectively.
[0424] 1. Example 1
[0425] (1) Preparation of Composition for Forming Horizontal Alignment Film
[0426] 5 parts by mass of a photo-alignment material having the following structure (weight average molecular weight: 30,000) and 95 parts by mass of cyclopentanone (solvent) were mixed as components, and the obtained mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a horizontal alignment film.
[0427] [Chemical formula 17]
[0428]
[0429] (2) Preparation of polymerizable liquid crystal compounds
[0430] A polymerizable liquid crystal compound (X1) having the following molecular structure was produced by the method described in Japanese Unexamined Patent Publication No. 2010-31223: In addition, a polymerizable liquid crystal compound (III-1) having k2=4 (III-1-4) was produced by the method described in Japanese Unexamined Patent Publication No. 2010-270108.
[0431] Polymerizable liquid crystal compound (X1)
[0432] [Chemical formula 18]
[0433]
[0434] (3) Preparation of polymerizable liquid crystal composition (1) for forming a horizontally aligned liquid crystal cured film
[0435] The polymerizable liquid crystal compound (X1) and the polymerizable liquid crystal compound LC242 represented by the following formula (LC242): Paliocolor LC242 (registered trademark of BASF) are mixed in a mass ratio of 65:35 to obtain a mixture. 0.1 mass parts of the leveling agent "BYK-361N" (manufactured by BM Chemie) and 6 mass parts of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)-1-butanone ("Irgacure (registered trademark) 369 (Irg369)" manufactured by BASF JAPAN Co., Ltd.) as a photopolymerization initiator are added to 100 mass parts of the obtained mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) is added in such a way that the solid content concentration becomes 10%. The mixture is stirred at 80°C for 1 hour to obtain a polymerizable liquid crystal composition (1) for forming a horizontally aligned liquid crystal cured film.
[0436] LC242: Paliocolor LC242 (registered trademark of BASF)
[0437] [Chemical formula 19]
[0438]
[0439] (4) Formation of horizontally aligned liquid crystal cured film
[0440] After corona treatment, a COP film (ZF14-50) manufactured by Zeon Co., Ltd. was coated with a horizontal alignment film-forming composition using a bar coater, dried at 80°C for 1 minute, and then irradiated with a polarized UV light device (SPOT CURE SP-9; manufactured by Ushio Electric Co., Ltd.) at a wavelength of 313 nm with a cumulative light intensity of 100 mJ / cm 2Polarized UV light exposure was performed under the conditions of to obtain a horizontal alignment film. The film thickness of the obtained horizontal alignment film was measured by an ellipsometer and the result was 200 nm.
[0441] Next, the polymerizable liquid crystal composition (1) for forming a horizontally aligned liquid crystal cured film was applied onto the horizontally aligned film, and after heating at 120° C. for 60 seconds, ultraviolet rays (in a nitrogen atmosphere, the accumulated light amount at a wavelength of 365 nm: 500 mJ / cm ) were irradiated from the surface coated with the polymerizable liquid crystal composition (1) for forming a horizontally aligned liquid crystal cured film using a high-pressure mercury lamp (Unicure VB-15201BY-A, manufactured by Ushio Electric Co., Ltd.). 2 ), thereby forming an optically anisotropic layer X composed of a horizontally aligned liquid crystal cured film. The film thickness of the obtained horizontally aligned liquid crystal cured film was measured with an ellipsometer and found to be 1.4 μm.
[0442] <Measurement of Phase Difference of Horizontally Aligned Liquid Crystal Cured Film>
[0443] The horizontally oriented liquid crystal cured film surface of the laminate composed of the substrate, the horizontally oriented film, and the horizontally oriented liquid crystal cured film was subjected to corona treatment, and was bonded to glass via a 25 μm pressure-sensitive adhesive manufactured by Lintec. Then, for the laminate composed of glass, adhesive, horizontally oriented liquid crystal cured film, horizontally oriented film, and substrate, after confirming in advance that there was no phase difference in the substrate, KOBRA-WPR manufactured by Oji Instruments Co., Ltd. was used to measure Re (450) and Re (550) of the horizontally oriented liquid crystal cured film, and A = Re (450) / Re (550) was calculated. The results are shown in Table 1.
[0444] (5) Preparation of polymerizable liquid crystal composition (1) for forming a vertically aligned liquid crystal cured film
[0445] The polymerizable liquid crystal compound (X1) and the polymerizable liquid crystal compound LC242: Paliocolor LC242 (registered trademark of BASF) were mixed at a mass ratio of 70:30 to obtain a mixture. 0.25 mass parts of a leveling agent "F-556" (manufactured by DIC Corporation), 1.5 mass parts of an ionic compound A (molecular weight: 645) prepared with reference to Japanese Patent Application No. 2016-514802, 0.5 mass parts of a silane coupling agent "KBE-9103" (manufactured by Shin-Etsu Chemical Co., Ltd.), and 6 mass parts of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)-1-butanone (manufactured by BASF JAPAN Co., Ltd. "Irgacure (registered trademark) 369 (Irg369)") as a photopolymerization initiator were added to 100 mass parts of the obtained mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) was added in such a way that the solid content concentration became 13%. The mixture was stirred at 80° C. for 1 hour to obtain a polymerizable liquid crystal composition (1) for forming a vertically aligned liquid crystal cured film.
