Transparent conductive film
By designing an indium-tin composite oxide layer with an amorphous layer of more than 30 nm and a crystalline layer with a ratio of more than 15% in the transparent conductive film, the contradiction between low resistance and high transparency in the transparent conductive film is solved, and the realization of Transparent conductive films suitable for a variety of electronic devices.
Patent Information
- Application Number
- CN202410362669.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-01
AI Technical Summary
Existing transparent conductive films have contradictions in balancing low resistance and high transparency, making it difficult to meet the requirements of transparent electrodes at the same time.
A transparent substrate and a transparent conductive layer with a thickness of more than 100nm are used along the thickness direction. The conductive layer is composed of an amorphous layer and a crystalline layer with a thickness of more than 30nm. The thickness of the crystalline layer accounts for 15% of the thickness of the conductive layer. Above, and the tin oxide ratio of the amorphous layer is higher than that of the crystalline layer, an indium tin composite oxide layer is used as the conductive material.
It has achieved a transparent conductive film suitable for a variety of electronic devices while ensuring low resistance and high transparency, and is suitable for applications such as contact sensors and dimming components.
Smart Images

Figure CN118737524A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a transparent conductive film. Background Art
[0002] Conventionally, a transparent conductive film having a resin transparent substrate and a transparent conductive layer (transparent conductive layer) in sequence along the thickness direction is known. The transparent conductive layer is used as a conductor film for forming a transparent electrode in various devices such as a display panel, a touch panel, and a solar cell. The transparent conductive layer is formed in the form of a crystalline or amorphous conductive oxide layer by forming a conductive oxide on a transparent substrate, for example, by sputtering. The technology related to such a transparent conductive film is described in, for example, the following Patent Document 1.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2016-157021 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] The transparent conductive layer of the transparent conductive film is required to have low resistance. In particular, this requirement is strict for the transparent conductive film used for transparent electrode. From the viewpoint of low resistance, it is better when the transparent conductive layer is crystalline than when the transparent conductive layer is amorphous. On the other hand, the transparent conductive layer of the transparent conductive film is also required to have high transparency. From the viewpoint of transparency, it is better when the transparent conductive layer is amorphous than when the transparent conductive layer is crystalline. There is such a trade-off relationship between the low resistance and transparency of the transparent conductive layer. However, the present inventors have obtained the following insights.
[0008] The composite transparent conductive layer including an amorphous layer and a crystalline layer stacked together may have higher transparency than an amorphous transparent conductive layer (amorphous single layer) when the transparent conductive layer is thick. The present invention is based on this finding.
[0009] The present invention provides a transparent conductive film suitable for achieving both low resistance and transparency of a transparent conductive layer.
[0010] Solutions for solving problems
[0011] The present invention [1] includes a transparent conductive film, which comprises a transparent substrate and a transparent conductive layer in order along the thickness direction, the transparent conductive layer having a thickness of 100 nm or more, the transparent conductive layer comprising an amorphous layer and a crystalline layer in order from the transparent substrate side, the amorphous layer having a thickness of 30 nm or more, and the ratio of the thickness of the crystalline layer to the thickness of the transparent conductive layer is 15% or more.
[0012] The present invention [2] comprises the transparent conductive film described in the above [1], wherein the above ratio is 70% or less.
[0013] The present invention [3] comprises the transparent conductive film described in [1] or [2] above, wherein the transparent conductive layer is an indium tin composite oxide layer.
[0014] The present invention [4] includes the transparent conductive film according to the above [3], wherein the tin oxide ratio of the amorphous layer is higher than the tin oxide ratio of the crystalline layer.
[0015] Effects of the Invention
[0016] In the transparent conductive film of the present invention, as described above, the transparent conductive layer has a thickness of 100 nm or more, and the transparent conductive layer has an amorphous layer and a crystalline layer with a thickness of 30 nm or more in order from the transparent substrate side, and the ratio of the thickness of the crystalline layer to the thickness of the transparent conductive layer is 15% or more. The transparent conductive layer has a thickness of 100 nm or more and the ratio of the thickness of the crystalline layer in the transparent conductive layer is 15% or more, which is suitable for ensuring the low resistivity of the transparent conductive layer. The transparent conductive layer with a thickness of 100 nm or more has an amorphous layer and a crystalline layer with a thickness of 30 nm or more in order from the transparent substrate side, which is suitable for ensuring the transparency of the transparent conductive layer. This transparent conductive film is suitable for taking into account both the low resistivity and transparency of the transparent conductive layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a schematic cross-sectional view of one embodiment of the transparent conductive film of the present invention.
[0018] Figure 2 express Figure 1 An example of a method for producing a transparent conductive film is shown in . Figure 2 A represents the preparation process. Figure 2 B represents the first layer forming step, Figure 2 C represents the second layer forming step, Figure 2 D represents a heating process.
[0019] Figure 3 express Figure 1 The transparent conductive layer in the transparent conductive film shown in FIG. 1 is patterned.
