Preparation method and application of polyvinyl chloride derived chlorine atom doped carbon material
By calcining PVC transparent plates under inert argon gas and high temperature conditions to prepare polyvinyl chloride-derived chlorine atom-doped carbon materials, the problem of poor sodium storage performance of graphite in sodium-ion batteries is solved, and efficient sodium-ion battery electrode performance is achieved. promote.
Patent Information
- Application Number
- CN202411061871.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-01
AI Technical Summary
As the negative electrode of sodium-ion batteries, graphite has poor sodium storage performance. Existing preparation methods have problems such as difficulty in temperature control, production of by-products and uneven particle size distribution, which limits its development in the field of sodium-ion batteries.
Using the preparation method of polyvinyl chloride-derived chlorine atom-doped carbon material, the chlorine-doped carbon material is formed by calcining the PVC transparent plate under inert argon gas and high temperature conditions, and is activated by mixing with an activator in an argon atmosphere, accurately Build a carbon material structure to avoid structural breakdown and by-product production.
Efficient preparation of polyvinyl chloride-derived chlorine atom-doped carbon materials was achieved, which improved the storage potential and surface utilization of sodium-ion battery electrodes, reduced the ion diffusion area, and improved the performance of sodium-ion batteries.
Smart Images

Figure CN118738352A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochemical materials, and in particular relates to a preparation method and application of a polyvinyl chloride-derived chlorine atom-doped carbon material. Background Art
[0002] Carbon-based materials are the earliest skeletons used as electrodes for sodium-ion batteries. They can not only provide high conductivity and ion channels for sodium-ion batteries, but also alleviate the problem of volume expansion. Therefore, they were the first to be widely studied. However, due to the smaller interlayer spacing of graphite than the radius of sodium, the sodium storage performance of graphite as a negative electrode of the battery is poor. This limits its further development in the field of sodium-ion batteries.
[0003] At present, the more mature and complete methods include post-synthesis, in-situ synthesis, catalytic growth and template methods. Among them, post-synthesis and in-situ synthesis require a long time with the help of high-temperature atmosphere, so if the temperature cannot be accurately controlled, the yield will be relatively low, and too high temperature may cause damage to the structure of the carbon material itself that needs to be doped; the catalytic growth method uses metal catalysts that are more active in the reaction process, so in order to avoid reacting with other impurities, the preparation environment is more stringent; the template method, if the template is not enough during the reaction process, will result in a larger particle size distribution of the prepared material. Summary of the invention
[0004] In view of this, the purpose of the present invention is to propose a preparation method and application of polyvinyl chloride-derived chlorine atom-doped carbon material to solve the problem of poor sodium storage performance of graphite as a battery negative electrode in the prior art.
[0005] Based on the above purpose, the present invention provides a method for preparing a polyvinyl chloride-derived chlorine atom-doped carbon material, and the specific preparation steps are as follows:
[0006] Step (1): pre-cleaning the PVC transparent plate;
[0007] Step (2): drying the pretreated PVC transparent plate and placing it in a porcelain boat, heating it to 750° C. in an argon atmosphere and calcining it for 12 h to obtain a chlorine-doped carbon material;
[0008] Step (3): The chlorine-doped carbon material and the activator are mixed in a mass ratio of 1:6, and the temperature is raised to 400° C. in an argon atmosphere for activation for 12 hours to obtain a polyvinyl chloride-derived chlorine atom-doped carbon material.
[0009] Preferably, the specific steps of cleaning and pre-treating the PVC transparent plate in step (1) are as follows:
[0010] (a) Cut a PVC transparent plate into small cubes and put them into a low-profile flask, add 2 mol / L hydrochloric acid and seal the flask with a sealing film, stir with a magnetic stirrer for 12 h, and set the speed to 500 r / min; after 12 h, the hydrochloric acid on the surface of the PVC is completely removed and the PVC is neutral;
[0011] (b) Add 2 mol / L NaOH alkaline solution to the cleaned PVC and seal the flask with a sealing film, stir with a magnetic stirrer for 12 hours, and set the speed to 500 r / min; after 12 hours, the NaOH on the surface of the PVC is completely removed and the PVC is neutral.