[0446] Ionic compound A:
[0447] [Chemical formula 20]
[0448]
[0449] (6) Formation of vertically aligned liquid crystal cured film
[0450] The horizontally aligned liquid crystal cured film of the laminate formed of the substrate, the horizontally aligned film and the horizontally aligned liquid crystal cured film prepared as described above was subjected to corona treatment, and then the polymerizable liquid crystal composition (1) for forming the vertically aligned liquid crystal cured film was applied using a bar coater and heated at 120° C. for 60 seconds. Next, while the temperature was kept at 120° C., a high pressure mercury lamp (Unicure VB-15201BY-A, manufactured by Ushio Electric Co., Ltd.) was used to irradiate the surface coated with the polymerizable liquid crystal composition (1) with ultraviolet rays (in a nitrogen atmosphere, the accumulated light amount at a wavelength of 365 nm: 500 mJ / cm 2 ), thereby forming an optically anisotropic layer Y formed of a vertically oriented liquid crystal cured film, and obtaining a laminated body in which a substrate, a horizontally oriented film, a horizontally oriented liquid crystal cured film, and a vertically oriented liquid crystal cured film are sequentially stacked adjacent to each other. The film thickness of the obtained vertically oriented liquid crystal cured film was measured with an ellipsometer (M-220 manufactured by JASCO Corporation), and the result was 1.0 μm.
[0451] <Measurement of Phase Difference of Vertically Aligned Liquid Crystal Cured Film>
[0452] The corona treatment was performed on the surface of the vertically aligned liquid crystal cured film of the laminate formed by the substrate, the horizontally aligned film, the horizontally aligned liquid crystal cured film, and the vertically aligned liquid crystal cured film produced through the above steps, and it was adhered to the glass through the 25 μm pressure-sensitive adhesive manufactured by Lintec Corporation. For the obtained laminate, after confirming in advance that there is no retardation in the substrate, using the KOBRA-WPR manufactured by Oji Keisoku K.K., the in-plane retardation value of the laminate including the vertically aligned liquid crystal cured film and the horizontally aligned liquid crystal cured film, and the retardation value when tilted 50° around the fast axis were measured by changing the incident angle of the sample for measuring the optical properties with respect to the light direction. In addition, the in-plane retardation value of the laminate formed by the glass, the adhesive, the horizontally aligned liquid crystal cured film, the horizontally aligned film, and the substrate, and the retardation value when tilted 50° around the fast axis were measured by the same method.
[0453] Next, for the above-mentioned vertically aligned liquid crystal cured film and horizontally aligned liquid crystal cured film, the average refractive index at each wavelength was measured respectively using the ellipsometer M-220 manufactured by JASCO Corporation. In addition, the film thickness was measured using the Optical Nano Gauge film thickness meter C12562-01 manufactured by Hamamatsu Photonics K.K. Based on the above in-plane retardation value, the retardation value when tilted 50° around the fast axis, the average refractive index, and the film thickness value, the three-dimensional refractive index was calculated with reference to the technical data of Oji Keisoku K.K. (http: / / www.oji-keisoku.co.jp / products / kobra / reference.html). Based on the obtained three-dimensional refractive index, the optical properties of the laminate including the vertically aligned liquid crystal cured film and the horizontally aligned liquid crystal cured film, and the horizontally aligned liquid crystal cured film were calculated according to the following formula, and the values of Rth(450) and Rth(550) of the vertically aligned liquid crystal cured film were calculated from the difference between the respective values, and B = Rth(450) / Rth(550) was calculated. The results are shown in Table 1.
[0454] (7) Evaluation of the laminate
[0455] <Confirmation of black display>
[0456] An adhesive layer and a polarizing film were sequentially laminated on the surface on the substrate side of the laminate manufactured in Example 1 to form a polarizing plate. At this time, the laminate was performed such that the angle formed by the absorption axis of the polarizing film and the slow axis of the optically anisotropic layer X of the laminate was 90 degrees. The obtained polarizing plate was adhered to the visual recognition side of the i-Pad (registered trademark) (manufactured by Apple Inc.) from which the visual recognition side polarizing plate was removed with the polarizing film as the outermost surface, and the light leakage during black display was visually confirmed from the direction with an azimuth angle of 45° and an elevation angle of 45° with respect to the panel surface, and the color bleeding (Japanese: 色抜け) was judged according to the following criteria. The results are shown in Table 1.
[0457] Evaluation criteria:
[0458] A: There is almost no coloring when viewed from an oblique direction.
[0459] B: Slight coloring was observed when visually observed from an oblique direction.
[0460] C: Intense coloring was observed when visually observed from an oblique direction.
[0461] <Confirmation of heat resistance>
[0462] The substrate and the horizontal alignment film were peeled off from the laminated body composed of the substrate, the horizontal alignment film, the horizontal alignment liquid crystal cured film, and the vertical alignment liquid crystal cured film manufactured in Example 1, thereby obtaining a laminated body composed of the horizontal alignment liquid crystal cured film and the vertical alignment liquid crystal cured film. The laminated body after the substrate was peeled off was placed in an oven at 100° C. and left to stand for 30 minutes, and it was confirmed that the laminated body after the substrate was peeled off was not deformed by heat.