[0020] Description of Reference Numerals
[0021] XTransparent Conductive Film
[0022] HThickness direction
[0023] 10 Transparent substrate
[0024] 11 Page 1
[0025] 12 Side 2
[0026] 20 Transparent conductive layer
[0027] 21 Amorphous layer
[0028] 22 Crystalline layer DETAILED DESCRIPTION
[0029] The transparent conductive film X as one embodiment of the present invention includes a transparent substrate 10 and a transparent conductive layer 20 in this order along the thickness direction H. The transparent conductive film X has a sheet shape extending in a direction (surface direction) perpendicular to the thickness direction H. The transparent conductive film X is an element included in, for example, a touch sensor device, a dimming element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, and an image display device.
[0030] The transparent substrate 10 is an element for ensuring the strength of the transparent conductive film X. The transparent substrate 10 has a first surface 11 and a second surface 12 , and the second surface 12 is located on the opposite side to the first surface 11 .
[0031] The transparent substrate 10 is, for example, a flexible transparent resin film. As the material of the resin film, polyester resin, polyolefin resin, acrylic resin, polycarbonate resin, polyethersulfone resin, polyarylate resin, melamine resin, polyamide resin, polyimide resin, cellulose resin and polystyrene resin can be listed. As the polyester resin, polyethylene terephthalate (PET), polybutylene terephthalate and polyethylene naphthalate can be listed. As the polyolefin resin, polyethylene, polypropylene and cycloolefin polymer can be listed. As the acrylic resin, polymethacrylate can be listed. From the viewpoint of transparency and strength, the material of the resin film is preferably polyester resin, more preferably PET.
[0032] The transparent substrate 10 may have a multilayer structure in which a cured resin layer (not shown) is formed on one or both sides of a resin film. Examples of the cured resin layer include a hard coat layer and an anti-adhesion layer. The cured resin layer is a cured product of a curable resin composition. The curable resin composition contains a curable resin. Examples of curable resins include polyester resins, acrylic carbamate resins, acrylic resins (excluding acrylic carbamate resins), carbamate resins (excluding acrylic carbamate resins), amide resins, silicone resins, epoxy resins, and melamine resins. These curable resins may be used alone or in combination of two or more. In addition, examples of curable resins include ultraviolet curable resins and thermosetting resins.
[0033] The curable resin composition may contain particles. Examples of the particles include inorganic oxide particles and organic particles. Examples of materials for the inorganic oxide particles include silicon dioxide, aluminum oxide, titanium dioxide, zirconium oxide, calcium oxide, tin oxide, indium oxide, cadmium oxide, and antimony oxide. Examples of materials for the organic particles include polymethyl methacrylate, polystyrene, polyurethane, acrylic-styrene copolymers, benzoguanamine, melamine, and polycarbonate.
[0034] From the viewpoint of exhibiting the function of the cured resin layer in the transparent conductive film X, the thickness of the cured resin layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, and further preferably 1 μm or more. From the viewpoint of ensuring the transparency of the transparent conductive film X, the thickness of the cured resin layer is preferably 10 μm or less, more preferably 5 μm or less, and further preferably 3 μm or less.
[0035] The first surface 11 (the surface on the transparent conductive layer 20 side) of the transparent substrate 10 may be subjected to a surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment.
[0036] From the viewpoint of ensuring the strength of the transparent conductive film X, the thickness of the transparent substrate 10 is preferably 1 μm or more, more preferably 10 μm or more, further preferably 50 μm or more, further preferably 80 μm or more, and further preferably 90 μm or more. From the viewpoint of ensuring the handling properties of the transparent substrate 10 in a roll-to-roll method, the thickness of the transparent substrate 10 is preferably 500 μm or less, more preferably 300 μm or less, further preferably 200 μm or less, and further preferably 150 μm or less.
[0037] From the viewpoint of ensuring the transparency of the transparent substrate 10, the total light transmittance (JIS K7375-2008) of the transparent substrate 10 is preferably 80% or more, more preferably 85% or more, and further preferably 88% or more. The total light transmittance of the transparent substrate 10 is, for example, 100% or less.
[0038] The transparent conductive layer 20 is a film having both light transmittance and conductivity. The transparent conductive layer 20 is arranged on the transparent substrate 10 in the present embodiment. Specifically, the transparent conductive layer 20 contacts the first surface 11 of the transparent substrate 10. In addition, the transparent conductive layer 20 has an amorphous layer 21 as a first layer and a crystalline layer 22 as a second layer in order from the transparent substrate 10 side. In the present embodiment, the amorphous layer 21 contacts the transparent substrate 10. The crystalline layer 22 is arranged on the side opposite to the transparent substrate 10 relative to the amorphous layer 21. In the present embodiment, the crystalline layer 22 contacts the amorphous layer 21. The crystalline layer 22 is arranged on the side opposite to the transparent substrate 10 relative to the amorphous layer 21 and contacts the amorphous layer 21, which is preferred from the viewpoint of the bendability of the transparent conductive layer 20 (suppression of fragmentation during bending).
