Formation method of semiconductor structure
By forming a protective layer on the exposed end of the hard mask opening and performing an etching process, the problem of hard mask layer damage and adjacent gate exposure is solved, and the performance of the semiconductor structure and the formation quality of the isolation structure are improved.
Patent Information
- Application Number
- CN202310325968.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
In the semiconductor manufacturing process, the traditional single-diffusion isolation process can easily cause damage to the hard mask layer and exposure of the adjacent gate structure, affecting the formation of the isolation structure and semiconductor performance.
The first protective layer is formed on the exposed end of the hard mask opening, and the gate structure at the bottom of the mask opening is removed through an isotropic etching process to form an isolation opening, thereby reducing the probability of damage to the hard mask layer, thereby reducing the risk of damage to the hard mask layer. The impact of small partition structures on adjacent gate structures.
It effectively reduces the risk of damage to the hard mask layer and exposure of the adjacent gate structure, and improves the performance of the semiconductor structure and the formation quality of the isolation structure.
Smart Images

Figure CN118737962A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the field of semiconductor manufacturing, and in particular to a method for forming a semiconductor structure. Background Art
[0002] With the rapid development of semiconductor manufacturing technology, semiconductor devices are moving towards higher component density and higher integration. Transistors, as one of the basic semiconductor devices, are currently being widely used. Therefore, with the increase in density and integration of semiconductor devices, the gate size of planar transistors is getting shorter and shorter. The control ability of traditional planar transistors over channel current becomes weaker, resulting in short channel effects, causing leakage current to increase, and ultimately affecting the electrical performance of semiconductor devices.
[0003] In order to better adapt to the reduction of feature size, semiconductor processes have gradually begun to transition from planar MOSFET to three-dimensional transistors with higher efficiency, such as fin field effect transistors (FinFET). In FinFET, the gate can control the ultra-thin body (fin) from at least two sides. Compared with planar MOSFET, the gate has stronger control over the channel and can effectively suppress the short channel effect; and FinFET has better compatibility with existing integrated circuit manufacturing than other devices.
[0004] However, as the size of semiconductor devices continues to shrink, process nodes are also shrinking. In order to improve the process density of devices, the Single Diffusion Break (SDB) process is introduced to achieve the isolation of adjacent device units and prevent bridging between adjacent devices. Summary of the invention
[0005] The problem solved by the embodiments of the present invention is to provide a method for forming a semiconductor structure to improve the performance of the semiconductor structure.
[0006] To solve the above problems, an embodiment of the present invention further provides a method for forming a semiconductor structure, comprising: providing a substrate, the substrate including an isolation region, a gate structure formed on the substrate, an interlayer dielectric layer formed on the substrate on the side of the gate structure, the top of the gate structure and the interlayer dielectric layer covered with a hard mask structure, the hard mask structure is a stacked structure, and includes a hard mask layer closest to the top of the gate structure; forming a mask opening at the top of the gate structure located in the isolation region in the hard mask structure; forming a first protective layer at the end of the hard mask layer exposed by the mask opening; after forming the first protective layer, removing the gate structure at the bottom of the mask opening and a portion of the thickness of the substrate along the mask opening to form an isolation opening; and forming a partition structure in the isolation opening.
[0007] Optionally, after forming a mask opening at the top of the gate structure located in the isolation region in the hard mask structure, and before forming a first protective layer at the end of the hard mask layer exposed by the mask opening, the method further includes: laterally removing a portion of the width of the hard mask layer along a direction perpendicular to the side wall of the mask opening to form an inner groove in the hard mask structure, wherein the inner groove is connected to the mask opening; in the step of forming the first protective layer at the end of the hard mask layer exposed by the mask opening, the first protective layer is formed in the inner groove.
[0008] Optionally, in the process of laterally removing a portion of the width of the hard mask layer along a direction perpendicular to the sidewall of the mask opening, a portion of the thickness of the gate structure at the bottom of the mask opening is also removed.
[0009] Optionally, the process of laterally removing a portion of the width of the hard mask layer along a direction perpendicular to the sidewall of the mask opening includes an isotropic etching process.
[0010] Optionally, the isotropic etching process is a wet etching process, and the wet etching process uses a hydrogen peroxide solution and a hydrochloric acid solution in sequence, the temperature of the hydrogen peroxide solution is 60 degrees Celsius to 80 degrees Celsius, the treatment time of the hydrogen peroxide solution is 50 seconds to 100 seconds, the temperature of the hydrochloric acid solution is room temperature, and the treatment time of the hydrochloric acid solution is 10 seconds to 20 seconds.
[0011] Optionally, along a direction perpendicular to the sidewall of the mask opening, a lateral depth of the inner groove is 50 angstroms to 100 angstroms.
[0012] Optionally, the step of forming a first protective layer at the end of the hard mask layer exposed by the mask opening includes: depositing a monolayer precursor on the side walls of the mask opening, the inner walls of the inner groove, the top of the hard mask structure, and the gate structure at the bottom of the mask opening, wherein the monolayer precursor covers the end of the hard mask layer, the monolayer precursor has a hydrophobic group, and the hydrophobic group of the monolayer precursor faces away from the side walls of the mask opening, the inner walls of the inner groove, the top of the hard mask structure, and the gate structure at the bottom of the mask opening; performing plasma bombardment treatment on the monolayer precursor to decompose the monolayer precursor located on the side walls of the mask opening, the top of the hard mask structure, and the gate structure at the bottom of the mask opening to obtain a monolayer, and the remaining monolayer precursor located in the inner groove serves as the first protective layer.
[0013] Optionally, in the step of forming a monolayer precursor, the monolayer precursor also has hydrophilic groups, and the hydrophilic groups of the monolayer precursor are adsorbed on the side walls of the mask opening, the inner walls of the inner groove, the top of the hard mask structure, and the gate structure at the bottom of the mask opening.
[0014] Optionally, in the step of forming a monolayer precursor, the monolayer precursor includes an alkylamine complex.
[0015] Optionally, in the step of forming a monolayer precursor, the alkylamine complex includes one or both of a long-chain alkylamine complex and an alkylamine complex containing an aromatic ring.
