Preparation method of high-nickel single-crystal ternary positive electrode material

By mixing lithium sources and temperature segmented sintering technology, the problem of surface defects and lithium and nickel mixing in high-nickel single crystal cathode materials during high-temperature sintering is solved, achieving good crystallinity and electrochemical performance of high-nickel single crystal materials, and simplifying Streamline the process and reduce costs.

CN118738367APending Publication Date: 2024-10-01WANHUA CHEM GRP BATTERY TECH CO LTD +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310272339.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-21
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Traditional high-nickel single crystal ternary cathode materials are prone to surface defects and bulk lithium and nickel mixing during high-temperature and long-term sintering processes, resulting in deterioration of electrochemical performance. The existing process is complex and costly.

Method used

Using mixed lithium source delayed lithiation technology and temperature segmented one-time sintering technology, single crystal fusion and surface defect repair are respectively achieved through high-temperature short-time and low-temperature long-time segmented sintering, and the lithium-nickel mixing rate is reduced.

Benefits of technology

A high-nickel single crystal ternary cathode material with good crystallinity and excellent electrochemical properties is prepared, which simplifies the process flow, reduces material manufacturing costs, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004135143250000121
    Figure BDA0004135143250000121
  • Figure HDA0004135143270000011
    Figure HDA0004135143270000011
  • Figure HDA0004135143270000012
    Figure HDA0004135143270000012
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-nickel single-crystal ternary positive electrode material. By adopting a delayed lithiation technology of a mixed lithium source and a one-time sintering technology of temperature segmentation, the processes of single crystal fusion, particle growth and surface repair and lithium-nickel rearrangement are respectively completed through sintering at different temperatures in the one-time sintering process, and then the high-nickel single crystal ternary positive electrode material with good crystallinity and excellent electrochemical performance is prepared. Meanwhile, the method disclosed by the invention is simple in process, greatly reduces the process cost and is suitable for large-scale production and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of positive electrode materials, and specifically relates to a method for preparing a high-nickel single crystal ternary positive electrode material. Background Art

[0002] With the large-scale application of lithium-ion batteries in energy storage, consumer electronics and electric vehicles, the market demand for high energy density and long cycle performance lithium-ion batteries has become more urgent. As the core component of lithium-ion batteries, positive electrode materials play a decisive role in the overall performance of the entire battery system. At present, the most common positive electrode materials in lithium-ion batteries are lithium iron phosphate and ternary materials. Among them, ternary materials have the advantages of high energy density, good low temperature performance, and strong environmental adaptability. They have become the mainstream solution for high-end consumer electronics and automotive power batteries.

[0003] In ternary materials, due to the consideration of high specific capacity and reducing the use of expensive cobalt elements, high nickel materials with a nickel molar content of more than 80% have gradually become one of the main development directions, and their industrialization process is also accelerating. With the increase of nickel content, the degree of lithium ion deintercalation in ternary materials increases, and the specific capacity is significantly improved. However, studies have found that during deep charging and discharging, the shrinkage and expansion of various crystal anisotropies will also be more intense, which leads to local over-concentration of stress at the grain boundaries in traditional high-nickel polycrystalline ternary materials, which in turn causes microcracks in the particles and electrolyte penetration, ultimately leading to a significant attenuation of cycle and safety performance.

[0004] In order to solve this problem of high-nickel polycrystalline ternary materials, the industry usually adopts the method of preparing high-nickel single-crystal ternary positive electrode materials. Compared with polycrystalline materials, single-crystal materials eliminate the grain boundaries between primary particles, and thus have many advantages such as high mechanical strength, small specific surface area, and no volume phase stress concentration. However, single-crystal materials usually require higher sintering temperatures and longer sintering times to achieve fusion between primary particles. For single-crystal ternary positive electrode materials with low nickel content, due to the high Ni 3+ The ion content is low, the structure is stable, and the high temperature and long reaction environment have little effect on the material performance. However, when the nickel content exceeds 80%, the stable temperature of the ternary material gradually becomes lower than the synthesis temperature required for single crystal fusion. The high temperature and long sintering process will cause the hexagonal layered structure on the surface of the particles to decompose first, resulting in rock salt phase or spinel phase degradation. The volatilization of the lithium source causes the material to be lithium-deficient. At the same time, the cations in the bulk phase will be more easily mixed with lithium ions at high temperatures. These factors lead to a large number of defects on the surface and bulk of the material when the traditional high temperature and long time scheme is used to prepare high nickel single crystal ternary positive electrode materials, which leads to the deterioration of electrochemical performance.