[0039] In the present embodiment, the amorphous layer 21 is formed of an amorphous conductive oxide. As conductive oxides, for example, conductive oxides containing indium and conductive oxides containing antimony can be listed. As conductive oxides containing indium, for example, indium tin composite oxide (ITO), indium zinc composite oxide (IZO), indium gallium composite oxide (IGO) and indium gallium zinc composite oxide (IGZO) can be listed. As conductive oxides containing antimony, for example, antimony tin composite oxide (ATO) can be listed. From the viewpoint of achieving high transparency and good conductivity of the transparent conductive layer 20, the conductive oxide is preferably a conductive oxide containing indium, and more preferably ITO. ITO can contain metals or semimetals other than In and Sn in an amount less than the content of each of In and Sn.
[0040] From the viewpoint of ensuring the amorphous nature of the amorphous layer 21, the ratio of the amount of tin oxide in the ITO in the amorphous layer 21 to the total amount of indium oxide (In2O3) and tin oxide (SnO2) (tin oxide ratio R1) is preferably 11% by mass or more, more preferably 12% by mass or more, and further preferably 12.5% by mass or more, and preferably 15% by mass or less, more preferably 14% by mass or less, and further preferably 13% by mass or less. From the viewpoint of ensuring the amorphous nature of the amorphous layer 21, the tin oxide ratio R1 is preferably higher than the tin oxide ratio R2 of the crystalline layer 22 described later.
[0041] The tin oxide ratio in ITO can be identified, for example, by the following operation. First, the existence ratio of indium atoms (In) and tin atoms (Sn) in ITO as the object of measurement is obtained by X-ray photoelectron spectroscopy. According to the existence ratios of In and Sn in ITO, the ratio of the number of atoms of Sn in ITO relative to the number of atoms of In is obtained. Thus, the tin oxide ratio in ITO can be obtained. In addition, the tin oxide ratio in ITO can also be determined based on the tin oxide (SnO2) content ratio of the ITO target used in sputtering film formation.
[0042] Whether a film such as the amorphous layer 21 is an amorphous film can be determined by observing the cross section of the film (target film) using a field emission transmission electron microscope (FE-TEM). When no crystal grains are confirmed but an amorphous region is confirmed in the cross-sectional observation of the target film based on FE-TEM, the target film can be determined to be an amorphous film.
[0043] In the present embodiment, the crystalline layer 22 is formed of a crystalline conductive oxide. As the conductive oxide, the conductive oxide layer described above for the amorphous layer 21 can be cited. From the viewpoint of achieving high transparency and good conductivity of the transparent conductive layer 20, the conductive oxide is preferably a conductive oxide containing indium, and more preferably ITO. The material of the crystalline layer 22 and the material of the amorphous layer 21 can be different types, preferably the same type. The transparent conductive layer 20 having the amorphous layer 21 and the crystalline layer 22 is preferably a conductive oxide layer containing indium, and more preferably an indium tin composite oxide layer.
[0044] From the viewpoint of ensuring the crystallinity of the crystalline layer 22, the ratio of the amount of tin oxide in the ITO in the crystalline layer 22 to the total amount of indium oxide and tin oxide (tin oxide ratio R2) is preferably 1 mass % or more, more preferably 3 mass % or more, further preferably 5 mass % or more, and is preferably less than 11 mass %, more preferably 10.5 mass % or less, further preferably 10 mass % or less.
[0045] Whether a film such as the crystalline layer 22 is a crystalline film can be determined by observing the cross section of the film (target film) using a field emission transmission electron microscope (FE-TEM). When no amorphous region is confirmed but crystal grains are confirmed in the cross-sectional observation of the target film based on FE-TEM, the target film can be determined to be a crystalline film.
[0046] The thickness (total thickness) of the transparent conductive layer 20 is 100 nm or more. A transparent conductive layer 20 having a thickness of 100 nm or more is suitable for reducing the resistance of the transparent conductive layer 20. From the viewpoint of reducing the resistance of the transparent conductive layer 20, the thickness of the transparent conductive layer 20 is preferably 110 nm or more, more preferably 120 nm or more, and further preferably 125 nm or more. From the viewpoint of transparency of the transparent conductive layer 20, the thickness of the transparent conductive layer 20 is preferably 300 nm or less, more preferably 200 nm or less, and further preferably 150 nm or less.
[0047] The thickness T1 of the amorphous layer 21 is 30 nm or more. In the transparent conductive layer 20 having a thickness of 100 nm or more, the thickness T1 of the amorphous layer 21 disposed on the transparent substrate 10 side is 30 nm or more, which is suitable for ensuring the transparency of the transparent conductive layer 20. From the viewpoint of transparency of the transparent conductive layer 20, the thickness T1 of the amorphous layer 21 is preferably 45 nm or more, and more preferably 50 nm or more. From the viewpoint of low resistance of the transparent conductive layer 20, the thickness T1 is preferably 120 nm or less, more preferably 100 nm or less, and further preferably 80 nm or less. In addition, from the viewpoint of transparency of the transparent conductive layer 20, the ratio of the thickness T1 of the amorphous layer 21 to the thickness (total thickness) of the transparent conductive layer 20 is preferably 30% or more, more preferably 35% or more, and further preferably 40% or more. From the viewpoint of low resistance of the transparent conductive layer 20, the ratio is preferably less than 85%, more preferably 65% or less, and further preferably 45% or less.