[0463] 2. Example 2
[0464] Except that the preparation of the polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film and the formation of the vertically aligned liquid crystal cured film are changed as follows, the same operation as in Example 1 is performed to prepare a laminated body in which a substrate, a horizontally aligned film, a horizontally aligned liquid crystal cured film, and a vertically aligned liquid crystal cured film are stacked adjacent to each other in sequence. In addition, the same operation as in Example 1 is performed to prepare a polarizing plate by attaching a polarizing film to the surface on the substrate side, and the visual recognition during black display is confirmed. The results are shown in Table 1.
[0465] (1) Preparation of polymerizable liquid crystal composition for forming vertically aligned liquid crystal cured film (2)
[0466] The polymerizable liquid crystal compound (X1) and the polymerizable liquid crystal compound LC242: Paliocolor LC242 (registered trademark of BASF) were mixed at a mass ratio of 50:50 to obtain a mixture. 0.25 mass parts of a leveling agent "F-556" (manufactured by DIC Corporation), 1.5 mass parts of an ionic compound A (molecular weight: 645) prepared with reference to Japanese Patent Application No. 2016-514802, 0.5 mass parts of a silane coupling agent "KBE-9103" (manufactured by Shin-Etsu Chemical Co., Ltd.), and 6 mass parts of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)-1-butanone (manufactured by BASF JAPAN Co., Ltd. "Irgacure (registered trademark) 369 (Irg369)") as a photopolymerization initiator were added to 100 mass parts of the obtained mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) was added in such a way that the solid content concentration became 13%. The mixture was stirred at 80° C. for 1 hour to obtain a polymerizable liquid crystal composition (2) for forming a vertically aligned liquid crystal cured film.
[0467] (2) Preparation of vertically oriented liquid crystal cured film
[0468] After corona treatment was applied to the horizontally aligned liquid crystal cured film surface of the laminate composed of a substrate, a horizontally aligned film, and a horizontally aligned liquid crystal cured film prepared in the same manner as in Example 1, a polymerizable liquid crystal composition (2) for forming a vertically aligned liquid crystal cured film was applied using a bar coater and heated at 120° C. for 60 seconds. Next, a high-pressure mercury lamp (Unicure VB-15201BY-A, manufactured by Ushio Electric Co., Ltd.) was used to irradiate ultraviolet rays (under a nitrogen atmosphere, the cumulative light amount at a wavelength of 365 nm: 500 mJ / cm 2 ), thereby forming an optically anisotropic layer Y composed of a vertically oriented liquid crystal cured film. The film thickness of the obtained vertically oriented liquid crystal cured film was measured by an ellipsometer (M-220 manufactured by JASCO Corporation), and the result was 1.4 μm. It should be noted that the substrate and the horizontally oriented film were peeled off from the laminated body formed by the substrate, the horizontally oriented film, the horizontally oriented liquid crystal cured film, and the vertically oriented liquid crystal cured film, and the laminated body formed by the horizontally oriented liquid crystal cured film and the vertically oriented liquid crystal cured film after the substrate was peeled off was placed in an oven at 100°C and left to stand for 30 minutes. As a result, it was confirmed that the laminated body after the substrate was peeled off was not deformed by heat.
[0469] 3. Example 3
[0470] Except that the preparation of the polymerizable liquid crystal composition for forming the horizontal alignment liquid crystal cured film and the formation of the horizontal alignment liquid crystal cured film are changed as follows, the same operation as in Example 1 is performed to prepare a laminated body in which a substrate, a horizontal alignment film, a horizontal alignment liquid crystal cured film and a vertical alignment liquid crystal cured film are stacked adjacent to each other in sequence. In addition, the same operation as in Example 1 is performed to prepare a polarizing plate by attaching a polarizing film to the surface on the substrate side, and the visual recognition during black display is confirmed. The results are shown in Table 1.
[0471] (1) Preparation of polymerizable liquid crystal composition for forming a horizontally aligned liquid crystal cured film (2)
[0472] The polymerizable liquid crystal compound (X1) and the polymerizable liquid crystal compound LC242: Paliocolor LC242 (registered trademark of BASF) are mixed in a mass ratio of 50:50 to obtain a mixture. To 100 parts by mass of the obtained mixture, 0.1 parts by mass of a leveling agent "BYK-361N" (manufactured by BM Chemie) and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)-1-butanone ("Irgacure (registered trademark) 369 (Irg369)" manufactured by BASF JAPAN Co., Ltd.) as a photopolymerization initiator are added. Furthermore, N-methyl-2-pyrrolidone (NMP) is added in such a manner that the solid content concentration becomes 13%. The mixture is stirred at 80°C for 1 hour to obtain a polymerizable liquid crystal composition (2) for forming a horizontally aligned liquid crystal cured film.
[0473] (2) Formation of horizontally aligned liquid crystal cured film
[0474] After forming a horizontal alignment film on the substrate in the same manner as in Example 1, a polymerizable liquid crystal composition (2) for forming a horizontal alignment liquid crystal curable film was applied to the horizontal alignment film, and after heating at 120° C. for 60 seconds, a high-pressure mercury lamp (Unicure VB-15201BY-A, manufactured by Ushio Electric Co., Ltd.) was used to irradiate the surface coated with the polymerizable liquid crystal composition (2) with ultraviolet light (cumulative light intensity at a wavelength of 365 nm under a nitrogen atmosphere: 500 mJ / cm 2 ), thereby forming an optically anisotropic layer X composed of a horizontally aligned liquid crystal cured film. The film thickness of the obtained horizontally aligned liquid crystal cured film was measured with an ellipsometer and found to be 1.3 μm.