[0012] Preferably, the activator is KOH.
[0013] In a second aspect, the present invention provides a polyvinyl chloride-derived chlorine atom-doped carbon material, which is prepared using the preparation method of the polyvinyl chloride-derived chlorine atom-doped carbon material.
[0014] In a third aspect, the present invention provides the use of the polyvinyl chloride-derived chlorine atom-doped carbon material in a sodium ion battery.
[0015] Furthermore, the application is specifically as follows: grinding the polyvinyl chloride-derived chlorine atom-doped carbon material, the conductive agent and the adhesive for 5-10 minutes, then dispersing them in an NMP solution, and continuing to grind for 5-10 minutes to form a homogeneous slurry; then coating the slurry on the rough side of the copper sheet, and drying it under vacuum at 40°C for 10 hours until it is completely dry, to obtain a sodium ion negative electrode material for use in sodium ion batteries.
[0016] Preferably, the mass ratio of the chlorine-doped carbon material, the conductive agent and the adhesive is 7:2:1.
[0017] Preferably, the conductive agent is carbon black and the adhesive is PVDF.
[0018] The present invention places polyvinyl chloride under inert and high temperature conditions, and pyrolyzes polyvinyl chloride to produce HCl and conjugated olefins. The conjugated olefins are broken and cyclized or further form alkyl aromatics and solid carbides between molecules. As the temperature rises, chlorine and carbonization products form chlorine-doped carbon materials. This method can effectively avoid the generation of by-products. The precise control of temperature can achieve the precise construction of the carbon material structure, avoiding the destruction of the carrier structure.
[0019] The activation step of the present invention can generate a large number of micropores, which not only allows the electrolyte to penetrate into the material to effectively improve the surface utilization of the chlorine-doped carbon material, but also reduces the ion diffusion area to obtain more sodium ion storage potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1SEM images and TEM images of the unactivated (a, c) and activated (b, d) chlorine-doped carbon materials provided in the examples ((a) and (b) are SEM images; (c) and (d) are TEM images);
[0021] Figure 2 The XRD pattern of the unactivated chlorine-doped carbon material provided in the embodiment;
[0022] Figure 3 Adsorption-desorption curves and pore size distribution relationship diagrams of the unactivated (a, b) and activated (c, d) chlorine-doped carbon materials provided in the examples ((a) and (c) are adsorption-desorption curves; (b) and (d) are pore size distribution relationship diagrams);
[0023] Figure 4 XPS graphs of activated (a) and unactivated (b) chlorine-doped carbon materials provided in the examples;
[0024] Figure 5 The electrochemical energy of the unactivated chlorine-doped carbon material at a rate of 200 mA / g (A), the electrochemical energy of the activated chlorine-doped carbon material at a rate of 1000 mA / g (B), and the electrochemical energy of the unactivated chlorine-doped carbon material at various rates (C) provided in the examples. DETAILED DESCRIPTION
[0025] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0026] Example
[0027] (1) Cut 200 mg of PVC transparent plate into small cubes and put them into a low-profile flask. Add 2 mol / L hydrochloric acid and seal the flask with a sealing film. Stir with a magnetic stirrer for 12 hours at a speed of 500 r / min. After 12 hours, collect the hydrochloric acid in the low-profile flask into a brown glass bottle for next use. Wash the PVC in the flask with alcohol three times and then with deionized water three times to completely remove the hydrochloric acid on the surface of the PVC and make it neutral.
[0028] (2) Add 2 mol / L NaOH alkaline solution to the cleaned PVC and seal the flask with a sealing film. Stir with a magnetic stirrer for 12 hours at a speed of 500 r / min. After 12 hours, collect the alkaline solution in the low-profile flask into a brown glass bottle for next use. Wash the PVC in the flask three times with alcohol and then with deionized water to completely remove the NaOH on the surface of the PVC and make it neutral.
[0029] (3) The flask was sealed with filter paper and placed in an oven for drying. The temperature was set at about 30 degrees Celsius. After the PVC was completely dried, it was placed in a porcelain boat and then placed in a tube furnace for calcination at 750 degrees Celsius under argon vacuum for 12 hours. The calcined material was collected and weighed, and the weighing result was 10 mg.