[0048] The ratio of the thickness T2 of the crystalline layer 22 to the thickness (total thickness) of the transparent conductive layer 20 is 15% or more. In the transparent conductive layer 20 having a thickness of 100 nm or more, the crystalline layer 22 is arranged on the opposite side of the transparent substrate 10 relative to the amorphous layer 21, and the thickness T2 of the crystalline layer 22 is 15% or more, which is suitable for ensuring the low resistance of the transparent conductive layer 20. From the viewpoint of the low resistance of the transparent conductive layer 20, the ratio of the thickness T2 of the crystalline layer 22 to the thickness of the transparent conductive layer 20 is preferably 35% or more, more preferably 40% or more, and more preferably 50% or more. From the viewpoint of the transparency of the transparent conductive layer 20, the ratio is preferably 70% or less, more preferably 65% or less, and more preferably 60% or less. In addition, from the viewpoint of the low resistance of the transparent conductive layer 20, the thickness T2 of the crystalline layer 22 is preferably 15 nm or more, more preferably 35 nm or more, more preferably 40 nm or more, and more preferably 50 nm or more. From the viewpoint of transparency of the transparent conductive layer 20 , the thickness T2 is preferably 70 nm or less, more preferably 65 nm or less, and even more preferably 60 nm or less.
[0049] From the viewpoint of ensuring the transparency of the transparent conductive layer 20, the total light transmittance (JIS K7375-2008) of the transparent conductive layer 20 is preferably 80% or more, more preferably 85% or more, and further preferably 88% or more. The total light transmittance of the transparent conductive layer 20 is, for example, 100% or less.
[0050] From the viewpoint of reducing the resistance of the transparent conductive layer 20, the resistivity of the transparent conductive layer 20 is preferably 3.5×10 -4 Ω·cm or less, more preferably 3.2×10 -4 Ω·cm or less, more preferably 3.0×10 -4 Ω·cm or less, more preferably 2.8×10 -4 The resistivity of the transparent conductive layer 20 is, for example, 0.5×10 -4 Ω·cm or more, 1.0×10 -4 Ω·cm or more, 2.0×10 -4 The method for measuring the resistivity is as described later in the examples.
[0051] The total light transmittance (JIS K 7375-2008) of the transparent conductive film X is preferably 80% or more, more preferably 85% or more, and further preferably 88% or more. This configuration is suitable for ensuring the transparency required for the transparent conductive film X when the transparent conductive film X is provided in a touch sensor device, a dimming element, a photoelectric conversion element, a heat line control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device, etc. The total light transmittance of the transparent conductive film X is, for example, 100% or less. The method for measuring the total light transmittance is as described later in the examples.
[0052] The transparent conductive film X is produced, for example, as follows.
[0053] First, if Figure 2 As shown in A, a transparent substrate 10 is prepared (preparation step).
[0054] Then, if Figure 2 As shown in FIG. 2B , a first layer 21′ is formed on the transparent substrate 10 (first layer forming step). The first layer 21′ is an amorphous first conductive oxide layer. The first conductive oxide layer is formed in the heating step ( Figure 2 D) Amorphous layer is maintained thereafter. In this step, specifically, a conductive oxide is deposited on the first surface 11 of the transparent substrate 10 by sputtering to form an amorphous first conductive oxide layer (first layer 21').
[0055] In the sputtering method, it is preferred to use a sputtering film forming device that can implement a film forming process by a roll-to-roll method. When a roll-to-roll sputtering film forming device is used in the first layer formation process, a long transparent substrate 10 as a workpiece film is allowed to travel from a take-off roller provided in the device to a winding roller, and at the same time, a material is formed on the workpiece film to form a first layer 21'. The travel speed of the workpiece film is, for example, 0.5 to 5 m / min. In addition, in the sputtering method, a sputtering film forming device having one film forming chamber can be used, or a sputtering film forming device having a plurality of film forming chambers arranged in sequence along the travel path of the transparent substrate 10 can be used (the same is also true in the second layer formation process described later).
[0056] In the sputtering method, specifically, a sputtering gas (inactive gas) is introduced into a film forming chamber of a sputtering film forming device under vacuum conditions, and a negative voltage is applied to a target on a cathode arranged in the film forming chamber. This generates a glow discharge to ionize the gas atoms, causing the gas ions to collide with the target surface at high speed, ejecting the target material from the target surface, and causing the ejected target material to accumulate on the workpiece film (transparent substrate 10). As a target material, for example, a sintered body of a conductive oxide described above for the amorphous layer 21 can be used. As sputtering gases, for example, argon, krypton, xenon and mixed gases thereof can be listed. The sputtering method is preferably a reactive sputtering method. In the reactive sputtering method, for example, in addition to the sputtering gas, oxygen as a reactive gas is also introduced into the film forming chamber.