[0475] On the horizontally oriented liquid crystal cured film of the laminated body formed of the substrate, the horizontally oriented film and the horizontally oriented liquid crystal cured film produced in the above manner, a vertically oriented liquid crystal cured film was formed in the same manner as in Example 1, thereby obtaining a laminated body, and a polarizing film was attached to the surface on the substrate side, thereby obtaining a polarizing plate. It should be noted that the substrate and the horizontally oriented film were peeled off from the laminated body formed of the substrate, the horizontally oriented film, the horizontally oriented liquid crystal cured film and the vertically oriented liquid crystal cured film, and the laminated body formed of the horizontally oriented liquid crystal cured film and the vertically oriented liquid crystal cured film after the substrate was peeled off was placed in an oven at 100° C. and left to stand for 30 minutes. As a result, it was confirmed that the laminated body after the substrate was peeled off was not deformed by heat.
[0476] 4. Example 4
[0477] Using the polymerizable liquid crystal composition (2) for forming a horizontally aligned liquid crystal curing film prepared in Example 3, the same operation as in Example 3 was performed to prepare a laminated body in which a substrate, a horizontally aligned film, and a horizontally aligned liquid crystal curing film with a thickness of 1.4 μm were stacked in sequence. Next, in the same manner as in Example 2, a polymerizable liquid crystal composition (2) for forming a vertically aligned liquid crystal curing film was used to form a vertically aligned liquid crystal curing film with a thickness of 1.4 μm on the above-mentioned horizontally aligned liquid crystal curing film, thereby obtaining a laminated body, and a polarizing film was attached to the surface on the substrate side to prepare a polarizing plate, and the visual recognition during black display was confirmed. The results are shown in Table 1. It should be noted that the substrate and the horizontally aligned film were peeled off from the laminated body formed by the substrate, the horizontally aligned film, the horizontally aligned liquid crystal curing film, and the vertically aligned liquid crystal curing film, and the laminated body after the substrate was peeled off was placed in an oven at 100°C for 30 minutes. As a result, it was confirmed that the laminated body after the substrate was peeled off was not deformed by heat.
[0478] 5. Example 5
[0479] Except that the preparation of the polymerizable liquid crystal composition for forming the vertically aligned liquid crystal cured film and the formation of the vertically aligned liquid crystal cured film are changed as follows, the same operation as in Example 3 is performed to prepare a laminated body in which a substrate, a horizontally aligned film, a horizontally aligned liquid crystal cured film and a vertically aligned liquid crystal cured film are stacked adjacent to each other in sequence. In addition, the same operation as in Example 3 is performed to prepare a polarizing plate by attaching a polarizing film to the surface on the substrate side, and the visual recognition during black display is confirmed. The results are shown in Table 1.
[0480] (1) Preparation of polymerizable liquid crystal composition for forming vertically aligned liquid crystal cured film (3)
[0481] The polymerizable liquid crystal compound (X1) and the polymerizable liquid crystal compound LC242: Paliocolor LC242 (registered trademark of BASF) were mixed at a mass ratio of 30:70 to obtain a mixture. 0.25 mass parts of a leveling agent "F-556" (manufactured by DIC Corporation), 1.5 mass parts of an ionic compound A (molecular weight: 645) prepared with reference to Japanese Patent Application No. 2016-514802, 0.5 mass parts of a silane coupling agent "KBE-9103" (manufactured by Shin-Etsu Chemical Co., Ltd.), and 6 mass parts of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)-1-butanone (manufactured by BASF JAPAN Co., Ltd. "Irgacure (registered trademark) 369 (Irg369)") as a photopolymerization initiator were added to 100 mass parts of the obtained mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration became 13%. The mixture was stirred at 80° C. for 1 hour to obtain a polymerizable liquid crystal composition (3) for forming a vertically aligned liquid crystal cured film.
[0482] (2) Preparation of vertically oriented liquid crystal cured film
[0483] Using the polymerizable liquid crystal composition (2) for forming a horizontally oriented liquid crystal curing film prepared in Example 3, the same operation as in Example 3 was performed to produce a laminated body in which a substrate, a horizontally oriented film, and a horizontally oriented liquid crystal curing film with a thickness of 1.5 μm were stacked adjacent to each other in sequence. Next, after the surface of the horizontally oriented liquid crystal curing film was subjected to corona treatment, a rod coater was used to apply the polymerizable liquid crystal composition (3) for forming a vertically oriented liquid crystal curing film, and heated at 120°C for 60 seconds. Next, a high-pressure mercury lamp (Unicure VB-15201BY-A, manufactured by Ushio Electric Co., Ltd.) was used to irradiate ultraviolet rays from the surface coated with the polymerizable liquid crystal composition (3) for forming a vertically oriented liquid crystal curing film (under a nitrogen atmosphere, the accumulated light amount at a wavelength of 365 nm: 500 mJ / cm 2 ), thereby forming an optically anisotropic layer Y composed of a vertically oriented liquid crystal cured film. The film thickness of the obtained vertically oriented liquid crystal cured film was measured by an ellipsometer (M-220 manufactured by JASCO Corporation), and the result was 1.3 μm. It should be noted that the substrate and the horizontally oriented film were peeled off from the laminated body formed by the substrate, the horizontally oriented film, the horizontally oriented liquid crystal cured film, and the vertically oriented liquid crystal cured film, and the laminated body formed by the horizontally oriented liquid crystal cured film and the vertically oriented liquid crystal cured film after the substrate was peeled off was placed in an oven at 100°C and left to stand for 30 minutes. As a result, it was confirmed that the laminated body after the substrate was peeled off was not deformed by heat.
