Gallium oxide vertical trench gate MOSFET (Metal-Oxide-Semiconductor Field Effect Transistor) with dielectric columns and preparation method thereof

By introducing oxide dielectric pillars into the gallium oxide vertical trench gate MOSFET to form a capacitor and improve the potential distribution, the problem of low breakdown voltage of the existing gallium oxide vertical trench gate MOSFET is solved, and the reliability and performance of the device are improved.

CN118738093AActive Publication Date: 2024-10-01SOUTH CHINA NORMAL UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410767717.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

The breakdown voltage of existing gallium oxide vertical trench gate MOSFETs is low, which limits the performance and reliability of the devices.

Method used

Introduce oxide dielectric pillars into vertical trench gate MOSFETs, and form a capacitor by setting dielectric pillars on both sides of the drift layer to improve the potential distribution during breakdown, adjust the breakdown position, and increase the breakdown voltage.

Benefits of technology

It effectively improves the reverse breakdown voltage of gallium oxide vertical trench gate MOSFET, improves the reliability and performance of the device, and alleviates the avalanche multiplication effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738093A_ABST
    Figure CN118738093A_ABST
Patent Text Reader

Abstract

The invention discloses a gallium oxide vertical trench gate MOSFET (Metal-Oxide-Semiconductor Field Effect Transistor) with dielectric columns and a preparation method of the gallium oxide vertical trench gate MOSFET, and relates to the technical field of gallium oxide MOSFETs. According to the gallium oxide vertical trench gate MOSFET with the dielectric columns, the oxide dielectric columns improve potential distribution during breakdown, a capacitor is formed among the source electrode, the dielectric columns and the drain electrode in a reverse state, and the potential distribution in the dielectric columns and a drift region is more uniform in the vertical direction due to the coupling effect of the oxide dielectric columns. In addition, the breakdown position under the condition that no dielectric column exists originally is adjusted, so that the avalanche multiplication effect of the device is relieved, the breakdown voltage is improved, and the reliability and the performance of the device are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of gallium oxide MOSFET, in particular to a gallium oxide vertical trench gate MOSFET with a dielectric column and a preparation method thereof. Background Art

[0002] Compared with traditional wide bandgap semiconductor materials such as SiC and GaN, Ga 2 O 3 Due to its excellent material properties such as ultra-wide bandgap (4.5-4.9eV) and high critical breakdown electric field (8MV / cm), as well as high Baliga merit of more than 3000, it has become an emerging important player in the field of electric energy switching, electronic and electrical industry, power and radio frequency electronics industry. In recent years, through the innovation and efforts of researchers in the semiconductor field, various Ga with excellent performance have been proposed. 2 O 3 Based devices, such as Schottky diodes (SBD), field effect transistors (MOSFET), heterojunction diodes (HJD), all of which indicate that Ga 2 O 3 It has great potential and development prospects in power device applications. However, due to the 2 O 3 The p-type doping technology is currently not perfect, which hinders the further development of power devices.

[0003] In order to better play the role of 2 O 3 Compared with lateral MOSFET devices, vertical MOSFET devices have the advantages of occupying smaller size and higher power density. The existing vertical MOSFET can basically be divided into two types: fin field effect transistor (FinFET) and current blocking type (CBL) field effect transistor. However, since the forward turn-on of FinFET devices depends largely on the size of the fin channel, its manufacturing process hinders the production efficiency and yield of the device. CBL field effect transistors have developed rapidly in recent years and attracted the interest of a large number of researchers. CBL field effect transistors include current aperture vertical electron transistors (CAVET), vertical diffused barrier field effect transistors (VDBFET), and U-type trench gate field effect transistors (UMOSFET), but compared with the relatively mature FinFET, the performance still needs to be improved. Summary of the invention

[0004] Based on this, the purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a gallium oxide vertical trench gate MOSFET with dielectric pillars and a preparation method thereof. The gallium oxide vertical trench gate MOSFET with dielectric pillars provided by the present invention can improve the performance of the device and alleviate the problem of low breakdown voltage of traditional gallium oxide vertical trench gate MOSFET.