[0016] Optionally, in the step of forming a monolayer precursor, the monolayer precursor also includes a metal element; in the step of bombarding the monolayer precursor, the monolayer obtained by decomposing the monolayer precursor is a metal nitride layer.
[0017] Optionally, plasma bombardment treatment is performed under bias voltage conditions, and the parameters of the plasma bombardment treatment include: the bombardment gas includes one or both of argon and hydrogen, the bias voltage is 150 volts to 200 volts, the process temperature is 200 degrees Celsius to 300 degrees Celsius, and the process time is 5 seconds to 10 seconds.
[0018] Optionally, after forming the first protection layer at the end of the hard mask layer exposed by the mask opening and before forming the isolation opening, the method further includes: forming a second protection layer covering the first protection layer on the sidewall of the mask opening.
[0019] Optionally, the step of forming a second protective layer covering the first protective layer includes: forming a second protective material layer on the side walls of the mask opening, the side walls of the first protective layer, the top of the hard mask structure, and the bottom of the mask opening; removing the top of the hard mask structure and the second protective material layer at the bottom of the mask opening, and the remaining second protective material layer serves as the second protective layer.
[0020] Optionally, in the step of removing the gate structure at the bottom of the mask opening along the mask opening, the process of removing the gate structure at the bottom of the mask opening includes: a wet etching process.
[0021] Optionally, in the step of providing a substrate, the hard mask layer is a metal hard mask layer.
[0022] Optionally, the material of the hard mask layer includes titanium nitride or aluminum nitride.
[0023] Optionally, the step of forming a partition structure in the isolation opening includes: filling the isolation opening with insulating material through the mask opening, the insulating material also filling the mask opening and covering the top of the hard mask structure; removing the insulating material above the gate structure and the top of the interlayer dielectric layer, and the remaining insulating material in the isolation opening serves as the partition structure.
[0024] Compared with the prior art, the technical solution of the embodiment of the present invention has the following advantages:
[0025] In the method for forming a semiconductor structure provided by an embodiment of the present invention, a first protective layer is formed at the end of the hard mask layer exposed by the mask opening; the first protective layer can protect the hard mask layer in the process of removing the gate structure at the bottom of the mask opening along the mask opening to form an isolation opening, thereby reducing the probability of the hard mask layer being damaged and causing gaps, thereby reducing the risk of adjacent gate structures being exposed due to the gaps in the hard mask layer, and correspondingly reducing the probability of adjacent gate structures being damaged through the gaps in the hard mask layer in the process of removing the gate structure at the bottom of the mask opening along the mask opening, thereby reducing the influence of the formation of the partition structure on the adjacent gate structure and improving the performance of the semiconductor structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figures 1 to 3 It is a schematic structural diagram corresponding to each step in a method for forming a semiconductor structure;
[0027] Figure 4 It is a schematic structural diagram corresponding to each step in another method for forming a semiconductor structure;
[0028] Figures 5 to 14 It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor structure of the present invention. DETAILED DESCRIPTION
[0029] As can be seen from the background art, currently, in order to realize the isolation of adjacent device units, a single diffusion isolation process is introduced. However, the formation of a single diffusion isolation structure is likely to cause adverse effects on other film layers, thereby causing the performance of the semiconductor structure to deteriorate.
[0030] Combined with a method for forming a semiconductor structure, reasons why the performance of the semiconductor structure needs to be improved are analyzed. Figures 1 to 3 The present invention is a schematic structural diagram corresponding to each step in a method for forming a semiconductor structure.
[0031] refer to Figure 1 A substrate 10 is provided, the substrate 10 includes an isolation region i, a gate structure 20 is formed on the substrate 10, an interlayer dielectric layer 30 is formed on the substrate 10 at the side of the gate structure 20, the top of the gate structure 20 and the interlayer dielectric layer 30 are covered with a hard mask structure 40, the hard mask structure 40 is a stacked structure, and includes a hard mask layer 41 closest to the top of the gate structure 20.
[0032] refer to Figure 2 , the hard mask structure 40 located on the top of the gate structure 20 in the isolation region i is removed, and a mask opening 45 is formed in the hard mask structure 40 .
[0033] refer to Figure 3, along the mask opening 45 , the gate structure 20 at the bottom of the mask opening 45 and a portion of the thickness of the substrate 10 are removed to form an isolation opening 50 .
[0034] However, if Figure 3 As shown, if a wet etching process is used to remove the gate structure 20 at the bottom of the mask opening 45 to form an isolation opening 50, the hard mask layer 41 closest to the gate structure 20 may be damaged and a gap 42 may be generated when the gate structure 20 at the bottom of the mask opening 45 is removed. Correspondingly, the adjacent gate structure 20 may be exposed due to the gap 42, thereby increasing the probability that the adjacent gate structure 20 is damaged in the process of forming the isolation opening 50.
[0035] Therefore, in order to improve the above problem, it is proposed to use a dry etching process to remove the gate structure 20' (eg Figure 4 However, due to the fact that the aspect ratio of the isolation opening 50' to be formed is often large and the flatness of the sidewall of the gate structure 20' is poor, it is easy to make it difficult to completely remove the gate structure 20' by the dry etching process, that is, it is easy to leave residues of the gate structure 20' on the sidewall of the isolation opening 50', which is easy to affect the formation quality of the partition structure formed subsequently.
[0036] In order to solve the above technical problems, an embodiment of the present invention provides a method for forming a semiconductor structure, including: providing a substrate, the substrate including an isolation region, a gate structure formed on the substrate, an interlayer dielectric layer formed on the substrate on the side of the gate structure, the top of the gate structure and the interlayer dielectric layer is covered with a hard mask structure, the hard mask structure is a stacked structure, and includes a hard mask layer closest to the top of the gate structure; forming a mask opening at the top of the gate structure located in the isolation region in the hard mask structure; forming a first protective layer at the end of the hard mask layer exposed by the mask opening; after forming the first protective layer, removing the gate structure at the bottom of the mask opening and a portion of the thickness of the substrate along the mask opening to form an isolation opening; and forming a partition structure in the isolation opening.