[0484] 6. Example 6
[0485] Except that the preparation of the polymerizable liquid crystal composition for forming the horizontal alignment liquid crystal cured film and the formation of the horizontal alignment liquid crystal cured film are changed as follows, the same operation as in Example 4 is performed to prepare a laminated body in which a substrate, a horizontal alignment film, a horizontal alignment liquid crystal cured film and a vertical alignment liquid crystal cured film are stacked adjacent to each other in sequence. In addition, the same operation as in Example 4 is performed to prepare a polarizing plate by attaching a polarizing film to the surface on the substrate side, and the visual recognition during black display is confirmed. The results are shown in Table 1.
[0486] (1) Preparation of polymerizable liquid crystal composition (3) for forming a horizontally aligned liquid crystal cured film
[0487] The polymerizable liquid crystal compound (X1) and the polymerizable liquid crystal compound LC242: Paliocolor LC242 (registered trademark of BASF) are mixed in a mass ratio of 30:70 to obtain a mixture. To 100 parts by mass of the obtained mixture, 0.1 parts by mass of a leveling agent "BYK-361N" (manufactured by BM Chemie) and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)-1-butanone ("Irgacure (registered trademark) 369 (Irg369)" manufactured by BASF JAPAN Co., Ltd.) as a photopolymerization initiator are added. Furthermore, N-methyl-2-pyrrolidone (NMP) is added in such a manner that the solid content concentration becomes 13%. The mixture is stirred at 80°C for 1 hour to obtain a polymerizable liquid crystal composition (3) for forming a horizontally aligned liquid crystal cured film.
[0488] (2) Formation of horizontally aligned liquid crystal cured film
[0489] After forming a horizontal alignment film on the substrate in the same manner as in Example 4, a polymerizable liquid crystal composition (3) for forming a horizontal alignment liquid crystal curable film was applied to the horizontal alignment film, and after heating at 120° C. for 60 seconds, a high-pressure mercury lamp (Unicure VB-15201BY-A, manufactured by Ushio Electric Co., Ltd.) was used to irradiate the surface coated with the polymerizable liquid crystal composition (3) with ultraviolet light (cumulative light intensity at a wavelength of 365 nm under a nitrogen atmosphere: 500 mJ / cm 2), thereby forming an optically anisotropic layer X composed of a horizontally oriented liquid crystal cured film. The film thickness of the obtained horizontally oriented liquid crystal cured film was measured with an ellipsometer, and the result was 1.1μm. On the horizontally oriented liquid crystal cured film of the laminate formed by the substrate, the horizontally oriented film and the horizontally oriented liquid crystal cured film prepared in the above manner, the same operation as in Example 4 was performed, and a polymerizable liquid crystal composition (2) for forming a vertically oriented liquid crystal cured film was used to form a vertically oriented liquid crystal cured film with a thickness of 0.9μm, thereby obtaining a laminate, and a polarizing film was attached to the surface on the substrate side, thereby obtaining a polarizing plate. It should be noted that the substrate and the horizontally oriented film were peeled off from the manufactured laminate formed by the substrate, the horizontally oriented film, the horizontally oriented liquid crystal cured film, and the vertically oriented liquid crystal cured film, and the laminate formed by the horizontally oriented liquid crystal cured film and the vertically oriented liquid crystal cured film after the substrate was peeled off was placed in an oven at 100°C and left to stand for 30 minutes. As a result, it was confirmed that the laminate after the substrate was peeled off was not deformed due to heat.
[0490] 7. Example 7
[0491] Using the polymerizable liquid crystal composition (3) for forming a horizontally aligned liquid crystal solidified film prepared in Example 6, the same operation as in Example 6 was performed to prepare a laminated body in which a substrate, a horizontally aligned film, and a horizontally aligned liquid crystal solidified film with a film thickness of 1.2 μm were stacked in sequence. Next, in the same manner as in Example 5, a polymerizable liquid crystal composition (3) for forming a vertically aligned liquid crystal solidified film was applied to the above-mentioned horizontally aligned liquid crystal solidified film to form a vertically aligned liquid crystal solidified film with a film thickness of 1.2 μm, thereby obtaining a laminated body, and a polarizing film was attached to the surface on the substrate side to prepare a polarizing plate, and the visual recognition during black display was confirmed. The results are shown in Table 1. It should be noted that the substrate and the horizontally aligned film were peeled off from the laminated body formed by the substrate, the horizontally aligned film, the horizontally aligned liquid crystal solidified film, and the vertically aligned liquid crystal solidified film, and the laminated body after the substrate was peeled off was placed in an oven at 100°C for 30 minutes. As a result, it was confirmed that the laminated body after the substrate was peeled off was not deformed by heat.
