Inductor and preparation method and application thereof

Through the combination of the Tcore model and metal soft magnetic materials, combined with the winding and hot pressing process, the problem of volume reduction and performance improvement of the inductor device is solved, the high performance and compact size requirements of the inductor device are realized, and the stability of the circuit is ensured.

CN118737623APending Publication Date: 2024-10-01KUNSHAN MAZO TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410875787.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult for existing inductor devices to maintain or improve saturation current performance while reducing size, and the technical progress of magnetic core materials is relatively slow, which cannot meet the needs of modern electronic equipment for high performance and compact size.

Method used

Using Tcore models, windings, coils and metal soft magnetic materials, the inductor is prepared through steps such as pressing Tcore, winding, hot pressing and spray painting to ensure the stability and performance of the inductor device.

Benefits of technology

Without sacrificing saturation current, the size of the inductor device is reduced, the area is saved, the demand for high performance and compact size of modern electronic equipment is met, and the stability of the circuit is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737623A_ABST
    Figure CN118737623A_ABST
Patent Text Reader

Abstract

The invention provides an inductor. The inductor comprises a Tcore model, a coil and a metal soft magnetic material. According to the inductor provided by the invention, the volume of an inductor device can be reduced on the premise of not sacrificing saturation current. By means of the novel structure, the limitation of performance improvement of a traditional magnetic core material can be broken through, and therefore the requirements of modern electronic equipment for high performance and compact size of an inductance device are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of inductors (H01F), and more specifically relates to an inductor and a preparation method and application thereof. Background Art

[0002] With the rapid development of electronic technology, the performance and volume requirements of inductor devices are becoming increasingly stringent. This includes miniaturization of device size while maintaining or improving the performance of saturation current. Usually, the realization of these requirements depends on significant improvements in the performance of magnetic materials, but the technological progress of magnetic core materials is often relatively slow.

[0003] In order to reduce the area of ​​the inductor device, Chinese invention patent CN116631739A discloses a micro coil, a micro inductor including the micro coil and a preparation method thereof. In the disclosed patent, the technical problems such as the difficulty in winding small and medium-sized inductor coils in the prior art are solved by winding the micro coil, and the batch production of small-sized and large-cross-sectional area coils is realized; the coil does not need to be wound, and the performance requirements of the inductor device can be fully met by simply combining and pressing the coil and the magnetic core of the magnet part, and the coil is not easily deformed or damaged during the processing.

[0004] The reduction in the volume of the inductor device by inductor structure design without sacrificing the saturation current is another innovative way to break through the limitations of traditional magnetic core material performance improvement and meet the high performance and compact size requirements of modern electronic devices for inductor devices. Summary of the invention

[0005] In order to solve the above technical problems, a first aspect of the present invention provides an inductor, including a Tcore model, a winding, a coil, and a metal soft magnetic material.

[0006] In some preferred embodiments, the Tcore model includes a T-shaped planar magnetic core and / or a magnetic core column.

[0007] In some preferred embodiments, the number of windings is ≥1.

[0008] Further preferably, the number of windings is 2.

[0009] Further preferably, the Tcore model includes a T-shaped planar magnetic core.

[0010] More preferably, the Tcore model includes a T-shaped planar magnetic core and a magnetic core column.

[0011] In some preferred embodiments, the magnetic core column is selected from one of a racetrack shape, a circular shape, an elliptical shape, a rectangular shape, and a square shape.

[0012] More preferably, the magnetic core column is of a racetrack type.

[0013] In some preferred embodiments, the coil includes one of a circular coil and a rectangular coil.

[0014] Further preferably, the coil is a rectangular coil.

[0015] In some preferred embodiments, the coil is a rectangular coil; the ratio of the width d of the rectangular coil to the thickness n of the coil is: d / n≤15.

[0016] Further preferably, the ratio of d / n can be listed as: 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, 2, and 1.

[0017] In some preferred embodiments, the coil thickness and the number of turns satisfy the following relationship:

[0018] Coil thickness*number of turns ≤ inductor thickness*9 / 10.