[0057] From the appropriate formation in the heating step described later ( Figure 2 D) From the viewpoint of maintaining the amorphous first conductive oxide layer thereafter, the conditions (first sputtering film formation conditions) related to film formation by sputtering (sputtering film formation) in the first layer formation step are as follows.
[0058] The desired vacuum degree in the film forming chamber before sputtering is 0.9×10 -4 Pa or less. In the reactive sputtering method, the ratio of the amount of oxygen introduced into the film forming chamber to the total amount of sputtering gas and oxygen introduced is preferably 1 flow % or more, more preferably 2 flow % or more, and preferably 8 flow % or less, more preferably 5 flow % or less. The film forming temperature (the temperature of the transparent substrate 10 on which the first layer 21' is to be formed) is preferably -50°C or more, more preferably -25°C or more, and preferably 20°C or less, more preferably 0.0°C or less. By adjusting the achieved vacuum degree, oxygen introduction ratio, film forming temperature and gas pressure during film formation in the first layer forming step, it is possible to form a vacuum in the heating step ( Figure 2 D) The amorphous first conductive oxide layer is maintained thereafter.
[0059] In the first layer formation step, as a power source for applying a voltage to the target, for example, a DC power source, an AC power source, an MF power source, and an RF power source can be listed. As the power source, a DC power source and an RF power source can be used in combination. The absolute value of the discharge voltage in the sputtering film formation is, for example, 50 V or more, and, for example, 500 V or less. The horizontal magnetic field intensity on the target is, for example, 10 mT or more, and, for example, 100 mT or less.
[0060] Then, if Figure 2 As shown in FIG. 3 , a second layer 22′ is formed on the first layer 21′ (second layer forming step). The second layer 22′ is an amorphous second conductive oxide layer. The second conductive oxide layer is formed by a heating step (described later) Figure 2 D) is a layer that is crystallized. Specifically, in this step, a conductive oxide is formed on the first layer 21' by sputtering to form an amorphous second conductive oxide layer (second layer 22'). The first layer 21' and the second layer 22' form an amorphous transparent conductive layer 20'.
[0061] In the sputtering method, it is preferred to use a sputtering film forming device that can implement the film forming process using a roll-to-roll method. When a roll-to-roll sputtering film forming device is used in the second layer forming process, a long transparent substrate 10 with a first layer 21' as a workpiece film is made to travel from a take-up roll provided in the device to a take-up roll, and a material is formed on the workpiece film to form the second layer 22'. The implementation method of the sputtering method and the reactive sputtering method, which is preferably the sputtering method, are the same as those described above for the first layer forming process.
[0062] From the appropriate formation through the heating step described later ( Figure 2 D) from the viewpoint of generating a crystallized second conductive oxide layer, the conditions related to sputtering film formation in the second layer forming step (second sputtering film formation conditions) are as follows.
[0063] The desired vacuum degree in the film forming chamber before sputtering is 5.0×10 -4 Pa or less. In the reactive sputtering method, the ratio of the amount of oxygen introduced into the film forming chamber to the total amount of sputtering gas and oxygen introduced is preferably 1 flow % or more, more preferably 1.5 flow % or more, and preferably 6 flow % or less, more preferably 3 flow % or less. The film forming temperature (the temperature of the workpiece thin film on which the second layer 22' is to be formed) is preferably -50°C or more, more preferably -25°C or more, and preferably 20°C or less, more preferably 0.0°C or less. By adjusting the achieved vacuum degree, oxygen introduction ratio, film forming temperature and gas pressure during film formation in the second layer forming process, it is possible to form a vacuum layer formed by the heating process ( Figure 2 D) and a crystallized second conductive oxide layer.
[0064] In the second layer forming step, the power supply for applying voltage to the target, the absolute value of the discharge voltage in sputtering film formation, and the horizontal magnetic field intensity on the target are the same as those described above for the first layer forming step.
[0065] In the present manufacturing method, Figure 2 As shown in D, the second layer 22' is crystallized by heating to form a crystalline layer 22 (heating process). As heating means, for example, infrared heaters and ovens can be listed. As heating ovens, for example, heat medium heating ovens and hot air heating ovens can be listed. The environment during heating can be any one of a vacuum environment and an atmospheric environment. Heating is preferably performed in the presence of oxygen. From the viewpoint of ensuring a high crystallization rate, the heating temperature is preferably above 100°C, more preferably above 120°C. From the viewpoint of suppressing the effect of heating on the transparent substrate 10, the heating temperature is preferably below 180°C, more preferably below 160°C. From the viewpoint of sufficient crystallization of the crystalline layer 22, the heating time is preferably above 5 minutes, preferably above 10 minutes, and more preferably above 20 minutes. From the viewpoint of shortening the tact time in this process, the heating time is preferably below 200 minutes, more preferably below 100 minutes, and more preferably below 80 minutes.