[0030] (4) The chlorine-doped carbon material obtained in (3) was mixed with an activating agent KOH in a ratio of 1:6, and then placed in a tubular furnace under argon conditions at 400°C and maintained for 12 hours for activation to obtain a polyvinyl chloride-derived chlorine atom-doped carbon material.
[0031] Preparation process of sodium ion negative electrode materials
[0032] The obtained chlorine-doped carbon material (70 mg) main material, Super P (20 mg) conductive agent and PVDF (10 mg) binder were ground for 5-10 minutes and then dispersed in NMP. After adding NMP, further continuous grinding for 10-15 minutes was performed to form a homogeneous slurry. The slurry was then coated on the rougher side of the copper sheet. The copper sheet was dried under vacuum at 40°C for 10 hours to completely dry it. Finally, the dried coated copper foil was cut into discs with a diameter of 12 mm using a battery slicer.
[0033] Electrochemical performance testing
[0034] The sodium ion battery is assembled with chlorine-doped carbon as the positive electrode, Celgard 2400 (normal membrane) as the separator and sodium negative electrode, and uses 1 mol / L NaClO4 solution prepared with propylene carbonate (PC) as the electrolyte. The battery is cycled in the voltage test range of 0.01V-3.00V. The cycle performance and rate performance are based on constant current testing.
[0035] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.
Claims
1. A method for preparing a polyvinyl chloride-derived chlorine atom-doped carbon material, characterized in that: The specific preparation steps are as follows: Step (1): pre-cleaning the PVC transparent plate; Step (2): drying the pretreated PVC transparent plate and placing it in a porcelain boat, heating it to 750° C. in an argon atmosphere and calcining it for 12 h to obtain a chlorine-doped carbon material; Step (3): The chlorine-doped carbon material and the activator are mixed in a mass ratio of 1:6, and the temperature is raised to 400° C. in an argon atmosphere for activation for 12 hours to obtain a polyvinyl chloride-derived chlorine atom-doped carbon material.
2. The method for preparing a polyvinyl chloride-derived chlorine atom-doped carbon material according to claim 1, characterized in that: The specific steps of cleaning and pre-treating the PVC transparent plate in step (1) are as follows: (a) Cut a PVC transparent plate into small cubes and put them into a low-profile flask, add 2 mol / L hydrochloric acid and seal the flask with a sealing film, stir with a magnetic stirrer for 12 h, and set the speed to 500 r / min; after 12 h, the hydrochloric acid on the surface of the PVC is completely removed and the PVC is neutral; (b) Add 2 mol / L NaOH alkaline solution to the cleaned PVC and seal the flask with a sealing film, stir with a magnetic stirrer for 12 hours, and set the speed to 500 r / min; after 12 hours, the NaOH on the surface of the PVC is completely removed and the PVC is neutral.
3. The method for preparing a polyvinyl chloride-derived chlorine atom-doped carbon material according to claim 1, characterized in that: The activating agent is KOH.
4. A polyvinyl chloride-derived chlorine atom-doped carbon material, characterized in that: The carbon material is prepared by the method for preparing a polyvinyl chloride-derived chlorine atom-doped carbon material as described in any one of claims 1 to 3.
5. Use of the polyvinyl chloride-derived chlorine atom-doped carbon material according to claim 4 in sodium ion batteries.
6. The use according to claim 5, characterized in that: The application is specifically as follows: grinding the polyvinyl chloride-derived chlorine atom-doped carbon material, the conductive agent and the adhesive for 5-10 minutes, then dispersing them in an NMP solution, and continuing to grind for 5-10 minutes to form a homogeneous slurry; then coating the slurry on the rough side of a copper sheet, and drying it under vacuum at 40° C. for 10 hours until it is completely dry, to obtain a sodium ion negative electrode material for use in a sodium ion battery.
7. The use according to claim 6, characterized in that: The mass ratio of the polyvinyl chloride-derived chlorine atom-doped carbon material, the conductive agent and the adhesive is 7:2:
1.