[0005] To achieve the above object, the technical solution adopted by the present invention is: a gallium oxide vertical trench gate MOSFET with a dielectric pillar, comprising a drain metal layer, a highly doped N-type gallium oxide substrate layer, a low-doped N-type gallium oxide drift layer, an oxide dielectric pillar, a current blocking layer, a highly doped N-type ohmic contact layer, a source metal layer, an oxide dielectric layer, and a gate metal layer;

[0006] The drain metal layer, the highly doped N-type gallium oxide substrate layer, and the low doped N-type gallium oxide drift layer are sequentially arranged, the upper surface of the drain metal layer contacts the lower surface of the highly doped N-type gallium oxide substrate layer, and oxide dielectric pillars are respectively arranged on both sides of the low doped N-type gallium oxide drift layer; the lower surface of the oxide dielectric pillar contacts the highly doped N-type gallium oxide substrate layer;

[0007] The current blocking layer and the highly doped N-type ohmic contact layer are sequentially arranged, and the lower surface of the current blocking layer is in contact with the low-doped N-type gallium oxide drift layer and the oxide dielectric column;

[0008] The vertical trench gate MOSFET is provided with a U-shaped trench, and the U-shaped trench is recessed downward from the upper surface of the highly doped N-type ohmic contact layer to the low-doped N-type gallium oxide drift layer;

[0009] The oxide dielectric layer covers the inner wall of the U-shaped groove and the upper surface of the highly doped N-type ohmic contact layer. The oxide dielectric layer has a through hole that penetrates the upper and lower surfaces. The through hole is located above the highly doped N-type ohmic contact layer. A source metal layer is arranged in the through hole. The lower surface of the source metal layer contacts the highly doped N-type ohmic contact layer. A gate metal layer is arranged on the upper surface of the oxide dielectric.

[0010] The current blocking layer is formed by N ion implantation to form a compensation semiconductor and plays a role of current blocking.

[0011] The present invention adds dielectric pillars on both sides of the drift layer, so that the source, dielectric pillars and drain form a capacitor in the reverse state of the device. The coupling effect can improve the potential distribution during breakdown, adjust the original breakdown position, and increase the breakdown voltage of the MOSFET, thereby improving the reliability and performance of the device. Therefore, the MOSFET structure of the present invention can effectively increase the reverse breakdown voltage of the gallium oxide vertical trench gate MOSFET.

[0012] Preferably, the thickness of the highly doped N-type gallium oxide substrate layer is 2-4 μm, and the effective doping concentration of the N-type gallium oxide is 2×10 18 -4×10 18 cm -3 .

[0013] Further preferably, the thickness of the highly doped N-type gallium oxide substrate layer is 2 μm, and the effective doping concentration of the N-type gallium oxide is 2×10 18 cm -3 .

[0014] Preferably, the thickness of the low-doped N-type gallium oxide drift layer is 5-7 μm, and the effective doping concentration of the N-type gallium oxide is 1×10 16 -2.5×10 16 cm -3 .

[0015] Further preferably, the thickness of the low-doped N-type gallium oxide drift layer is 6 μm, and the effective doping concentration of the N-type gallium oxide is 2×10 16 cm -3

[0016] Preferably, the oxide dielectric pillar has a width of 2-3.5 μm and a thickness of 5-7 μm.

[0017] Preferably, the thickness of the oxide dielectric layer is 20-40 nm. Further preferably, the thickness of the oxide dielectric layer is 20 nm.

[0018] Preferably, the thickness of the current blocking layer is 0.2-0.4 μm, and the effective doping concentration of nitrogen ions is 5×10 18 -7×10 18 cm -3 .

[0019] Preferably, the thickness of the highly doped N-type ohmic contact layer is 100-150 nm, and the effective doping concentration of N-type gallium oxide is 2×10 18 -4×10 18 cm -3 .

[0020] Further preferably, the thickness of the highly doped N-type ohmic contact layer is 100 nm, and the effective doping concentration of N-type gallium oxide is 2×10 18 cm -3 .