[0037] In the method for forming a semiconductor structure provided by an embodiment of the present invention, a first protective layer is formed at the end of the hard mask layer exposed by the mask opening; the first protective layer can protect the hard mask layer in the process of removing the gate structure at the bottom of the mask opening along the mask opening to form an isolation opening, thereby reducing the probability of the hard mask layer being damaged and causing gaps, thereby reducing the risk of adjacent gate structures being exposed due to the gaps in the hard mask layer, and correspondingly reducing the probability of adjacent gate structures being damaged through the gaps in the hard mask layer in the process of removing the gate structure at the bottom of the mask opening along the mask opening, thereby reducing the influence of the formation of the partition structure on the adjacent gate structure and improving the performance of the semiconductor structure.
[0038] In order to make the above-mentioned purposes, features and advantages of the embodiments of the present invention more obvious and understandable, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings. Figures 5 to 14 It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor structure of the present invention.
[0039] refer to Figure 5 A substrate 100 is provided, the substrate 100 includes an isolation region I, a gate structure 200 is formed on the substrate 100, an interlayer dielectric layer 110 is formed on the substrate 100 at the side of the gate structure 200, the top of the gate structure 200 and the interlayer dielectric layer 110 are covered with a hard mask structure 120, the hard mask structure 120 is a stacked structure, and includes a hard mask layer 121 closest to the top of the gate structure 200.
[0040] The substrate 100 is used to provide a process platform for subsequent process steps.
[0041] In this embodiment, the substrate 100 is used to form a field effect transistor. As an example, the substrate 100 is used to form a fin field effect transistor.
[0042] In this embodiment, the base 100 includes a substrate 101, and the substrate 101 is a silicon substrate. In other embodiments, the material of the substrate can also be other materials such as germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium, and the substrate can also be other types of substrates such as a silicon substrate on an insulator or a germanium substrate on an insulator.
[0043] It should be noted that the substrate may be a planar substrate or a substrate having a channel-convex structure.
[0044] In this embodiment, the substrate 100 is used to form a fin field effect transistor (FinFET). The substrate 100 includes a substrate 101 and a channel protrusion structure 102 protruding from the substrate 101, wherein the channel protrusion structure 102 is a fin.
[0045] The channel protrusion structure 102 protrudes from the substrate 101 , so that the gate structure 200 can cross the channel protrusion structure 102 and cover the top and part of the sidewall of the channel protrusion structure 102 .
[0046] As an example, the substrate 101 and the channel protrusion structure 102 are an integrated structure.
[0047] The isolation region I is a region where a partition structure is subsequently formed, and the gate structure 200 in the isolation region I is removed in a subsequent process.
[0048] In this embodiment, in the step of providing the substrate 100 , source-drain doped layers 300 are formed in the substrate 100 on both sides of the gate structure 200 . Specifically, source-drain doped layers 300 are formed in the channel protrusion structures 102 on both sides of the gate structure 200 .
[0049] The source-drain doped layer 300 is used as the source region and the drain region of the transistor. When the device is working, the source-drain doped layer 300 is used to provide a carrier source.
[0050] The gate structure 200 is used to form a field effect transistor together with the channel protrusion structure 102 and the source-drain doped layer 300 .
[0051] In this embodiment, a gate structure 200 is also formed on the substrate 100 of the isolation region I. The gate structure 200 of the isolation region I can play the role of a pseudo gate structure, which is beneficial to improving process reliability.
[0052] In this embodiment, the gate structure 200 is a device gate structure.
[0053] The gate structure 200 includes a gate dielectric layer (not shown) and a gate electrode layer (not shown) covering the gate dielectric layer.
[0054] The gate dielectric layer is used to isolate the gate electrode layer from the channel protrusion structure 102 .
[0055] In this embodiment, the gate structure 200 is a metal gate structure, and therefore, the material of the gate electrode layer includes one or more of TiN, TaN, Ta, Ti, TiAl, W, Al, TiSiN and TiAlC. The gate electrode layer includes a work function layer and an electrode layer covering the work function layer, or may include only the work function layer.
[0056] Correspondingly, the gate dielectric layer includes a high-k gate dielectric layer. The material of the high-k gate dielectric layer is a high-k dielectric material, and the high-k dielectric material refers to a dielectric material having a relative dielectric constant greater than the relative dielectric constant of silicon oxide. Specifically, the material of the high-k gate dielectric layer can be selected from HfO2, ZrO2, HfSiO, HfSiON, HfTaO, HfTiO, HfZrO or Al2O3, etc.
[0057] In other embodiments, the gate structure may also be a polysilicon gate structure.
[0058] In this embodiment, in the step of providing the substrate 100 , a sidewall spacer 210 is formed on the sidewall of the gate structure 200 .
[0059] The sidewall spacer 210 is used to protect the sidewall of the device gate structure. The sidewall spacer 210 can be a single-layer structure or a stacked structure, and the material of the sidewall spacer 210 includes one or more of silicon oxide, silicon nitride, silicon carbide, silicon carbonitride, silicon carbonitride oxide, silicon oxynitride, boron nitride and boron carbonitride.
[0060] The interlayer dielectric layer 110 is used to isolate adjacent devices. The material of the interlayer dielectric layer 110 is an insulating material, for example, one or more of silicon oxide, silicon nitride, silicon oxynitride, silicon oxycarbide, silicon carbonitride and silicon carbon oxynitride. In this embodiment, the material of the interlayer dielectric layer 110 is silicon oxide.
[0061] The hard mask structure 120 is used to protect the gate structure 200 in other areas except the isolation region I in the subsequent process of forming a mask opening at the top of the gate structure 200 located in the isolation region I in the hard mask structure 120 and removing the gate structure 200 at the bottom of the mask opening.
[0062] The hard mask structure 120 is a stacked structure, which helps to reduce the difficulty of subsequently forming a mask opening in the hard mask structure 120 .
[0063] Specifically, the hard mask layer 121 is a metal hard mask layer. The subsequent process of forming the partition structure includes a step of using a planarization process to remove the insulating material above the gate structure 200 and the top of the interlayer dielectric layer 110. The metal hard mask layer has a high hardness. In the subsequent process of removing the insulating material above the gate structure 200 and the top of the interlayer dielectric layer 110, the surface of the interlayer dielectric layer 110 is not prone to dishing, which is beneficial to improving the surface flatness of the interlayer dielectric layer 110, which is correspondingly beneficial to controlling the height of the source-drain interconnection layer formed subsequently, and further beneficial to improving the performance of the semiconductor structure.