[0019] In some preferred embodiments, the coil width and the magnetic core column height satisfy the following relationship:

[0020] The coil width is ≤ 1 / 2 of the core column height.

[0021] In some preferred embodiments, the metallic soft magnetic material includes at least one of iron silicon, iron silicon aluminum, iron silicon chromium, iron nickel, amorphous alloy, and nanocrystalline alloy.

[0022] Further preferably, the metal soft magnetic material can be used alone, that is, one of iron silicon, iron silicon aluminum, iron silicon chromium, iron nickel, amorphous alloy, and nanocrystalline alloy can be used to fill the Tcore model and obtain an inductor.

[0023] A second aspect of the present invention provides a method for preparing an inductor, comprising the following steps:

[0024] S1: suppress Tcore;

[0025] S2: Wind the coil on Tcore and fix the lead wire of the coil after winding;

[0026] S3: Put the wound Tcore assembly into the mold, fill it with metal soft magnetic material, and perform hot pressing;

[0027] S4: spray paint the hot pressed product;

[0028] S5: Use laser to strip the paint layer at the lead position, then electroplate and tin the lead to obtain the inductor.

[0029] In some preferred embodiments, the lead fixing method includes: folding the lead to the back of the Tcore or pressing the lead to the bottom of the Tcore.

[0030] In some preferred embodiments, the lead fixing method includes: folding the lead to the back of the Tcore.

[0031] In some preferred embodiments, the winding methods in step 3 include α winding and spiral winding.

[0032] In some preferred embodiments, the conditions of the hot pressing are as follows: pressure of 900kg to 1300kg / pcs, temperature of 140 to 200°C, and holding time of 0 to 200s.

[0033] In some preferred embodiments, the hot pressing pressure can be listed as: 900kg / pcs, 920kg / pcs, 930kg / pcs, 950kg / pcs, 980kg / pcs, 1000kg / pcs, 1050kg / pcs, 1110kg / pcs, 1130kg / pcs, 1160kg / pcs, 1200kg / pcs, 1220kg / pcs, 1240kg / pcs, 1270kg / pcs, and 1300kg / pcs.

[0034] In some preferred embodiments, the temperature of the hot pressing is 140°C, 145°C, 150°C, 155°C, 159°C, 162°C, 165°C, 170°C, 175°C, 180°C, 182°C, 186°C, 188°C, 195°C, 197°C, and 200°C.

[0035] In some preferred embodiments, the holding time of the hot pressing is as follows: 0s, 5s, 10s, 15s, 20s, 30s, 40s, 50s, 60s, 70s, 80s, 90s, 100s, 120s, 144s, 150s, 168s, 180s, 186s, 190s, and 200s.

[0036] In some preferred embodiments, the paint layer is an oil-based paint or a water-based paint.

[0037] Further preferably, the color of the paint is gray, black or transparent.

[0038] The paint used in the present invention is common commercially available water-based paint or oil-based paint.

[0039] In some preferred embodiments, the main components of the paint can be listed as: epoxy resin and / or amino resin.

[0040] More preferably, when spray painting the hot pressed product, spray painting is performed on all six sides of the product.

[0041] A third aspect of the present invention provides an application of an inductor for use in a PCB circuit board.

[0042] One or more technical solutions of the present invention have the following beneficial effects:

[0043] 1. The inductor prepared by the present invention can save 35% of the area of ​​the PCB circuit board compared with the traditional 0420-R47 product, and can reduce the volume of the inductor without sacrificing the saturation current, thereby meeting the requirements of modern electronic equipment for high performance and compact size of the inductor.

[0044] 2. The inductor provided by the present invention adopts a specific Tcore model, and when the lead is folded to the back of the Tcore model, it can be ensured that the prepared inductor is stably fixed in the Tcore model after hot pressing, and there will be no looseness when used on a PCB board, thereby ensuring the circuit stability during use. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is a schematic diagram of the Tcore model structure of Example 1, in which: 1-T-type planar magnetic core; 2-magnetic core column.