[0021] Preferably, the drain metal layer comprises a titanium layer and a gold layer stacked from bottom to top, the gold layer is connected to the highly doped N-type gallium oxide substrate layer, wherein the thickness of the gold layer is 130-160nm, and the thickness of the titanium layer is 40-70nm; the source metal layer comprises a gold layer and a titanium layer stacked from bottom to top, wherein the thickness of the titanium layer is 130-160nm, and the thickness of the gold layer is 40-70nm; the gate metal layer comprises a gold layer and a nickel layer stacked from bottom to top, wherein the thickness of the nickel layer is 130-160nm, and the thickness of the gold layer is 40-70nm.

[0022] In addition, the present invention provides a method for preparing the gallium oxide vertical trench gate MOSFET with dielectric pillars, comprising the following steps:

[0023] S1, depositing a low-doped N-type gallium oxide drift layer on the upper surface of the highly doped N-type gallium oxide substrate layer;

[0024] S2, applying glue on the upper surface of the low-doped N-type gallium oxide drift layer, and etching both sides to form two grooves;

[0025] S3, depositing oxide dielectrics in the trenches to fill the trenches to obtain oxide dielectric pillars and removing the resist;

[0026] S4, continuing to deposit a low-doped N-type gallium oxide drift layer on the upper surface of the oxide dielectric pillar and the low-doped N-type gallium oxide drift layer to prepare a current blocking layer;

[0027] S5, implanting nitrogen ions into the drift layer of the sample and annealing to activate the implanted nitrogen ions to form a current blocking layer;

[0028] S6, implanting silicon ions into the sample and annealing to activate the implanted silicon ions to form a highly doped N-type ohmic contact layer;

[0029] S7, applying glue on the upper surface of the highly doped N-type ohmic contact layer, and then etching to form a U-shaped groove in the middle of the square of the highly doped N-type ohmic contact layer, and etching the bottom of the groove to the low-doped N-type gallium oxide drift layer;

[0030] S8, depositing an oxide dielectric layer on the sample after the U-shaped groove is formed;

[0031] S9, etching and depositing the upper surface of the oxide dielectric layer on both sides of the U-shaped groove to obtain a source metal layer;

[0032] S10, depositing on the lower surface of the highly doped N-type gallium oxide substrate layer, and rapidly annealing to obtain a drain metal layer;

[0033] S11. In the U-shaped trench, a gate metal layer is deposited on the upper surface of the oxide dielectric layer to obtain the gallium oxide vertical trench gate MOSFET with dielectric pillars.

[0034] Preferably, in step S1, before depositing the low-doped N-type gallium oxide drift layer on the upper surface of the highly doped N-type gallium oxide substrate layer, the highly doped N-type gallium oxide substrate layer needs to be cleaned, and the specific steps are: cleaning with acetone, ethanol, and deionized water for 10-15 minutes each, and drying in a high-purity (>99%) nitrogen environment.

[0035] Preferably, in the step S1, the method of depositing the low-doped N-type gallium oxide drift layer on the upper surface of the highly doped N-type gallium oxide substrate layer is one of hydride vapor phase epitaxy (HVPE) and metal-organic chemical vapor deposition (MOCVD).

[0036] Preferably, the glue coating in steps S2 and S7 includes a first spin coating, a second spin coating and annealing in sequence; the first spin coating has a rotation speed of 300-800 rpm and a time of 10-15 s; the second spin coating has a rotation speed of 500-1600 rpm and a time of 60-90 s; the annealing temperature is 100-150° C. and the time is 60-90 s.

[0037] Preferably, in S3, the method for depositing the oxide dielectric pillars is a plasma enhanced chemical vapor deposition (PECVD) process method, and after the deposition is completed under the condition of 80-90° C., the sample is stripped.

[0038] Preferably, in S5 and S6, the ion implantation method comprises the following steps: depositing a 120 nm thick silicon dioxide film on the upper surface of the sample as a sacrificial layer for implantation, then implanting N ions or Si ions into the drift layer through an ion implantation device, removing the sacrificial layer after the implantation is completed, and finally annealing at 1200°C for 25 minutes to activate the implanted N ions or Si ions.