[0064] As an example, the material of the hard mask layer 121 includes titanium nitride or aluminum nitride.
[0065] In this embodiment, the hard mask layer 121 serves as a first mask layer, and the hard mask structure 120 includes the first mask layer, a second mask layer 122 covering the first mask layer, and a third mask layer 123 covering the second mask layer 122 .
[0066] The top of the hard mask layer 121 is covered with a second mask layer 122 and a third mask layer 123, which is beneficial to reducing the probability of damage to the hard mask layer 121 on the top of the adjacent gate structure 200 during the subsequent lateral removal of a portion of the width of the hard mask layer 121 along a direction perpendicular to the side wall of the mask opening.
[0067] In this embodiment, the material of the second mask layer 122 includes silicon nitride, and the material of the third mask layer 123 includes silicon oxide.
[0068] It should be noted that a photoresist layer (not shown) may be formed on the top of the third mask layer 123, and the mask opening 125 may be formed by patterning the photoresist layer and then etching the hard mask structure 120. The photoresist layer is formed on the top of the silicon oxide layer, which is conducive to exposing the photoresist layer.
[0069] It is also necessary to explain that covering the top of the hard mask layer 121 with a silicon nitride layer makes it easy to combine the subsequent chemical mechanical planarization treatment with the existing process flow to improve process compatibility and reduce costs when removing the insulating material above the gate structure 200 and the top of the interlayer dielectric layer 110.
[0070] refer to Figure 6 , a mask opening 125 located at the top of the gate structure 200 in the isolation region I is formed in the hard mask structure 120.
[0071] The mask opening 125 is used to provide a process basis for subsequently forming an isolation opening, and is also used to subsequently form a partition structure in the isolation opening through the mask opening 125 .
[0072] As an example, an anisotropic etching process is used to etch the hard mask structure 120 of the isolation region I to form a mask opening 125. The anisotropic etching process is used to improve the morphology quality and dimensional accuracy of the mask opening 125. For example, the anisotropic etching process is a plasma dry etching process.
[0073] refer to Figure 7 In this embodiment, after forming a mask opening 125 at the top of the gate structure 200 located in the isolation region I in the hard mask structure 120, before forming a first protective layer at the end of the hard mask layer 121 exposed by the mask opening 125, it also includes: laterally removing a portion of the width of the hard mask layer 121 along a direction perpendicular to the side wall of the mask opening 125, forming an inner groove 126 in the hard mask structure 120, and the inner groove 126 is connected to the mask opening 125.
[0074] The inner groove 126 is used to provide a spatial position for the subsequent formation of the first protective layer. Compared with the end of the hard mask layer 121, the surface area of the inner groove 126 is larger, which is conducive to improving the formation quality of the first protective layer, and further to improving the degree of protection of the first protective layer to the hard mask layer 121. In addition, the inner groove 126 has a certain lateral depth, which is convenient for the lateral width of the first protective layer to meet the process requirements. Thirdly, the end of the hard mask layer 121 exposed by the inner groove 126 is recessed inward relative to the side wall of the mask opening 125, which is convenient for the subsequent retention of the first protective layer in the inner groove 126.
[0075] Specifically, in the process of laterally removing a portion of the width of the hard mask layer 121 along a direction perpendicular to the sidewall of the mask opening 125 , a portion of the thickness of the gate structure 200 at the bottom of the mask opening 125 is also removed.
[0076] In the process of laterally removing a portion of the width of the hard mask layer 121, a portion of the thickness of the gate structure 200 at the bottom of the mask opening 125 is also removed, thereby reducing the thickness of the gate structure 200 that needs to be removed in the subsequent process of removing the gate structure 200 at the bottom of the mask opening 125, thereby easily reducing the probability of damage to the hard mask layer 121 during the process of removing the gate structure 200 at the bottom of the mask opening 125.
[0077] In this embodiment, the hard mask layer 121 is a metal hard mask layer and the gate structure 200 is a metal gate structure. Therefore, it is easy to remove a portion of the thickness of the gate structure 200 at the bottom of the mask opening 125 during the process of laterally removing a portion of the width of the hard mask layer 121 .
[0078] It should be noted that the lateral depth of the inner groove 126 should not be too large or too small along the direction perpendicular to the side wall of the mask opening 125. If the lateral depth of the inner groove 126 is too large, the probability of damage to the hard mask layer 121 at the top of the adjacent gate structure 200 is increased during the process of forming the inner groove 126 in the hard mask structure 120, which may easily lead to the top of the adjacent gate structure 200 being exposed; if the lateral depth of the inner groove 126 is too small, the surface area of the inner groove 126 is correspondingly small, which may easily lead to poor formation quality of the first protective layer formed subsequently, and further make the protective effect of the first protective layer on the hard mask layer 121 unsatisfactory. Therefore, in this embodiment, the lateral depth of the inner groove 126 along the direction perpendicular to the side wall of the mask opening 125 is 50 angstroms to 100 angstroms.
[0079] It should also be noted that the process of laterally removing a portion of the width of the hard mask layer 121 along a direction perpendicular to the sidewall of the mask opening 125 includes an isotropic etching process; as an example, the isotropic etching process is a wet etching process.
[0080] The cost of the wet etching process is relatively low, and the operation steps are simple. It can also achieve a large etching selectivity ratio, which is beneficial to reduce the damage to other film layers (for example, the sidewall 210) during the process of lateral removal of a portion of the width of the hard mask layer 121. In addition, the wet etching process has the characteristic of isotropic etching, so that a portion of the width of the hard mask layer 121 can be lateral removed.
[0081] Among them, the wet etching process uses hydrogen peroxide solution and hydrochloric acid solution in sequence. The temperature of the hydrogen peroxide solution is 60 degrees Celsius to 80 degrees Celsius, the processing time of the hydrogen peroxide solution is 50 seconds to 100 seconds, the temperature of the hydrochloric acid solution is room temperature, and the processing time of the hydrochloric acid solution is 10 seconds to 20 seconds.