[0492] 8. Example 8
[0493] The same operation as in Example 3 is performed to prepare a laminated body in which a substrate, a horizontally oriented film, a horizontally oriented liquid crystal curing film, and a vertically oriented liquid crystal curing film are stacked adjacent to each other in sequence. Next, an adhesive is used to bond a polarizing film to the surface on the vertically oriented liquid crystal curing film side to form a polarizing plate. At this time, the angle formed by the absorption axis of the polarizing film and the slow axis of the optically anisotropic layer X of the laminate is 0 degrees. The obtained polarizing plate is bonded to the visual recognition side of the i-Pad (registered trademark) (made by Apple Inc.) with the polarizing film being the outermost surface, and the light leakage during the black display is confirmed by visual observation from the direction of 45 ° in azimuth and 45 ° in elevation relative to the panel surface. The results are shown in Table 1.
[0494] 9. Example 9
[0495] The same operation as in Example 4 was performed to prepare a laminated body in which a substrate, a horizontally oriented film, a horizontally oriented liquid crystal curing film, and a vertically oriented liquid crystal curing film were stacked in sequence. Next, a polarizing film was attached to the surface of the vertically oriented liquid crystal curing film using an adhesive to form a polarizing plate. At this time, the angle formed by the absorption axis of the polarizing film and the slow axis of the optically anisotropic layer X of the laminated body was 0 degrees. The visual recognition of the obtained polarizing plate during black display was confirmed in the same manner as in Example 8. The results are shown in Table 1.
[0496] 10. Comparative Example 1
[0497] Except that the preparation of the polymerizable liquid crystal composition for forming the horizontal alignment liquid crystal cured film and the formation of the horizontal alignment liquid crystal cured film are changed as follows, the same operation as in Example 3 is performed to prepare a laminated body in which a substrate, a horizontal alignment film, a horizontal alignment liquid crystal cured film and a vertical alignment liquid crystal cured film are stacked adjacent to each other in sequence. In addition, the same operation as in Example 3 is performed to prepare a polarizing plate by attaching a polarizing film to the surface on the substrate side, and the visual recognition during black display is confirmed. The results are shown in Table 1.
[0498] (1) Preparation of polymerizable liquid crystal composition (4) for forming a horizontally aligned liquid crystal curing film To the polymerizable liquid crystal compound (III-1-4), 0.1 parts by mass of a leveling agent "BYK-361N" (manufactured by BM Chemie) and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)-1-butanone ("Irgacure (registered trademark) 369 (Irg369)" manufactured by BASF JAPAN Co., Ltd.) as a photopolymerization initiator were added. Furthermore, N-methyl-2-pyrrolidone (NMP) was added in such a manner that the solid content concentration became 13%. The mixture was stirred at 80°C for 1 hour to obtain a polymerizable liquid crystal composition (4) for forming a horizontally aligned liquid crystal curing film.
[0499] (2) Formation of horizontally aligned liquid crystal cured film
[0500] After forming a horizontal alignment film on the substrate in the same manner as in Example 4, a polymerizable liquid crystal composition (4) for forming a horizontal alignment liquid crystal curing film was applied to the horizontal alignment film, and after heating at 120° C. for 60 seconds, a high-pressure mercury lamp (Unicure VB-15201BY-A, manufactured by Ushio Electric Co., Ltd.) was used to irradiate the surface coated with the polymerizable liquid crystal composition (4) with ultraviolet light (cumulative light intensity at a wavelength of 365 nm under a nitrogen atmosphere: 500 mJ / cm 2 ), thereby forming an optically anisotropic layer X' consisting of a horizontally aligned liquid crystal cured film. The film thickness of the obtained horizontally aligned liquid crystal cured film was measured with an ellipsometer and found to be 0.9 μm.
[0501] On the horizontally oriented liquid crystal cured film of the laminated body formed by the substrate, the horizontally oriented film and the horizontally oriented liquid crystal cured film prepared in the above manner, a vertically oriented liquid crystal cured film with a film thickness of 1.0 μm is formed in the same manner as in Example 3, thereby obtaining a laminated body, and a polarizing film is attached to the surface on the substrate side, thereby obtaining a polarizing plate.
[0502] 11. Comparative Example 2
[0503] Except that the preparation of the polymerizable liquid crystal composition for forming a vertically aligned liquid crystal cured film and the formation of the vertically aligned liquid crystal cured film are changed as follows, the same operation as in Example 1 is performed to prepare a laminated body in which a substrate, a horizontally aligned film, a horizontally aligned liquid crystal cured film, and a vertically aligned liquid crystal cured film are sequentially stacked adjacently. In addition, the same operation as in Example 3 is performed to prepare a polarizing plate by attaching a polarizing film to the surface on the substrate side, and the visual recognition during black display is confirmed. The results are shown in Table 1.