[0039] Preferably, the deposition method of the source metal layer, the drain metal layer and the gate metal layer is one of electron beam evaporation, thermal evaporation and magnetron sputtering technology.

[0040] Compared with the prior art, the beneficial effects of the present invention are as follows: the oxide dielectric column of the gallium oxide vertical trench gate MOSFET with dielectric column provided by the present invention improves the potential distribution during breakdown, and in the reverse state, forms a capacitor between the source, dielectric column and drain, and its coupling effect makes the potential distribution in the dielectric column and the drift region more uniform in the vertical direction. In addition, the present invention also adjusts the breakdown position in the case of no dielectric column, thereby alleviating the avalanche multiplication effect of the device, increasing the breakdown voltage, and improving the reliability and performance of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 It is a schematic structural diagram of a gallium oxide vertical trench gate MOSFET with a dielectric pillar according to Example 1;

[0042] Figure 2 Schematic diagram of the structure of a conventional gallium oxide vertical trench gate MOSFET of Comparative Example 1;

[0043] Figure 3 A comparison diagram of potential distribution when the MOSFET of Example 1 and Comparative Example 1 is broken down;

[0044] Figure 4 It is a comparison diagram of the reverse breakdown voltage simulation of the MOSFET devices of Examples 1-6 and Comparative Example 1;

[0045] Figure 1-2 Middle: 1. Drain metal layer; 2. Highly doped N-type gallium oxide substrate layer; 3. Low-doped N-type gallium oxide drift layer; 4. Oxide dielectric column; 5. Current blocking layer; 6. Highly doped N-type ohmic contact layer; 7. Source metal layer; 8. Oxide dielectric layer; 9. Gate metal layer. DETAILED DESCRIPTION

[0046] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. In the embodiments, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.

[0047] Example 1

[0048] like Figure 1 As shown, a gallium oxide vertical trench gate MOSFET with a dielectric column includes: a drain metal layer 1, a highly doped N-type gallium oxide substrate layer 2, a low-doped N-type gallium oxide drift layer 3, an oxide dielectric column 4, a current blocking layer 5, a highly doped N-type ohmic contact layer 6, a source metal layer 7, an oxide dielectric layer 8, and a gate metal layer 9;

[0049] The drain metal layer 1, the highly doped N-type gallium oxide substrate layer 2, and the low doped N-type gallium oxide drift layer 3 are arranged in sequence, the upper surface of the drain metal layer 1 is in contact with the lower surface of the highly doped N-type gallium oxide substrate layer 2, and oxide dielectric pillars 4 are respectively arranged on both sides of the low doped N-type gallium oxide drift layer 3; the lower surface of the oxide dielectric pillar 4 is in contact with the highly doped N-type gallium oxide substrate layer 2;

[0050] The current blocking layer 5 and the highly doped N-type ohmic contact layer 6 are sequentially arranged, and the lower surface of the current blocking layer 5 is in contact with the low-doped N-type gallium oxide drift layer 3 and the oxide dielectric column 4;

[0051] The vertical trench gate MOSFET is provided with a U-shaped trench, which is recessed downward from the upper surface of the highly doped N-type ohmic contact layer 6 to the low-doped N-type gallium oxide drift layer 3;

[0052] The oxide dielectric layer 8 covers the inner wall of the U-shaped groove and the upper surface of the highly doped N-type ohmic contact layer 6. The oxide dielectric layer 8 has a through hole, which passes through the upper and lower surfaces of 8. The through hole is located above 6. A source metal layer 7 is arranged in the through hole. The lower surface of the source metal layer 7 is in contact with the highly doped N-type ohmic contact layer 6; the upper surface of the oxide dielectric layer 8 is provided with a gate metal layer 9.

[0053] The drain metal layer 1 comprises a stacked gold layer and a titanium layer, wherein the gold layer is connected to the highly doped N-type gallium oxide substrate layer; wherein the thickness of the gold layer is 150 nm; and the thickness of the titanium layer is 50 nm.

[0054] The thickness of the highly doped N-type gallium oxide substrate layer 2 is 2 μm, and the effective doping concentration of the N-type gallium oxide is 2×10 18 cm -3 .