[0082] Hydrogen peroxide solution and hydrochloric acid solution can remove different types of impurities, such as oxides, metal ions or organic matter, and hydrogen peroxide solution and hydrochloric acid solution are commonly used solutions in wet etching processes, which can be easily combined with existing process steps to reduce process costs.
[0083] The process temperature of the wet etching process should not be too high or too low. If the process temperature of the wet etching process is too high, it is easy to cause the etching selectivity to deteriorate, thereby increasing the probability of causing damage to other film layers; if the process temperature of the wet etching process is too low, it is easy to cause the etching rate to be too low, which is not conducive to improving the etching efficiency. Therefore, in this embodiment, the temperature of the hydrogen peroxide solution is 60 degrees Celsius to 80 degrees Celsius, and the temperature of the hydrochloric acid solution is room temperature.
[0084] The process time of the wet etching process should not be too long or too short. If the process time of the wet etching process is too long, it is easy for other film layers to be exposed to the etching solution for too long, which is easy to increase the probability of damage to other film layers, and it is also easy to cause the lateral depth of the inner groove 126 to be too large; if the process time of the wet etching process is too short, it is easy to make the lateral depth of the inner groove 126 smaller, and correspondingly make the surface area of the inner groove 126 smaller, which is easy to make the formation quality of the first protective layer formed subsequently poor, and then make the first protective layer The protective effect of the hard mask layer 121 is not ideal. Therefore, in this embodiment, the treatment time of the hydrogen peroxide solution is 50 seconds to 100 seconds, and the treatment time of the hydrochloric acid solution is 10 seconds to 20 seconds.
[0085] refer to Figures 8 to 9 , a first protection layer 130 is formed at the end of the hard mask layer 121 exposed by the mask opening 125 .
[0086] A first protective layer 130 is formed at the end of the hard mask layer 121 exposed by the mask opening 125; the first protective layer 130 can protect the hard mask layer 121 in the process of removing the gate structure 200 at the bottom of the mask opening 125 along the mask opening 125 to form an isolation opening, thereby reducing the probability of the hard mask layer 121 being damaged and causing a gap, thereby reducing the risk of the adjacent gate structure 200 being exposed due to the gap in the hard mask layer 121, and correspondingly reducing the probability of the adjacent gate structure 200 being damaged through the gap in the hard mask layer 121 in the process of removing the gate structure 200 at the bottom of the mask opening 125 along the mask opening 125, thereby reducing the influence of the formation of the partition structure on the adjacent gate structure 200 and improving the performance of the semiconductor structure.
[0087] In this embodiment, after forming a mask opening 125 at the top of the gate structure 200 in the isolation region I in the hard mask structure 120, before forming a first protective layer at the end of the hard mask layer 121 exposed by the mask opening 125, the method further includes: removing a portion of the width of the hard mask layer 121 laterally along a direction perpendicular to the sidewall of the mask opening 125, and forming an inner groove 126 in the hard mask structure 120, wherein the inner groove 126 is connected to the mask opening 125. Accordingly, in the step of forming the first protective layer 130 at the end of the hard mask layer 121 exposed by the mask opening 125, the first protective layer 130 is formed in the inner groove 126.
[0088] Compared with the end of the hard mask layer 121, the surface area of the inner groove 126 is larger, which is beneficial to improving the quality of the first protective layer 130 formed in the inner groove 126, and correspondingly improves the degree of protection of the first protective layer 130 to the hard mask layer 121, thereby further reducing the probability of the hard mask layer 121 being damaged and causing a gap in the process of removing the gate structure 200 at the bottom of the mask opening 125 to form an isolation opening, and further reducing the risk of the adjacent gate structure 200 being exposed due to the gap in the hard mask layer 121, thereby further reducing the probability of the adjacent gate structure 200 being damaged through the gap in the hard mask layer 121 in the process of removing the gate structure 200 at the bottom of the mask opening 125 along the mask opening 125.
[0089] In this embodiment, the step of forming the first protective layer 130 at the end of the hard mask layer 121 exposed by the mask opening 125 includes: depositing a monolayer precursor 131 on the sidewalls of the mask opening 125, the inner wall of the inner groove 126, the top of the hard mask structure 120, and the gate structure 200 at the bottom of the mask opening 125, wherein the monolayer precursor 131 covers the end of the hard mask layer 121, and the monolayer precursor 131 has a hydrophobic group, and the hydrophobic group of the monolayer precursor 131 faces away from the mask opening. The side walls of the mask opening 125, the inner walls of the inner groove 126, the top of the hard mask structure 120, and the gate structure 200 at the bottom of the mask opening 125 are formed; the monolayer precursor 131 is subjected to plasma bombardment treatment to decompose the monolayer precursor 131 located on the side walls of the mask opening 125, the top of the hard mask structure 120, and the gate structure 200 at the bottom of the mask opening 125 to obtain a monolayer 132, and the remaining monolayer precursor 131 located in the inner groove 126 serves as the first protective layer 130.
[0090] The single-molecule precursor has a small molecular volume and a strong adsorption capacity, and can be adsorbed on a smaller surface area, which easily reduces the process difficulty of forming the first protective layer 130 at the end of the hard mask layer 121 exposed by the mask opening 125 .
[0091] The monolayer precursor 131 is subjected to plasma bombardment treatment to decompose the monolayer precursor 131 located on the sidewalls of the mask opening 125, the top of the hard mask structure 120, and the gate structure 200 at the bottom of the mask opening 125 to obtain a monolayer 132. The monolayer 132 does not have hydrophobic groups, so it is not easy to increase the difficulty of the subsequent removal of the gate structure 200 at the bottom of the mask opening 125. It is easy to combine with the existing process flow to save process steps.
[0092] In addition, the monomolecular layer 132 has no hydrophobic groups, which facilitates the subsequent formation of a second protective layer on the monomolecular layer 132 .