[0005] In order to solve the limitations of such problems, there are currently two main methods for preparing high-nickel single crystal ternary positive electrode materials: one is to use a multi-step sintering method, such as the Chinese invention patent CN114899391A, which uses a solid-phase method of step-by-step calcination combined with a step-by-step lithium supplementation technology to synthesize ultra-high nickel single crystal ternary positive electrode materials. This method solves the surface degradation and bulk lithium-nickel mixing problems in the preparation process of high-nickel single crystal materials to a certain extent through secondary sintering and replenishing lithium sources, but the process requires multiple mixing and sintering, and the synthesis route is complex and time-consuming, which is not conducive to cost reduction; the second is to use a high-temperature molten salt method, such as the Chinese invention patent CN111200129A, which uses two or more molten inorganic salts as mixed molten salts to prepare high-nickel single crystal positive electrode materials. This method is essentially to protect the surface and bulk of the high-nickel single crystal by lowering the sintering temperature of the single crystal by molten salt. Since molten salts are generally halides or sulfates, they cause severe corrosion to equipment during the actual production process, and all of them are by-products after sintering, which are bonded together with the positive electrode material. A large amount of solvent is required for liquid phase separation and environmental protection treatment. These drawbacks increase production costs and have an adverse effect on material properties, limiting the large-scale use of molten salt sintering in industrial production.

[0006] Therefore, how to improve the sintering process of high-nickel single crystal materials so that it can maintain the advantages of single crystal materials while reducing the damage to the main body and surface of the material caused by the high-temperature and long-time sintering environment, while taking into account economic benefits, has become an important improvement direction for the preparation of high-nickel single crystal ternary positive electrode materials. Summary of the invention

[0007] The present invention provides a method for preparing a high-nickel single crystal ternary positive electrode material. The delayed lithiation technology of a mixed lithium source and the temperature segmented one-time sintering technology are adopted to achieve the single crystal fusion, particle growth and bulk and surface defect repair respectively through segmented sintering at different temperatures in a one-time sintering process, thereby preparing a high-nickel single crystal ternary positive electrode material with good crystallinity and excellent electrochemical performance. The method introduces two lithium sources (lithium carbonate and lithium hydroxide monohydrate) with different decomposition temperatures and activities to mix with a precursor. During the high-temperature short-time sintering process of the mixed material in the first section, the lithium hydroxide monohydrate with higher activity reacts with the precursor to achieve the fusion growth of the single crystal particle morphology, while the lithium carbonate is decomposed. Then, during the low-temperature long-time sintering process of the mixed material in the second section, the lithium oxide produced after the decomposition of lithium carbonate is used to make the surface rock salt phase or spinel phase impurities react again to form layered oxides, while completing the reduction of the bulk lithium nickel mixing rate.

[0008] The method of the present invention has a simple process flow, does not require an additional sintering process, greatly reduces the material manufacturing cost, and is suitable for large-scale production applications.

[0009] In order to achieve the above technical objectives, the present invention adopts the following scheme:

[0010] The present invention provides a method for preparing a high-nickel single crystal ternary positive electrode material, comprising the following steps:

[0011] S1. mixing a high nickel ternary hydroxide precursor material with a mixed lithium source to obtain a mixture A;

[0012] S2. In the presence of a protective atmosphere, the mixed material A is sintered once, wherein the first stage of the sintering process is set as: sintering temperature T1, sintering time t1, and the second stage of the sintering process is set as: sintering temperature T2, sintering time t2; cooling, crushing, and sieving to obtain a high-nickel single crystal ternary positive electrode material.

[0013] Furthermore, the chemical formula of the high nickel ternary hydroxide precursor material in step S1 is Ni x Co y M 1-x-y (OH)2, wherein 0.8≤x<1, 0≤y≤0.2, and the M element is at least one of Mn and Al.

[0014] Furthermore, the particle size D of the high nickel ternary hydroxide precursor material in step S1 is 50 It is preferably 2 to 8 um, and more preferably 3 to 5 um.

[0015] Furthermore, the mixed lithium source in step S1 is a mixture of lithium hydroxide monohydrate and lithium carbonate.

[0016] Furthermore, in step S1, the molar ratio of the high nickel ternary hydroxide precursor material, lithium hydroxide monohydrate and lithium carbonate is 1:(0.95-1.05):(0.005-0.05).

[0017] Furthermore, in step S2, the protective atmosphere is an oxygen-containing atmosphere, wherein the oxygen concentration is preferably greater than 80v%, more preferably greater than 90v%.

[0018] Furthermore, in step S2, the sintering is carried out in a tubular furnace, a muffle furnace, a box furnace, a rotary kiln, a push plate kiln or a roller kiln.

[0019] Furthermore, the first stage sintering process in step S2 includes the following steps: heating to a sintering temperature T1 at a heating rate of 1 to 5°C / min, and sintering for a time of t1.