[0055] The thickness of the low-doped N-type gallium oxide drift layer 3 is 6 μm, and the effective doping concentration of the N-type gallium oxide is 2×10 16 cm -3 The lower surface of the low-doped N-type gallium oxide drift layer 3 is in contact with the high-doped N-type gallium oxide substrate layer 2 .

[0056] The oxide dielectric column 4 is made of silicon dioxide and consists of two identical regions with a width of 3 μm and a thickness of 6 μm, which are respectively located on both sides of the low-doped N-type gallium oxide drift layer 3 . The lower surface of the oxide dielectric column 4 is in contact with the high-doped N-type gallium oxide substrate layer 2 .

[0057] The thickness of the current blocking layer 5 is 0.3 μm, and the effective nitrogen ion doping concentration is 6×10 18 cm -3 ,

[0058] The thickness of the highly doped N-type ohmic contact layer 6 is 100 nm, and the effective doping concentration of N-type gallium oxide is 2×10 18 cm -3 .

[0059] The source metal layer 7 includes a stacked titanium layer and a gold layer; the thickness of the titanium layer is 150 nm, and the thickness of the gold layer is 50 nm.

[0060] The oxide dielectric layer 8 is made of aluminum oxide, is located outside the U-shaped groove, and has a thickness of 20 nm.

[0061] The gate metal layer 9 includes a stacked nickel layer and a gold layer; the thickness of the nickel layer is 150 nm, and the thickness of the gold layer is 50 nm.

[0062] A method for preparing a gallium oxide vertical trench gate MOSFET with a dielectric pillar comprises the following steps:

[0063] S1. The highly doped N-type gallium oxide substrate layer 2 was cleaned in acetone, ethanol, and deionized water for 10 min each. 2 Dry conditions;

[0064] S2. Depositing a low-doped N-type gallium oxide drift layer 3 on the upper surface of the high-doped N-type gallium oxide substrate layer 2 by using hydride vapor phase epitaxy (HVPE) technology.

[0065] S3, applying glue on the upper surface of the low-doped N-type gallium oxide drift layer 3, using photolithography and etching technology, using BCl gas for etching, and preparing two grooves with the same thickness as the low-doped N-type gallium oxide drift layer 3 and a width of 3 μm on the upper surface of the epitaxial layer.

[0066] 3a) The coating in step 3 comprises placing the sample in a spin coater, and firstly spinning the sample at a speed of 500 rpm for 15 seconds; then spinning the sample at a speed of 1000 rpm for 80 seconds; and finally annealing the sample at a temperature of 150° C. for 80 seconds;

[0067] 3b) exposing the annealed sample in a photolithography machine for 1.5 seconds, and then placing it in a developer for development to expose the low-doped N-type gallium oxide drift layer 3 of the portion to be etched;

[0068] 3c) Place the developed sample in deionized water to remove the developer remaining on the sample surface and 2 Drying in the environment;

[0069] 3d) The dried sample was placed in a reaction chamber of an inductively coupled plasma (ICP) etching instrument and etched using BCl gas to obtain two grooves with a thickness of 6 μm and a width of 3 μm on the upper surface of the epitaxial layer.

[0070] S4. Deposit oxide dielectric pillars 4 in two grooves of the low-doped N-type gallium oxide drift layer 3 using a plasma enhanced chemical vapor deposition (PECVD) process. After the deposition is completed at 80-90° C., remove the sample from the adhesive.

[0071] S5 , using hydride vapor phase epitaxy (HVPE) technology to continue depositing a drift layer on the upper surface of the low-doped N-type gallium oxide drift layer 3 and the oxide dielectric pillar 4 to prepare a current blocking layer 5 .

[0072] S6. Deposit a 120 nm thick silicon dioxide film as a sacrificial layer for injection on the upper surface of the drift layer used to prepare the current blocking layer 5, and then inject nitrogen ions into the drift layer through an ion implantation device. After the implantation is completed, remove the sacrificial layer, and finally anneal at 1200° C. for 25 minutes to activate the injected nitrogen ions.