[0046] Figure 2 This is a schematic diagram of a three-dimensional view of the inductor winding of Example 1;

[0047] Figure 3 This is a schematic diagram of the front view of the inductor winding of Example 1;

[0048] Figure 4 This is a schematic diagram of a rear view of the inductor winding of Example 1;

[0049] Figure 5 It is a schematic diagram of the right side view of the inductor winding of Example 1;

[0050] Figure 6 This is a schematic diagram of a three-dimensional view of the inductor winding of Example 2;

[0051] Figure 7 This is a schematic diagram of the front view of the inductor winding of Example 2;

[0052] Figure 8 This is a schematic diagram of a rear view of the inductor winding of Example 2;

[0053] Fig. 9 It is a schematic diagram of the right side view of the inductor winding of Example 2;

[0054] Fig.10 This is a schematic diagram of a three-dimensional view of the inductor winding of Example 3;

[0055] Fig.11 This is a schematic diagram of the front view of the inductor winding of Example 3;

[0056] Fig.12 This is a schematic diagram of a rear view of the inductor winding of Example 3;

[0057] Fig.13 It is a schematic diagram of the right side view of the inductor winding of Example 3;

[0058] Fig.14 This is a schematic diagram of a three-dimensional view of the inductor winding of Example 4;

[0059] Fig.15 This is a schematic diagram of the front view of the inductor winding of Example 4;

[0060] Fig.16 This is a schematic diagram of a rear view of the inductor winding of Example 4;

[0061] Fig.17 It is a schematic diagram of the right side view of the inductor winding of Example 4;

[0062] Fig.18 It is a schematic diagram of the T-type planar magnetic core structure;

[0063] Fig.19 This is a physical picture of the inductor;

[0064] Fig. 20 The current inductance data diagram of the traditional inductor R47 and an inductor R47 in Example 3, wherein the black line represents the test result of the traditional single inductor; the red line represents the test result of one of the inductors R47 in Example 3;

[0065] Fig.21 1 is a curve diagram of the inductance change rate of a traditional inductor R47 and an inductor R47 in Example 3, wherein the black line represents the test result of a traditional single inductor; the red line represents the test result of one of the inductors R47 in Example 3;

[0066] Fig. 22 1 is a quality factor Q curve of a traditional inductor R47 and an inductor R47 in Example 3, wherein the black line represents the test result of a traditional single inductor; the blue line represents the test result of one of the inductors R47 in Example 3. DETAILED DESCRIPTION

[0067] Example

[0068] Embodiment 1 (the winding method is α winding, and the winding directions of the two windings are the same)

[0069] An inductor comprises a Tcore model, a winding, a coil, and a metal soft magnetic material. The Tcore model comprises a T-shaped planar magnetic core 1 and a magnetic core column 2.

[0070] The number of windings is 2;

[0071] The magnetic core column is in a racetrack shape;

[0072] The metal soft magnetic material is a mixed powder of amorphous alloy and iron-nickel, and the weight ratio of the amorphous alloy to iron-nickel is 3.5:6.5;

[0073] The coil is a rectangular coil;

[0074] The ratio of the rectangular coil width d (0.6 mm) to the coil thickness n (0.3 mm) is 2:1;

[0075] The relationship between coil thickness and number of turns is as follows:

[0076] a. Coil thickness*number of turns (4 turns)=1.2mm<inductor thickness (3.0mm)*9 / 10;

[0077] b. The height of the magnetic core column is: 1.35mm; the coil width (0.6mm) is less than 1 / 2 of the height of the magnetic core column

[0078] A second aspect of the present invention provides a method for preparing an inductor, comprising the following steps:

[0079] S1: suppress Tcore;

[0080] S2: Wrap the coil around the Tcore, and after winding is completed, fix the lead wire of the coil to the back of the Tcore;

[0081] S3: Put the wound Tcore assembly into the mold, fill it with metal soft magnetic material, and perform hot pressing;

[0082] S4: spray paint the hot pressed product;

[0083] S5: Use laser to strip the paint layer at the lead position, then electroplate and tin the lead to obtain the inductor.