[0093] Moreover, the hydrophobic groups of the monolayer precursor 131 face away from the inner wall of the inner groove 126, and the remaining monolayer precursor 131 in the inner groove 126 serves as the first protective layer 130. It can be seen that the surface of the inner groove 126 is repellent to aqueous solutions, which makes the inner groove 126 less susceptible to various aqueous solutions, thereby improving the protective effect of the first protective layer 130 on the hard mask layer 121.
[0094] Specifically, in the step of forming the monolayer precursor 131, the monolayer precursor 131 also has hydrophilic groups, and the hydrophilic groups of the monolayer precursor 131 are adsorbed on the side walls of the mask opening 125, the inner walls of the inner groove 126, the top of the hard mask structure 120, and the gate structure 200 at the bottom of the mask opening 125.
[0095] The hydrophilic groups of the monolayer precursor 131 are adsorbed on the side walls of the mask opening 125, the inner walls of the inner groove 126, the top of the hard mask structure 120, and the gate structure 200 at the bottom of the mask opening 125, which makes it easier for the monolayer precursor 131 to cover the side walls of the mask opening 125, the inner walls of the inner groove 126, the top of the hard mask structure 120, and the gate structure 200 at the bottom of the mask opening 125. That is, the first protective layer 130 located in the inner groove 126 covers the inner wall of the inner groove 126 better, so that the protection effect of the first protective layer 130 on the inner wall of the inner groove 126 is also correspondingly better, thereby further improving the protection effect of the first protective layer 130 on the hard mask layer 121.
[0096] More specifically, in the step of forming the monomolecular layer precursor 131 , the monomolecular layer precursor 131 includes an alkylamine complex.
[0097] The alkylamine complex is not only hydrophobic, but also easy to volatilize during the cracking process of the monolayer precursor 131, so that the monolayer precursor 131 can be easily cracked to obtain the monolayer 132.
[0098] In addition, the alkyl chain of the alkylamine complex is adjustable, so it is convenient to introduce different degrees of hydrophobicity according to needs. As an example, in the step of forming the monolayer precursor 131, the alkylamine complex includes one or both of a long-chain alkylamine complex and an alkylamine complex containing an aromatic ring.
[0099] Long-chain alkylamine complexes and alkylamine complexes containing aromatic rings have better hydrophobic properties, that is, the surface of the inner groove 126 has greater repulsion to aqueous solutions, which correspondingly makes the inner groove 126 less susceptible to various aqueous solutions.
[0100] In the step of forming the monolayer precursor 131 , the monolayer precursor 131 also includes a metal element; in the step of bombarding the monolayer precursor 131 , the monolayer 132 obtained by decomposing the monolayer precursor 131 is a metal nitride layer.
[0101] During the bombardment treatment of the monolayer precursor 131, the metal element is easy to combine with the nitrogen element in the alkylamine complex to form a metal nitride layer. The metal nitride layer does not have a hydrophobic group, so the monolayer 132 located on the side wall of the mask opening 125 is not repellent to the aqueous solution, so it is not easy to increase the difficulty of the subsequent process of removing the gate structure 200 at the bottom of the mask opening 125 along the mask opening 125, and it is also easy to combine with the existing process to save process steps; and the metal nitride layer does not have a hydrophobic group, which is convenient for the subsequent formation of a second protective layer on the metal nitride layer, thereby forming a double protection for the end of the hard mask layer 121.
[0102] In this embodiment, the plasma bombardment treatment is performed under a bias voltage condition. Under the bias voltage condition, the plasma has directionality, thereby reducing the probability of the plasma bombarding the monomolecular layer precursor 131 in the inner groove 126 .
[0103] It should be noted that the parameters of the plasma bombardment treatment include: the bombardment gas includes one or both of argon and hydrogen, the bias voltage is 150 volts to 200 volts, the process temperature is 200 degrees Celsius to 300 degrees Celsius, and the process time is 5 seconds to 10 seconds.
[0104] Argon and hydrogen are common gases for plasma bombardment treatment, which have the advantages of low cost, high process compatibility and safe operation.
[0105] It should be noted that the bias voltage of the plasma bombardment treatment should not be too large or too small. Under the action of the bias voltage, the plasma can obtain kinetic energy to bombard the monolayer precursor 131. If the bias voltage is too large, it is easy for the plasma to pass through the monolayer precursor 131 and cause damage to other film layers; if the bias voltage is too small, the kinetic energy provided to the plasma is too small, which is easy to cause the effect and uniformity of the modification treatment to deteriorate, thereby affecting the subsequent removal of the gate structure 200 at the bottom of the mask opening 125 along the mask opening 125. Therefore, in this embodiment, the bias voltage is 150 volts to 200 volts.
[0106] It should also be noted that the process temperature of the plasma bombardment treatment should not be too high or too low. If the process temperature of the plasma bombardment treatment is too high, it is easy for the plasma to pass through the monolayer precursor 131 and damage other film layers; if the process temperature of the plasma bombardment treatment is too low, it is easy to cause the effect and uniformity of the modification treatment to deteriorate, thereby affecting the subsequent removal of the gate structure 200 at the bottom of the mask opening 125 along the mask opening 125. Therefore, in this embodiment, the process temperature is 200 degrees Celsius to 300 degrees Celsius.
[0107] It is also necessary to explain that the process time of the plasma bombardment treatment should not be too long or too short. If the process time of the plasma bombardment treatment is too long, it is easy for the plasma to pass through the monolayer precursor 131 and damage other film layers; if the process time of the plasma bombardment treatment is too short, it is easy to cause the effect and uniformity of the modification treatment to deteriorate, thereby affecting the subsequent removal of the gate structure 200 at the bottom of the mask opening 125 along the mask opening 125. Therefore, in this embodiment, the process time is 5 seconds to 10 seconds.
[0108] refer to Figure 10 to Figure 11 In this embodiment, after forming the first protective layer 130 at the end of the hard mask layer 121 exposed by the mask opening 125 and before forming the isolation opening, it also includes: forming a second protective layer 140 covering the first protective layer 130 on the sidewall of the mask opening 125.