[0073] S7. A 120 nm thick silicon dioxide film is deposited on the upper surface of the current blocking layer 5 as a sacrificial layer for injection, and then silicon ions are injected into the sample by ion injection equipment. After the injection is completed, the sacrificial layer is removed, and finally the silicon ions are activated by rapid annealing equipment.

[0074] S8, applying glue on the upper surface of the highly doped N-type ohmic contact layer 6, using photolithography and etching technology, using BCl gas for etching, forming a U-shaped groove with a width of 77 μm in the middle of the highly doped N-type ohmic contact layer, etching the bottom of the groove to the low-doped N-type gallium oxide drift layer 3 and removing the glue.

[0075] 8a) The coating in step 8 comprises placing the sample in a spin coater, and firstly spinning the sample at a speed of 500 rpm for 15 seconds; then spinning the sample at a speed of 1000 rpm for 80 seconds; and finally annealing the sample at a temperature of 150° C. for 80 seconds;

[0076] 8b) exposing the annealed sample in a photolithography machine for 1.5 seconds, and then placing it in a developer for development to expose the highly doped N-type ohmic contact layer 6 of the portion to be etched;

[0077] 8c) Place the developed sample in deionized water to remove the developer remaining on the sample surface and 2 Drying in the environment;

[0078] 8d) The dried sample is placed in a reaction chamber of an inductively coupled plasma (ICP) etching instrument and etched using BCl gas to form a 77 μm wide U-shaped groove in the middle of the highly doped N-type ohmic contact layer 6. The bottom of the groove is etched to the low-doped N-type gallium oxide drift layer 3 and the glue is removed.

[0079] S9. Depositing an oxide dielectric layer 8 in the U-shaped groove by a plasma enhanced chemical vapor deposition (PECVD) process at 80-90° C.

[0080] S10 , applying glue on the upper surface of the oxide dielectric layer 8 , and etching with BCl gas by means of photolithography and etching processes to etch out a source region above the highly doped N-type ohmic contact layer 6 .

[0081] 10a) The coating in step 10 comprises placing the sample in a spin coater, and firstly spinning the sample at a speed of 500 rpm for 15 seconds; then spinning the sample at a speed of 1000 rpm for 80 seconds; and finally annealing the sample at a temperature of 150° C. for 80 seconds.

[0082] 10b) exposing the annealed sample in a photolithography machine for 1.5 seconds, and then placing it in a developer for development to expose the highly doped N-type ohmic contact layer 6 of the portion to be etched;

[0083] 10c) Place the developed sample in deionized water to remove the developer remaining on the sample surface and 2 Drying in the environment;

[0084] 10d) The dried sample is placed in a reaction chamber of an inductively coupled plasma (ICP) etching instrument and etched using BCl gas to etch a source region above the highly doped N-type ohmic contact layer 6 .

[0085] S11, using an electron beam evaporation process to deposit and rapidly anneal in the source region to obtain a source metal layer 7, deposit and rapidly anneal on the lower surface of the highly doped N-type gallium oxide substrate layer 2 to obtain a drain metal layer 1, and deposit and rapidly anneal on the upper surface of the oxide dielectric layer 8 in the middle U-shaped groove to obtain a gate metal layer 9.

[0086] Example 2

[0087] The difference between Example 2 and Example 1 is that the effective doping concentration of the low-doped N-type gallium oxide drift layer 3 in Example 2 is 1×10 16 cm -3 The width of the oxide dielectric column 4 is 2.5 μm; the thickness of the current blocking layer 5 is 0.25 μm, and the effective nitrogen ion doping concentration is 5.6×10 18 cm -3 .

[0088] Example 3

[0089] The difference between Example 3 and Example 1 is that the effective doping concentration of the low-doped N-type gallium oxide drift layer 3 in Example 3 is 2.5×10 16 cm -3 ; The width of the oxide dielectric column 4 is 3.5 μm; the thickness of the current blocking layer 5 is 0.35 μm, and the effective nitrogen ion doping concentration is 6.5×10 18 cm -3 .

[0090] Example 4

[0091] The difference between Example 4 and Example 1 is that the effective doping concentration of the low-doped N-type gallium oxide drift layer 3 in Example 4 is 3×10 16 cm -3 .