[0084] The hot pressing conditions are as follows: pressure of 1200 kg, temperature of 165° C., and holding time of 120 s.

[0085] Embodiment 2 (the winding method is α winding, and the winding directions of the two windings are opposite)

[0086] An inductor comprises a Tcore model, a winding, a coil, and a metal soft magnetic material. The Tcore model comprises a T-shaped planar magnetic core 1 and a magnetic core column 2.

[0087] The number of windings is 2;

[0088] The magnetic core column is elliptical;

[0089] The metal soft magnetic material is a mixed powder of amorphous alloy and iron-nickel, and the weight ratio of the amorphous alloy to iron-nickel is 3.5:6.5;

[0090] The coil is a rectangular coil;

[0091] The ratio of the rectangular coil width d (0.6 mm) to the coil thickness n (0.3 mm) is 2:1;

[0092] The relationship between coil thickness and number of turns is as follows:

[0093] a. Coil thickness*number of turns (4 turns)=1.2mm<inductor thickness (3.0mm)*9 / 10;

[0094] b. The height of the magnetic core column is: 1.35mm; the coil width (0.6mm) is less than 1 / 2 of the height of the magnetic core column

[0095] A second aspect of the present invention provides a method for preparing an inductor, comprising the following steps:

[0096] S1: suppress Tcore;

[0097] S2: Wrap the coil around the Tcore, and after winding is completed, fix the lead wire of the coil to the back of the Tcore;

[0098] S3: Put the wound Tcore assembly into the mold, fill it with metal soft magnetic material, and perform hot pressing;

[0099] S4: spray paint the hot pressed product;

[0100] S5: Use laser to strip the paint layer at the lead position, then electroplate and tin the lead to obtain the inductor.

[0101] The conditions of the hot pressing are as follows: pressure is 900kg-1300kg / pcs, temperature is 140-200°C (170+ / -30°C), and holding time is 0-200s.

[0102] Embodiment 3 (the winding method is spiral winding, and the winding directions of the two windings are the same)

[0103] An inductor comprises a Tcore model, a winding, a coil, and a metal soft magnetic material. The Tcore model comprises a T-shaped planar magnetic core 1 and a magnetic core column 2.

[0104] The number of windings is 2;

[0105] The magnetic core column is in a racetrack shape;

[0106] The metal soft magnetic material is a mixed powder of amorphous alloy and iron-nickel, and the weight ratio of the amorphous alloy to iron-nickel is 3.5:6.5;

[0107] The coil is a rectangular coil;

[0108] The ratio of the rectangular coil width d (0.6 mm) to the coil thickness n (0.3 mm) is 2:1;

[0109] The relationship between coil thickness and number of turns is as follows:

[0110] a. Coil thickness n*number of turns h (4 turns) is 1.38~1.42mm;

[0111] Inductor thickness H (3.0mm) * 9 / 10;

[0112] A second aspect of the present invention provides a method for preparing an inductor, comprising the following steps:

[0113] S1: suppress Tcore;

[0114] S2: Wrap the coil around the Tcore, and after winding is completed, fix the lead wire of the coil to the back of the Tcore;

[0115] S3: Put the wound Tcore assembly into the mold, fill it with metal soft magnetic material, and perform hot pressing;

[0116] S4: spray paint the hot pressed product;

[0117] S5: Use laser to strip the paint layer at the lead position, then electroplate and tin the lead to obtain the inductor.

[0118] The hot pressing conditions are as follows: pressure is 1250 kg / pcs, temperature is 170° C., and holding time is 120 s.

[0119] Embodiment 4 (the winding method is spiral winding, and the winding directions of the two windings are opposite)

[0120] An inductor comprises a Tcore model, a winding, a coil, and a metal soft magnetic material. The Tcore model comprises a T-shaped planar magnetic core 1 and a magnetic core column 2.