[0109] The second protective layer 140 covers the first protective layer 130, that is, the end of the hard mask layer 121 is covered with the first protective layer 130 and the second protective layer 140. The second protective layer 140 can further protect the hard mask layer 121 in the process of removing the gate structure 200 at the bottom of the mask opening 125 along the mask opening 125 to form an isolation opening, thereby further reducing the probability of the hard mask layer 121 being damaged and causing a gap, so that in the process of removing the gate structure 200 at the bottom of the mask opening 125 to form an isolation opening, the probability of the adjacent gate structure 200 being damaged through the gap of the hard mask layer 121 is lower, thereby reducing the effect of reducing the influence of the formation of the partition structure on the adjacent gate structure 200, and improving the performance of the semiconductor structure.
[0110] Specifically, the step of forming the second protective layer 140 covering the first protective layer 130 includes: Fig.10 As shown, a second protective material layer 141 is formed on the sidewalls of the mask opening 125, the sidewalls of the first protective layer 130, the top of the hard mask structure 120, and the bottom of the mask opening 124; Fig.11 As shown, the top of the hard mask structure 120 and the second protection material layer 141 at the bottom of the mask opening 125 are removed, and the remaining second protection material layer 141 serves as the second protection layer 140 .
[0111] A second protective material layer 141 is formed on the sidewalls of the mask opening 125, the sidewalls of the first protective layer 130, the top of the hard mask structure 120, and the bottom of the mask opening 124, which can easily reduce the process difficulty of forming the second protective layer 140 and can also be easily combined with the existing process flow to save process steps.
[0112] It should be noted that in the step of removing the second protective material layer 141 on the top of the hard mask structure 120, the monolayer 132 on the top of the hard mask structure 120 is also removed. Removing the monolayer 132 on the top of the hard mask structure 120 is beneficial to reducing the aspect ratio of the mask opening 125, thereby reducing the subsequent process difficulty of removing the gate structure 200 at the bottom of the mask opening 125 along the mask opening 125 to form an isolation opening.
[0113] It should also be noted that the process of removing the second protective material layer 141 at the bottom of the mask opening 125 includes a dry etching process. The dry etching process has anisotropic etching characteristics, so the etching accuracy is high and the controllability of the cross section is better, which is beneficial to reduce the probability of the second protective material layer 141 located on the side wall of the first protective layer 130 being damaged during the process of removing the second protective material layer 141 at the bottom of the mask opening 125.
[0114] refer to Figure 12 to Figure 13 After forming the first protection layer 130 , the gate structure 200 at the bottom of the mask opening 125 and a portion of the thickness of the substrate 100 are removed along the mask opening 125 to form an isolation opening 220 .
[0115] The isolation opening 220 provides a space for subsequently forming an isolation structure.
[0116] It should be noted that, in the step of removing the gate structure 200 at the bottom of the mask opening 125 along the mask opening 125 , the process of removing the gate structure 200 at the bottom of the mask opening 125 includes: a wet etching process.
[0117] The cost of the wet etching process is relatively low, and the operation steps are simple. It can also achieve a larger etching selectivity ratio, which is beneficial to reducing the process difficulty of removing the gate structure 200 at the bottom of the mask opening 125; moreover, the wet etching process has an isotropic etching characteristic, which is beneficial to cleanly remove the gate structure 200 at the bottom of the mask opening 125.
[0118] In this embodiment, after the gate structure 200 at the bottom of the mask opening 125 is removed, an anisotropic etching process is used to continue etching a portion of the thickness of the substrate 100 along the mask opening 125 to form an isolation opening 220 .
[0119] As an example, the channel protrusion structure 102 and a portion of the thickness of the substrate 101 are removed along the mask opening 125 to improve the isolation effect of the partition structure.
[0120] It should be noted that, in the process of etching a portion of the thickness of the substrate 100 along the mask opening 125, the third mask layer 123 and a portion of the thickness of the second mask layer 122 are removed. Moreover, removing the third mask layer 123 and exposing the second mask layer 122 is conducive to the subsequent use of chemical mechanical planarization to remove the insulating material above the gate structure 200 and the top of the interlayer dielectric layer 110, which is combined with the existing process to improve process compatibility and reduce costs.
[0121] refer to Fig.14 , a partition structure 221 is formed in the isolation opening 220 .
[0122] The isolation structure 221 is used to isolate adjacent device units to prevent bridging between adjacent devices.
[0123] Specifically, the step of forming the isolation structure 221 in the isolation opening 220 includes: filling the isolation opening 220 with insulating material through the mask opening 125, the insulating material also filling the mask opening 125 and covering the top of the hard mask structure 120; removing the insulating material above the gate structure 200 and the top of the interlayer dielectric layer 110, and the remaining insulating material in the isolation opening 220 serves as the isolation structure 221.
[0124] The insulating material is filled in the isolation opening 220 through the mask opening 125. The insulating material is also filled in the mask opening 125 and covers the top of the hard mask structure 120, providing a process margin for the subsequent removal of the insulating material above the top of the gate structure 200 and the interlayer dielectric layer 110, which is conducive to reducing the process difficulty of forming the partition structure 221. In addition, removing the insulating material above the top of the gate structure 200 and the interlayer dielectric layer 110 can easily make the surface flatness of the isolation structure 221 better.
[0125] It should be noted that the process of removing the insulating material above the top of the gate structure 200 and the interlayer dielectric layer 110 includes a chemical mechanical planarization process. The chemical mechanical planarization process is a global planarization process with a high planarization efficiency, which is beneficial to improving the surface flatness of the isolation structure 221, the interlayer dielectric layer 110, and the gate structure 200 after planarization.
[0126] Continue to refer Fig.14 In this embodiment, after forming the partition structure 221 and the stop layer 150, a source-drain doped interconnection layer (not shown) is formed.
[0127] In the subsequent process of forming a source-drain doped interconnect layer electrically connected to the source-drain doped layer 300 , the stop layer 150 can function as an etching stop layer.
[0128] In this embodiment, the material of the stop layer 150 includes one or more of silicon nitride, silicon carbide, silicon oxycarbide or silicon carbon nanotube. As an example, the material of the stop layer 150 is silicon nitride.