[0092] Example 5

[0093] The only difference between Example 5 and Example 1 is that the width of the oxide dielectric pillar 4 in Example 5 is 1 μm.

[0094] Example 6

[0095] The only difference between Example 6 and Example 1 is that the thickness of the current blocking layer 5 in Example 6 is 0.1 μm.

[0096] Comparative Example 1

[0097] The difference between Comparative Example 1 and Example 1 is that: Figure 2 As shown, the low-doped N-type gallium oxide drift layer 3 of Comparative Example 1 does not contain oxide dielectric pillars 4 on both sides.

[0098] Performance Testing

[0099] Sentaurus software was used to set the device size and concentration parameters for the MOSFETs of Examples 1-3 and the comparative example, and a reverse breakdown voltage simulation comparison test of the device was performed. The data are shown in Tables 1 and Figure 4 .

[0100] Table 1 Reverse breakdown voltage of MOSFETs of Examples 1-6 and Comparative Example 1

[0101] Group Reverse breakdown voltage / V Example 1 865.2 Example 2 801.3 Example 3 822.4 Example 4 613.0 Example 5 575.3 Example 6 596.6 Comparative Example 1 430.7

[0102] From Table 1 and Figure 4 It can be seen that the reverse breakdown voltages of Examples 1-3 all reach above 700V. Compared with Comparative Example 1, Example 1 is improved by 100.9%, Example 2 is improved by 86.0%, and Example 3 is improved by 90.9%; Figure 3 By comparison, it can be seen that the potential distribution of the MOSFET with dielectric pillars in the vertical direction is indeed more uniform than that of the traditional MOSFET without dielectric pillars. Therefore, the MOSFET structure of the present invention can effectively alleviate the avalanche multiplication effect of the device, increase the breakdown voltage of the device, and improve the reliability and performance of the device.

[0103] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A gallium oxide vertical trench gate MOSFET with dielectric pillars, characterized in that: It includes a drain metal layer, a highly doped N-type gallium oxide substrate layer, a low doped N-type gallium oxide drift layer, an oxide dielectric column, a current blocking layer, a highly doped N-type ohmic contact layer, a source metal layer, an oxide dielectric layer, and a gate metal layer; The drain metal layer, the highly doped N-type gallium oxide substrate layer, and the low doped N-type gallium oxide drift layer are sequentially arranged, the upper surface of the drain metal layer contacts the lower surface of the highly doped N-type gallium oxide substrate layer, and oxide dielectric pillars are respectively arranged on both sides of the low doped N-type gallium oxide drift layer; the lower surface of the oxide dielectric pillar contacts the highly doped N-type gallium oxide substrate layer; The current blocking layer and the highly doped N-type ohmic contact layer are sequentially arranged, and the lower surface of the current blocking layer is in contact with the low-doped N-type gallium oxide drift layer and the oxide dielectric column; The vertical trench gate MOSFET is provided with a U-shaped trench, and the U-shaped trench is recessed downward from the upper surface of the highly doped N-type ohmic contact layer to the low-doped N-type gallium oxide drift layer; The oxide dielectric layer covers the inner wall of the U-shaped groove and the upper surface of the highly doped N-type ohmic contact layer. The oxide dielectric layer has a through hole that penetrates the upper and lower surfaces. The through hole is located above the highly doped N-type ohmic contact layer. A source metal layer is arranged in the through hole. The lower surface of the source metal layer contacts the highly doped N-type ohmic contact layer. A gate metal layer is arranged on the upper surface of the oxide dielectric.

2. The gallium oxide vertical trench gate MOSFET with dielectric pillars according to claim 1, characterized in that: The thickness of the highly doped N-type gallium oxide substrate layer is 2-4 μm, and the effective doping concentration of the N-type gallium oxide is 2×10 18 -4×10 18 cm -3 .

3. The gallium oxide vertical trench gate MOSFET with dielectric pillars according to claim 1, characterized in that: The thickness of the low-doped N-type gallium oxide drift layer is 5-7 μm, and the effective doping concentration of the N-type gallium oxide is 1×10 16 -2.5×10 16 cm -3 .