[0066] By heating in this process, the second layer 22' is crystallized while maintaining the amorphous nature of the first layer 21', thereby forming the transparent conductive layer 20 (amorphous layer 21, crystalline layer 22). In this process, as a method for maintaining the amorphous nature of the first layer 21' and crystallizing the second layer 22', there are the following methods: increasing the tin oxide ratio and / or Sn concentration of the first layer 21' compared to the second layer 22'; and increasing the amount of oxygen introduced during the first sputtering film formation compared to the second sputtering film formation (the higher the tin oxide ratio and / or Sn concentration in the first layer 21', the less likely it is to crystallize during heating).
[0067] In the above-described manner, a transparent conductive film X is produced.
[0068] like Figure 3 As schematically shown in FIG. 1 , the transparent conductive layer 20 in the transparent conductive film X may be patterned. The transparent conductive layer 20 may be patterned by etching the transparent conductive layer 20 through a predetermined etching mask. The patterned transparent conductive layer 20 is, for example, a wiring pattern.
[0069] In the transparent conductive film X, as described above, the transparent conductive layer 20 has a thickness of 100 nm or more, and the transparent conductive layer 20 has an amorphous layer 21 and a crystalline layer 22 with a thickness of 30 nm or more in this order from the transparent substrate side, and the ratio of the thickness of the crystalline layer 22 to the thickness of the transparent conductive layer 20 is 15% or more. The transparent conductive layer 20 has a thickness of 100 nm or more, and the ratio of the thickness of the crystalline layer 22 in the transparent conductive layer 20 is 15% or more, which is suitable for ensuring low resistance of the transparent conductive layer 20. The transparent conductive layer 20 with a thickness of 100 nm or more has an amorphous layer 21 and a crystalline layer 22 with a thickness of 30 nm or more in this order from the transparent substrate side, which is suitable for ensuring transparency of the transparent conductive layer 20.
[0070] Therefore, the transparent conductive film X is suitable for achieving both low resistance and transparency of the transparent conductive layer 20. Specifically, it is as shown in the examples and comparative examples described later.
[0071] Example
[0072] The present invention is specifically described below with reference to the following embodiments. The present invention is not limited to the embodiments. In addition, the specific numerical values of the compounding amount (content), physical property values, parameters, etc. described below can be replaced with the upper limit (numerical value defined as "below" or "less than") or lower limit (numerical value defined as "above" or "exceeding") of the compounding amount (content), physical property values, parameters, etc. corresponding to them described in the above-mentioned "Specific Implementation Methods".
[0073] [Example 1]
[0074] First, a long polyethylene terephthalate (PET) film (product name "GC100-JBN", thickness 100 μm, manufactured by Mitsubishi Chemical Corporation) was prepared as a transparent substrate.
[0075] Next, a conductive oxide film was formed on one side (first side) of the transparent substrate by reactive sputtering to form an amorphous first conductive oxide layer with a thickness of 100 nm as the first layer (on the first side). Figure 2 B is the first layer 21') (first layer forming process). In this process, a first sputtering film forming device (DC magnetron sputtering film forming device) of a roll-to-roll method is used. The device is equipped with a film forming chamber capable of advancing a workpiece thin film and performing a film forming process by a roll-to-roll method. The sputtering film forming conditions in this process are as follows.
[0076] The vacuum degree in the film forming chamber of the first sputtering film forming device after vacuum exhaust reached 0.9×10 -4After 0.2 Pa, argon as a sputtering gas and oxygen as a reactive gas are introduced into the film forming chamber, and the gas pressure in the film forming chamber is set to 0.2 Pa. The ratio of the amount of oxygen introduced into the film forming chamber to the total amount of argon and oxygen introduced is set to about 3.2% flow rate. As a target, a sintered body of indium oxide and tin oxide is used, and the proportion of tin oxide in the sintered body is 12.5% by mass. As a power source for applying voltage to the target, a DC power supply is used. The horizontal magnetic field intensity on the target is set to 30mT. The film forming temperature (the temperature of the transparent substrate to form the first layer) is set to -8°C. The travel speed of the PET film as the workpiece film is set to 2.7m / min.
[0077] Next, a conductive oxide film was formed on the first layer on the transparent substrate by reactive sputtering to form an amorphous second conductive oxide layer with a thickness of 25 nm as the second layer (on the Figure 2 C is the second layer 22') (second layer forming step). Thus, an amorphous transparent conductive layer (in Figure 2 C is a transparent conductive layer 20'). In this process, a second sputtering film forming device (DC magnetron sputtering film forming device) of a roll-to-roll method is used. The device has a film forming chamber that can make the workpiece film move and perform the film forming process by a roll-to-roll method. The sputtering film forming conditions in this process are as follows.