[0129] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for forming a semiconductor structure, characterized in that: include: Providing a substrate, the substrate comprising an isolation region, a gate structure formed on the substrate, an interlayer dielectric layer formed on the substrate at the side of the gate structure, the gate structure and the interlayer dielectric layer are covered with a hard mask structure on top, the hard mask structure is a stacked structure and includes a hard mask layer closest to the top of the gate structure; forming a mask opening in the hard mask structure at a top of the gate structure in the isolation region; forming a first protective layer at an end portion of the hard mask layer exposed by the mask opening; After forming the first protection layer, removing the gate structure at the bottom of the mask opening and a portion of the thickness of the substrate along the mask opening to form an isolation opening; A partition structure is formed in the isolation opening.
2. The method for forming a semiconductor structure according to claim 1, wherein: After forming a mask opening at the top of the gate structure in the isolation region in the hard mask structure, and before forming a first protective layer at the end of the hard mask layer exposed by the mask opening, the method further includes: laterally removing a portion of the hard mask layer in a direction perpendicular to the sidewall of the mask opening to form an inner groove in the hard mask structure, wherein the inner groove is connected to the mask opening; In the step of forming the first protection layer at the end of the hard mask layer exposed by the mask opening, the first protection layer is formed in the inner groove.
3. The method for forming a semiconductor structure according to claim 2, wherein: In the process of laterally removing a portion of the width of the hard mask layer along a direction perpendicular to the sidewall of the mask opening, a portion of the thickness of the gate structure at the bottom of the mask opening is also removed.
4. The method for forming a semiconductor structure according to claim 2, wherein: The process of laterally removing a portion of the width of the hard mask layer along a direction perpendicular to the sidewall of the mask opening includes an isotropic etching process.
5. The method for forming a semiconductor structure according to claim 4, wherein: The isotropic etching process is a wet etching process, and the wet etching process sequentially uses a hydrogen peroxide solution and a hydrochloric acid solution, the temperature of the hydrogen peroxide solution is 60 degrees Celsius to 80 degrees Celsius, the treatment time of the hydrogen peroxide solution is 50 seconds to 100 seconds, the temperature of the hydrochloric acid solution is room temperature, and the treatment time of the hydrochloric acid solution is 10 seconds to 20 seconds.
6. The method for forming a semiconductor structure according to claim 2, wherein: Along a direction perpendicular to the sidewall of the mask opening, a lateral depth of the inner groove is 50 angstroms to 100 angstroms.
7. The method for forming a semiconductor structure according to claim 2 or 3, characterized in that: The step of forming a first protective layer at the end of the hard mask layer exposed by the mask opening comprises: Depositing a monolayer precursor on the sidewalls of the mask opening, the inner wall of the inner groove, the top of the hard mask structure, and the gate structure at the bottom of the mask opening, wherein the monolayer precursor covers the end of the hard mask layer, the monolayer precursor has a hydrophobic group, and the hydrophobic group of the monolayer precursor faces away from the sidewalls of the mask opening, the inner wall of the inner groove, the top of the hard mask structure, and the gate structure at the bottom of the mask opening; The monolayer precursor is subjected to plasma bombardment treatment to decompose the monolayer precursor located on the sidewall of the mask opening, the top of the hard mask structure, and the gate structure at the bottom of the mask opening to obtain a monolayer, and the remaining monolayer precursor located in the inner groove serves as a first protective layer.
8. The method for forming a semiconductor structure according to claim 7, wherein: In the step of forming the monolayer precursor, the monolayer precursor also has hydrophilic groups, and the hydrophilic groups of the monolayer precursor are adsorbed on the side walls of the mask opening, the inner walls of the inner groove, the top of the hard mask structure, and the gate structure at the bottom of the mask opening.
9. The method for forming a semiconductor structure according to claim 8, wherein: In the step of forming the monolayer precursor, the monolayer precursor includes an alkylamine complex.
10. The method for forming a semiconductor structure according to claim 9, wherein: In the step of forming the monolayer precursor, the alkylamine complex includes one or both of a long-chain alkylamine complex and an alkylamine complex containing an aromatic ring.
11. The method for forming a semiconductor structure according to claim 9, wherein: In the step of forming the monomolecular layer precursor, the monomolecular layer precursor further comprises a metal element; In the step of bombarding the monomolecular layer precursor, the monomolecular layer obtained by decomposing the monomolecular layer precursor is a metal nitride layer.
12. The method for forming a semiconductor structure according to claim 7, wherein: The plasma bombardment treatment is performed under bias voltage conditions, and the parameters of the plasma bombardment treatment include: the bombardment gas includes one or both of argon and hydrogen, the bias voltage is 150 volts to 200 volts, the process temperature is 200 degrees Celsius to 300 degrees Celsius, and the process time is 5 seconds to 10 seconds.
13. The method for forming a semiconductor structure according to any one of claims 1 to 3, characterized in that: After forming a first protection layer at the end of the hard mask layer exposed by the mask opening and before forming the isolation opening, the method further includes: forming a second protection layer covering the first protection layer on the sidewall of the mask opening.
14. The method for forming a semiconductor structure according to claim 13, wherein: The step of forming a second protective layer covering the first protective layer comprises: forming a second protective material layer on the sidewalls of the mask opening, the sidewalls of the first protective layer, the top of the hard mask structure, and the bottom of the mask opening; The second protection material layer on the top of the hard mask structure and the bottom of the mask opening is removed, and the remaining second protection material layer serves as a second protection layer.
15. The method for forming a semiconductor structure according to claim 1, wherein: In the step of removing the gate structure at the bottom of the mask opening along the mask opening, the process of removing the gate structure at the bottom of the mask opening includes: a wet etching process.
16. The method for forming a semiconductor structure according to claim 1, wherein: In the step of providing a substrate, the hard mask layer is a metal hard mask layer.
17. The method for forming a semiconductor structure according to claim 16, wherein: The material of the hard mask layer includes titanium nitride or aluminum nitride.
18. The method for forming a semiconductor structure according to claim 1, wherein: The step of forming a partition structure in the isolation opening comprises: Filling the isolation opening with an insulating material through the mask opening, wherein the insulating material also fills the mask opening and covers the top of the hard mask structure; The insulating material above the gate structure and the top of the interlayer dielectric layer is removed, and the remaining insulating material in the isolation opening serves as a partition structure.