[0504] (1) Preparation of polymerizable liquid crystal composition (4) for forming a vertically aligned liquid crystal cured film
[0505] For the polymerizable liquid crystal compound (III-1-4), 0.25 parts by mass of the leveling agent "F-556" (manufactured by DIC Corporation), 1.5 parts by mass of the ionic compound A (molecular weight: 645) prepared with reference to Japanese Patent Application No. 2016-514802, 0.5 parts by mass of the silane coupling agent "KBE-9103" (manufactured by Shin-Etsu Chemical Co., Ltd.), and 6 parts by mass of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)-1-butanone (manufactured by BASF JAPAN Co., Ltd. "Irgacure (registered trademark) 369 (Irg369)") as a photopolymerization initiator were added. Furthermore, N-methyl-2-pyrrolidone (NMP) was added in such a manner that the solid content concentration became 13%. The mixture was stirred at 80°C for 1 hour to obtain a polymerizable liquid crystal composition (4) for forming a vertically aligned liquid crystal cured film.
[0506] (2) Preparation of vertically oriented liquid crystal cured film
[0507] Using the polymerizable liquid crystal composition (1) for forming a horizontally oriented liquid crystal curing film prepared in Example 1, the same operation as in Example 3 was performed to produce a laminated body in which a substrate, a horizontally oriented film, and a horizontally oriented liquid crystal curing film with a thickness of 1.6 μm were stacked adjacent to each other in sequence. Next, after the surface of the horizontally oriented liquid crystal curing film was subjected to corona treatment, a rod coater was used to apply a polymerizable liquid crystal composition (4) for forming a vertically oriented liquid crystal curing film, and heated at 120°C for 60 seconds. Next, a high-pressure mercury lamp (Unicure VB-15201BY-A, manufactured by Ushio Electric Co., Ltd.) was used to irradiate ultraviolet rays from the surface coated with the polymerizable liquid crystal composition (4) for forming a vertically oriented liquid crystal curing film (under a nitrogen atmosphere, the accumulated light amount at a wavelength of 365 nm: 500 mJ / cm 2 ), thereby forming an optically anisotropic layer Y' consisting of a vertically aligned liquid crystal cured film. The film thickness of the obtained vertically aligned liquid crystal cured film was measured with an ellipsometer (M-220 manufactured by JASCO Corporation) and found to be 0.8 μm.
[0508] 12. Comparative Example 3
[0509] A phase difference film (ZeonorFilm, manufactured by Optes Co., Ltd.) formed of a cycloolefin resin having a film thickness of 32 μm and an in-plane phase difference value of 140 nm was used as a substrate. The same operation as in Comparative Example 2 was performed. After the surface of the substrate was subjected to corona treatment, a polymerizable liquid crystal composition (4) for forming a vertically aligned liquid crystal curable film was applied using a bar coater and heated at 120° C. for 60 seconds. Next, a high-pressure mercury lamp (Unicure VB-15201BY-A, manufactured by Ushio Electric Co., Ltd.) was used to irradiate ultraviolet rays (under a nitrogen atmosphere, the cumulative light amount at a wavelength of 365 nm: 500 mJ / cm 2 ), thereby forming a vertically oriented liquid crystal curing film, thereby producing a laminate in which an optically anisotropic layer X formed by a substrate and an optically anisotropic layer Y' formed by a vertically oriented liquid crystal curing film are stacked adjacent to each other in sequence. The film thickness of the obtained vertically oriented liquid crystal curing film was measured with an ellipsometer (M-220 manufactured by JASCO Corporation), and the result was 0.8μm. In addition, a polarizing plate was prepared by bonding a polarizing film to the surface on the substrate side, and the visual recognition during black display was confirmed. The results are shown in Table 1. It should be noted that the laminate formed by the substrate and the vertically oriented liquid crystal curing film was placed in an oven at 100°C and allowed to stand for 30 minutes. As a result, it was confirmed that the laminate was deformed and curled due to heat.
[0510] 13. Comparative Example 4
[0511] Using the polymerizable liquid crystal composition (4) for forming a horizontally aligned liquid crystal cured film prepared in Comparative Example 1, the same operation as in Comparative Example 1 was performed to prepare a laminated body in which a substrate, a horizontally aligned film, and a horizontally aligned liquid crystal cured film with a film thickness of 0.9 μm were stacked in sequence. Next, in the same manner as in Comparative Example 2, a polymerizable liquid crystal composition (4) for forming a vertically aligned liquid crystal cured film was used to form a vertically aligned liquid crystal cured film with a film thickness of 0.7 μm on the above-mentioned horizontally aligned liquid crystal cured film, thereby obtaining a laminated body, and a polarizing film was attached to the surface on the substrate side to prepare a polarizing plate, and visual recognition during black display was confirmed. The results are shown in Table 1.
[0512] 14. Example 10
[0513] (1) Preparation of polymerizable liquid crystal composition (5) for forming a vertically aligned liquid crystal cured film
[0514] The polymerizable liquid crystal compound (X1) and the polymerizable liquid crystal compound LC242: Paliocolor LC242 (registered trademark of BASF) were mixed at a mass ratio of 60:40 to obtain a mixture. 0.25 mass parts of a leveling agent "F-556" (manufactured by DIC Corporation), 1.5 mass parts of an ionic compound A (molecular weight: 645) prepared with reference to Japanese Patent Application No. 2016-514802, 0.5 mass parts of a silane coupling agent "KBE-9103" (manufactured by Shin-Etsu Chemical Co., Ltd.), and 6 mass parts of 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)-1-butanone (manufactured by BASF JAPAN Co., Ltd. "Irgacure (registered trademark) 369 (Irg369)") as a photopolymerization initiator were added to 100 mass parts of the obtained mixture. Furthermore, N-methyl-2-pyrrolidone (NMP) was added so that the solid content concentration became 13%. The mixture was stirred at 80° C. for 1 hour to obtain a polymerizable liquid crystal composition (5) for forming a vertically aligned liquid crystal cured film.