[0078] The vacuum degree in the film forming chamber of the second sputtering film forming device after vacuum exhaust reached 5.0×10 -4 After 0.2 Pa, argon as a sputtering gas and oxygen as a reactive gas are introduced into the film forming chamber, and the gas pressure in the film forming chamber is set to 0.2 Pa. The ratio of the amount of oxygen introduced into the film forming chamber to the total amount of argon and oxygen introduced is set to about 1.5% flow rate. As a target, a sintered body of indium oxide and tin oxide is used, and the proportion of tin oxide in the sintered body is 10.0% by mass. As a power source for applying voltage to the target, a DC power supply is used. The horizontal magnetic field intensity on the target is set to 90mT. The film forming temperature (the temperature of the workpiece film to be formed as the second layer) is set to -5°C. The travel speed of the PET film as the workpiece film is set to 2.7m / min.
[0079] Next, the transparent conductive layer (first layer / second layer) on the transparent substrate was heated in a hot air heating oven (heating step). In this step, the heating temperature was set to 140°C and the heating time was set to 1 hour. Through this step, the amorphous nature of the first layer was maintained and the second layer was crystallized to form a transparent conductive layer (in Figure 2 D is a transparent conductive layer 20). The transparent conductive layer has an amorphous layer as a first layer after heating ( Figure 2 D is an amorphous layer 21) and a crystalline layer derived from the second layer that is crystallized by heating ( Figure 2D is the crystalline layer 22).
[0080] As described above, a transparent conductive film of Example 1 was prepared. The transparent conductive layer of the transparent conductive film of Example 1 had an amorphous indium tin composite oxide layer (thickness of 100 nm, tin oxide ratio of 12.5 mass%) and a crystalline indium tin composite oxide layer (thickness of 25 nm, tin oxide ratio of 10.0 mass%) in order from the transparent substrate side.
[0081] [Example 2]
[0082] A transparent conductive film of Example 2 was prepared in the same manner as the transparent conductive film of Example 1 except for the following: In the first layer forming step, the first layer was formed to a thickness of 75 nm, and in the second layer forming step, the second layer was formed to a thickness of 50 nm.
[0083] [Example 3]
[0084] A transparent conductive film of Example 3 was prepared in the same manner as the transparent conductive film of Example 1 except for the following: In the first layer forming step, the first layer was formed to a thickness of 50 nm, and in the second layer forming step, the second layer was formed to a thickness of 75 nm.
[0085] [Comparative Example 1]
[0086] A transparent conductive film of Comparative Example 1 was prepared in the same manner as the transparent conductive film of Example 1 except for the following: In the first layer forming step, the first layer was formed to a thickness of 125 nm, and the second layer forming step was not performed.
[0087] [Comparative Example 2]
[0088] A transparent conductive film of Comparative Example 2 was prepared in the same manner as the transparent conductive film of Example 1 except for the following: The first layer forming step was not performed, and in the second layer forming step, the second layer was formed to a thickness of 125 nm.
[0089] [Comparative Examples 3 to 8]
[0090] Each transparent conductive film of Comparative Examples 3 to 8 was prepared in the same manner as the transparent conductive film of Example 1 except for the following. The thickness of the first layer in the first layer forming step and the thickness of the second layer in the second layer forming step were set to the thickness shown in Table 1 (the second layer was not formed in Comparative Example 3, and the first layer was not formed in Comparative Example 8).
[0091] 〈Thickness of layer〉
[0092] The thickness (total thickness) of the transparent conductive layer of each transparent conductive film in Examples 1 to 3 and Comparative Examples 1 to 8 was measured by observation using a field emission transmission electron microscope (FE-TEM). Specifically, first, a cross-sectional observation sample of each transparent conductive layer in Examples 1 to 3 and Comparative Examples 1 to 8 was prepared using the FIB microsampling method. In the FIB microsampling method, a FIB device (product name "FB2200", manufactured by Hitachi) was used, and the acceleration voltage was set to 10 kV. Next, the cross section of the transparent conductive layer in the cross-sectional observation sample was observed using FE-TEM, and the thickness of the transparent conductive layer in the observed image was measured. In this observation, a FE-TEM device (product name "JEM-2800", manufactured by JEOL) was used, and the acceleration voltage was set to 200 kV.
[0093] The thickness of the amorphous layer (first layer) in Examples 1 to 3 and Comparative Examples 4 to 7 was measured by preparing a sample for cross-sectional observation from an intermediate product before forming the second layer on the first layer and performing FE-TEM observation of the sample. The thickness of the crystalline layer (second layer) of each transparent conductive layer in Examples 1 to 3 and Comparative Examples 4 to 7 was obtained by subtracting the thickness of the first layer from the total thickness of the transparent conductive layer.
[0094] 〈Crystallinity〉
[0095] The crystallinity (amorphous, crystalline) of the first layer and the second layer of each transparent conductive layer in Examples 1 to 3 and Comparative Examples 1 to 8 was examined as follows.