4. The gallium oxide vertical trench gate MOSFET with dielectric pillars according to claim 1, characterized in that: The oxide dielectric pillar has a width of 2-3.5 μm and a thickness of 5-7 μm.

5. The gallium oxide vertical trench gate MOSFET with dielectric pillars according to claim 1, characterized in that: The thickness of the oxide dielectric layer is 20-40 nm.

6. The gallium oxide vertical trench gate MOSFET with dielectric pillars according to claim 1, characterized in that: The thickness of the current blocking layer is 0.2-0.4 μm, and the effective doping concentration of nitrogen ions is 5×10 18 -7×10 18 cm -3 .

7. The gallium oxide vertical trench gate MOSFET with dielectric pillars according to claim 1, characterized in that: The thickness of the highly doped N-type ohmic contact layer is 100-150 nm, and the effective doping concentration of N-type gallium oxide is 2×10 18 -4×10 18 cm -3 .

8. The gallium oxide vertical trench gate MOSFET with dielectric pillars according to claim 1, characterized in that: The drain metal layer includes a titanium layer and a gold layer stacked from bottom to top, the gold layer is connected to the highly doped N-type gallium oxide substrate layer, wherein the thickness of the gold layer is 130-160nm, and the thickness of the titanium layer is 40-70nm; the source metal layer includes a gold layer and a titanium layer stacked from bottom to top, wherein the thickness of the titanium layer is 130-160nm, and the thickness of the gold layer is 40-70nm; the gate metal layer includes a gold layer and a nickel layer stacked from bottom to top, wherein the thickness of the nickel layer is 130-160nm, and the thickness of the gold layer is 40-70nm.

9. The gallium oxide vertical trench gate MOSFET with dielectric pillars according to claim 1, characterized in that: The thickness of the oxide dielectric layer is 20-40 nm.

10. The method for preparing a gallium oxide vertical trench gate MOSFET with a dielectric pillar according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1, depositing a low-doped N-type gallium oxide drift layer on the upper surface of the highly doped N-type gallium oxide substrate layer; S2, applying glue on the upper surface of the low-doped N-type gallium oxide drift layer, and etching both sides to form two grooves; S3, depositing oxide dielectrics in the trenches to fill the trenches to obtain oxide dielectric pillars and removing the resist; S4, continuing to deposit a low-doped N-type gallium oxide drift layer on the upper surface of the oxide dielectric pillar and the low-doped N-type gallium oxide drift layer to prepare a current blocking layer; S5, implanting nitrogen ions into the drift layer of the sample and annealing to activate the implanted nitrogen ions to form a current blocking layer; S6, implanting silicon ions into the sample and annealing to activate the implanted silicon ions to form a highly doped N-type ohmic contact layer; S7, applying glue on the upper surface of the highly doped N-type ohmic contact layer, and then etching to form a U-shaped groove in the middle of the square of the highly doped N-type ohmic contact layer, and etching the bottom of the groove to the low-doped N-type gallium oxide drift layer; S8, depositing an oxide dielectric layer on the sample after the U-shaped groove is formed; S9, etching and depositing the upper surface of the oxide dielectric layer on both sides of the U-shaped groove to obtain a source metal layer; S10, depositing on the lower surface of the highly doped N-type gallium oxide substrate layer, and rapidly annealing to obtain a drain metal layer; S11. In the U-shaped trench, a gate metal layer is deposited on the upper surface of the oxide dielectric layer to obtain the gallium oxide vertical trench gate MOSFET with dielectric pillars.

Citation Information

Patent Citations

  • Semiconductor device and manufacturing method therefor

    CN103201844A

  • Gallium oxide-based MOSFET device and preparation method thereof

    CN115939183A

  • Vertical-structure Ga2O3 transistor with SiO2 barrier layer and preparation method of vertical-structure Ga2O3 transistor

    CN116013989A

  • High-comprehensive-performance MOSFET (Metal-Oxide-Semiconductor Field Effect Transistor) with Schottky contact and source field plate and preparation method

    CN117038726A

  • Vertical gallium oxide transistor and preparation method thereof

    US20240079477A1