[0121] The number of windings is 2;

[0122] The magnetic core column is elliptical;

[0123] The metal soft magnetic material is a mixed powder of amorphous alloy and iron-nickel, and the weight ratio of the amorphous alloy to iron-nickel is 3.5:6.5;

[0124] The coil is a rectangular coil;

[0125] The ratio of the rectangular coil width d (0.6 mm) to the coil thickness n (0.3 mm) is 2:1;

[0126] The relationship between coil thickness and number of turns is as follows:

[0127] a. Coil thickness n*number of turns h (4 turns) is 1.38~1.42mm;

[0128] Inductor thickness H (3.0mm) * 9 / 10;

[0129] A second aspect of the present invention provides a method for preparing an inductor, comprising the following steps:

[0130] S1: suppress Tcore;

[0131] S2: Wrap the coil around the Tcore, and after winding is completed, fix the lead wire of the coil to the back of the Tcore;

[0132] S3: Put the wound Tcore assembly into the mold, fill it with metal soft magnetic material, and perform hot pressing;

[0133] S4: spray paint the hot pressed product;

[0134] S5: Use laser to strip the paint layer at the lead position, then electroplate and tin the lead to obtain the inductor.

[0135] The conditions of the hot pressing are as follows: pressure is 900kg-1300kg / pcs, temperature is 140-200°C (170+ / -30°C), and holding time is 0-200s.

[0136] Example 5

[0137] The specific implementation of Example 5 of the present application is the same as that of Example 1, and the difference from Example 1 is that the coil is a circular coil.

[0138] Example 6

[0139] The specific implementation of Example 6 of the present application is the same as that of Example 1, and the difference from Example 1 is that there is only one winding.

[0140] Performance Testing:

[0141] 1. The inductor prepared above is used in a PCB circuit board, and the circuit board area saved is shown in the following Table 1:

[0142] Table 1:

[0143]

[0144] 2. The inductance of one of the inductors R47 in Example 3 and the traditional single inductor R47 are measured, and the current and inductance data are shown in the figure. Fig. 20 , inductance value change rate curve diagram see Fig.21 , quality factor Q curve see Fig. 22 .

Claims

1. An inductor, characterized in that: It includes a Tcore model, a winding, a coil, and a metal soft magnetic material; the Tcore model includes a T-shaped planar magnetic core and / or a magnetic core column; The number of the magnetic core columns=the number of windings.

2. The inductor according to claim 1, characterized in that The magnetic core column is selected from one of a racetrack shape, a circular shape, an elliptical shape, a rectangular shape, and a square shape.

3. The inductor according to claim 1, wherein: The coil includes one of a circular coil and a rectangular coil.

4. The inductor according to claim 3, characterized in that The coil is a rectangular coil; the ratio of the width d of the rectangular coil to the thickness n of the coil is: d / n≤15.

5. The inductor according to claim 3 or 4, characterized in that: The relationship between coil thickness and number of turns is as follows: Coil thickness*number of turns ≤ inductor thickness*9 / 10.

6. The inductor according to claim 1 or 2, characterized in that: The metal soft magnetic material includes at least one of iron silicon, iron silicon aluminum, iron silicon chromium, iron nickel, amorphous alloy, and nanocrystalline alloy.

7. A method for preparing an inductor according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1: suppress Tcore; S2: Wind the coil on Tcore and fix the lead wire of the coil after winding; S3: Put the wound Tcore assembly into the mold, fill it with metal soft magnetic material, and perform hot pressing; S4: spray paint the hot pressed product; S5: Use laser to strip the paint layer at the lead position, then electroplate and tin the lead to obtain the inductor.

8. The method for preparing an inductor according to claim 7, characterized in that: The lead fixing method includes: folding the lead to the back of the Tcore or pressing the lead to the bottom of the Tcore.

9. The method for preparing an inductor according to claim 7, characterized in that: The conditions of the hot pressing are as follows: pressure of 900kg to 1300kg / pcs, temperature of 140 to 200°C, and holding time of 0 to 200s.

10. Use of the inductor according to any one of claims 1 to 6, characterized in that: Used for PCB circuit boards.