[0096] First, for the above-mentioned cross-sectional observation sample, a FE-TEM image is taken at an observation magnification of 2 million times (the sample preparation method and observation method are the same as those described above for the layer thickness measurement). Next, for the first and second layers in the captured image, when no lattice stripes (equivalent to the presence of crystal grains) are confirmed as amorphous as a whole, and when lattice stripes are confirmed as a whole, they are evaluated as crystalline. The results confirmed the following. The first layer in Examples 1 to 3 and Comparative Examples 4 to 7 is amorphous, and the second layer in Examples 1 to 3 and Comparative Examples 4 to 7 is crystalline. The transparent conductive layer (first layer) in Comparative Examples 1 and 3 is amorphous. The transparent conductive layer (second layer) in Comparative Examples 2 and 8 is crystalline. Their confirmation results are shown in Table 1.
[0097] 〈Resistivity〉
[0098] The resistivity of the transparent conductive layer of each transparent conductive film of Examples 1 to 3 and Comparative Examples 1 to 8 was measured. The specific details are as follows.
[0099] First, a 100 mm × 50 mm film for measurement was cut out from the transparent conductive film. Next, the surface resistance of the transparent conductive layer of the film for measurement was measured by the four-terminal method based on JIS K7194 (1994). Next, the resistivity (Ω·cm) was calculated by multiplying the surface resistance of the transparent conductive layer by the thickness of the transparent conductive layer. The values are shown in Table 1.
[0100] Total light transmittance
[0101] The total light transmittance of each transparent conductive film of Examples 1 to 3 and Comparative Examples 1 to 8 was measured using a "Haze Meter HZ-V3" manufactured by Suga Test Instruments in accordance with JIS K7375-2008.
[0102] [evaluate]
[0103] Among the transparent conductive films of Comparative Examples 3 to 8 (transparent conductive layer thickness 90 nm), the transparent conductive layer of the transparent conductive film of Comparative Example 3 is a single amorphous layer. The transparent conductive layer of the transparent conductive film of Comparative Example 8 is a single crystalline layer. The transparent conductive layer of the transparent conductive films of Comparative Examples 4 to 7 is a composite layer having an amorphous layer and a crystalline layer in order from the transparent substrate side. The transparent conductive films of Comparative Examples 4 to 7 have a higher total light transmittance than the transparent conductive film of Comparative Example 8, but have a lower total light transmittance than the transparent conductive film of Comparative Example 3. The greater the thickness ratio of the crystalline layer in the transparent conductive layer, the lower the total light transmittance (transparency).
[0104] Among the transparent conductive films of Examples 1 to 3 and Comparative Examples 1 and 2 (transparent conductive layer thickness of 125 nm), the transparent conductive layer of the transparent conductive film of Comparative Example 1 is an amorphous single layer. The transparent conductive layer of the transparent conductive film of Comparative Example 2 is a crystalline single layer. In contrast, the transparent conductive layer of the transparent conductive films of Examples 1 to 3 is a composite layer having an amorphous layer and a crystalline layer in order from the transparent substrate side. The transparent conductive films of Examples 1 to 3 have a higher total light transmittance (transparency) than any of the transparent conductive films in Comparative Examples 1 and 2. In the transparent conductive films of Examples 1 to 3, the greater the thickness ratio of the crystalline layer in the transparent conductive layer, the higher the total light transmittance (transparency). In addition, the transparent conductive films of Examples 1 to 3 having a transparent conductive layer with a thickness of 125 nm have a lower resistivity than the transparent conductive films of Comparative Examples 4 to 7 having a transparent conductive layer with a thickness of 90 nm, showing low resistivity.
[0105] [Table 1]
[0106] Table 1
[0107]
[0108] It should be noted that the above invention is provided as an exemplary embodiment of the present invention, which is merely an illustration and is not to be construed as limiting. Modifications of the present invention that are obvious to those skilled in the art are included in the above claims.
[0109] Industrial Applicability
[0110] The transparent conductive film X of the present invention can be suitably used for touch sensor devices, light control elements, photoelectric conversion elements, heat ray control members, antenna members, electromagnetic wave shielding members, heater members, lighting devices, image display devices, and the like.
Claims
1. A transparent conductive film comprising a transparent substrate and a transparent conductive layer in this order along a thickness direction, The transparent conductive layer has a thickness of 100 nm or more, The transparent conductive layer includes an amorphous layer and a crystalline layer in order from the transparent substrate side. The amorphous layer has a thickness of 30 nm or more, The ratio of the thickness of the crystalline layer to the thickness of the transparent conductive layer is 15% or more.
2. The transparent conductive film according to claim 1, wherein The ratio is 70% or less.
3. The transparent conductive film according to claim 1 or 2, wherein: The transparent conductive layer is an indium tin composite oxide layer.
4. The transparent conductive film according to claim 3, wherein: The tin oxide ratio of the amorphous layer is higher than the tin oxide ratio of the crystalline layer.
Citation Information
Patent Citations
Transparent conductive film for electric field drive type light control element, light control film, and electric field drive type light control element
JP2016157021A