[0515] (2) Preparation of vertically oriented liquid crystal cured film
[0516] A phase difference film formed of a cycloolefin resin having an in-plane phase difference value of 120 nm was used as a substrate. The same operation as in Comparative Example 3 was performed. After the above-mentioned substrate surface was subjected to corona treatment, a polymerizable liquid crystal composition (5) for forming a vertically aligned liquid crystal cured film was applied using a bar coater and heated at 120° C. for 60 seconds. Next, a high-pressure mercury lamp (Unicure VB-15201BY-A, manufactured by Ushio Electric Co., Ltd.) was used to irradiate ultraviolet rays (under a nitrogen atmosphere, the cumulative light amount at a wavelength of 365 nm: 500 mJ / cm 2 ), thereby forming a vertically oriented liquid crystal cured film, thereby preparing a laminated body in which an optically anisotropic layer X formed by a substrate and an optically anisotropic layer Y' formed by a vertically oriented liquid crystal cured film are stacked adjacent to each other in sequence. The film thickness of the obtained vertically oriented liquid crystal cured film was measured with an ellipsometer (M-220 manufactured by JASCO Corporation), and the result was 1.2 μm. In addition, a polarizing film was bonded to the surface on the substrate side to prepare a polarizing plate, and visual recognition during black display was confirmed. The results are shown in Table 1.
[0517] 15. Example 11
[0518] A phase difference film formed of a cycloolefin resin having an in-plane phase difference value of 120 nm was used as a substrate, and the substrate surface was subjected to a corona treatment in the same manner as in Comparative Example 3. Next, a polymerizable liquid crystal composition (2) for forming a vertically aligned liquid crystal cured film was applied to the corona-treated substrate surface using a bar coater in the same manner as in Example 9, and a vertically aligned liquid crystal cured film having a film thickness of 1.3 μm was formed on the substrate to obtain a laminate, and a polarizing film was bonded to the surface on the substrate side to prepare a polarizing plate, and visual recognition during black display was confirmed.
[0519] [Table 1]
[0520] A B AB Black for visual recognition Example 1 0.970 0.960 0.010 A Example 2 0.970 1.000 -0.030 A Example 3 1.000 0.960 0.040 A Example 4 1.000 1.000 0.000 A Example 5 1.000 1.040 -0.040 B Example 6 1.040 1.000 0.040 B Example 7 1.040 1.040 0.000 B Example 8 1.000 0.960 0.040 A Example 9 1.000 1.000 0.000 A Comparative Example 1 1.100 0.960 0.140 C Comparative Example 2 0.970 1.100 -0.130 C Comparative Example 3 1.000 1.100 -0.100 C Comparative Example 4 1.100 1.100 0.000 C Example 10 1.000 0.980 0.020 A Embodiment 11 1.000 1.000 0.000 A
[0521] According to the present invention, it is possible to provide a laminated body that is thinner and less deformed by heat, a polarizing plate including the laminated body, and an image display device including the laminated body.
Claims
1. A laminate comprising an optically anisotropic layer X satisfying the following formula (1) and an optically anisotropic layer Y satisfying the following formula (2), The laminate satisfies the following formula (3): 0.960≤ A ≤1.040 (1) 0.960≤ B ≤1.040 (2) -0.070≤ AB ≤0.070 (3) In formulas (1) to (3), A represents the ratio (Re(450) / Re(550)) of the in-plane retardation value (Re(450)) of the optical anisotropic layer X at a wavelength of 450 nm to the in-plane retardation value (Re(550)) at a wavelength of 550 nm, and B represents the ratio (Rth(450) / Rth(550)) of the retardation value in the thickness direction at a wavelength of 450 nm of the optical anisotropic layer Y to the retardation value in the thickness direction (Rth(550)) at a wavelength of 550 nm.
2. The laminate according to claim 1, wherein The optically anisotropic layer X has a thickness of 0.5 μm or more and 5 μm or less.
3. The laminate according to claim 1, wherein The optically anisotropic layer Y has a thickness of 0.3 μm or more and 5 μm or less. 4 . A polarizing plate comprising a polarizing film, the optically anisotropic layer X according to claim 1 , and the optically anisotropic layer Y according to claim 1 in this order. 5 . A polarizing plate comprising a polarizing film, the optically anisotropic layer Y according to claim 1 , and the optically anisotropic layer X according to claim 1 in this order.
6. The polarizing plate according to claim 4, wherein: The angle formed between the absorption axis of the polarizing film and the slow axis of the optically anisotropic layer X is 90±5°.
7. The polarizing plate according to claim 5, wherein: The angle formed between the absorption axis of the polarizing film and the slow axis of the optically anisotropic layer X is 0±5°. 8 . An image display device comprising the polarizing plate according to claim 4 .