[0020] Furthermore, in the first sintering process in step S2, the sintering temperature T1 = [(-500x + 1290) ± 5] ° C, the sintering time t1 = [(-600x + 900) ± 30] min, where x is the chemical formula of the high nickel ternary hydroxide precursor material in step S1, Ni xCo y M 1-x-y The molar fraction x of nickel in (OH)2.

[0021] Specifically, the first stage of the sintering process is characterized by high temperature and short time, wherein the sintering temperature T1 is slightly higher than the traditional single crystal sintering temperature, which can allow the precursor to quickly undergo a single crystal reaction with the more active lithium hydroxide monohydrate, eliminate the grain boundaries in the bulk phase, fuse the primary particles, and complete the decomposition reaction of lithium carbonate; the shorter sintering time can minimize surface degradation and lithium-nickel mixing, and reduce the lithium deficiency of the material.

[0022] Furthermore, the second sintering process in step S2 includes the following steps: cooling the temperature from sintering temperature T1 to T2 at a cooling rate of 0.5-2°C / min, and sintering for a time of t2.

[0023] Furthermore, in the second sintering process in step S2, the sintering temperature T2 = [(-600x + 1260) ± 5] ° C, the sintering time t2 = [(-600x + 1020) ± 30] min, where x is the chemical formula of the high nickel ternary hydroxide precursor material Ni in step S1. x Co y M 1-x-y The molar fraction x of nickel in (OH)2.

[0024] Specifically, the second stage sintering process is characterized by low temperature and long time, wherein the sintering temperature T2 is basically consistent with the sintering temperature of polycrystalline materials with the same nickel content. The lithium oxide produced by the decomposition of lithium carbonate can be used to allow the surface rock salt phase or spinel phase impurities to re-react to form layered oxides, thereby solving the lithium deficiency problem and surface defects of the material at high temperature. At the same time, suitable sintering experiments and longer calcination time can gradually rearrange the lithium ions and transition metal ions in the bulk phase, thereby reducing the bulk lithium-nickel mixing rate.

[0025] Compared with the prior art, the method for preparing the high-nickel single crystal ternary positive electrode material provided by the present invention has the following advantages:

[0026] The present invention introduces mixed lithium source and temperature segmented sintering technology, utilizes the different activities and decomposition temperatures of lithium hydroxide monohydrate and lithium carbonate, and reasonably sets the two-stage sintering temperature and time according to the nickel content of the material, and completes the single crystal growth and defect repair process respectively through one-step sintering. Among them, in the high-temperature sintering stage, lithium hydroxide monohydrate and the precursor react at a relatively high temperature to promote the fusion growth of the single crystal, and at the same time complete the decomposition of lithium carbonate, and the shorter sintering time avoids excessive lithium volatilization and surface degradation at high temperature; in the low-temperature sintering stage, the lithium source provided by the decomposition of lithium carbonate is used to repair the surface degradation caused by the high-temperature reaction, and the low-temperature and long-time sintering strategy can effectively reduce the lithium-nickel mixing rate of the bulk phase, so that the high-nickel single crystal ternary positive electrode material prepared by this method has good crystallinity and structural integrity, and excellent electrochemical performance.

[0027] In addition, the method of the present invention has a simple process flow, and on the basis of improving the performance of high-nickel single crystal ternary positive electrode materials, it greatly reduces the material manufacturing cost and is suitable for large-scale production applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a SEM image of the high-nickel single crystal ternary positive electrode material prepared in Example 1;

[0029] Figure 2 XRD patterns of the three materials obtained in Example 1, Comparative Example 1 and Comparative Example 3;

[0030] Figure 3 This is a SEM image of the ternary positive electrode material prepared in Comparative Example 2;

[0031] Figure 4 This is a SEM image of the high-nickel single crystal ternary positive electrode material prepared in Comparative Example 1;

[0032] Figure 5 This is a SEM image of the high-nickel single crystal ternary positive electrode material prepared in Comparative Example 5;

[0033] Figure 6 This is the SEM image of the high-nickel single crystal ternary positive electrode material prepared in Comparative Example 7. DETAILED DESCRIPTION

[0034] The present invention will be further described below in conjunction with examples, but the present invention is not limited to the following examples.

[0035] The material XRD data was tested by Malvern Aeris desktop XRD tester, and the data was calculated by Highscore Plus software. The SEM results were tested by Phenom Pro desktop electron scanning microscope, and the lithium content ICP data was tested by PEAvio 500.

[0036] Embodiment 1:

[0037] The method for preparing the high nickel single crystal ternary positive electrode material in this embodiment comprises the following steps:

[0038] S1, take 1 mol, D 50 4.5um high nickel ternary hydroxide precursor material Ni 0.83 Co 0.13 Mn 0.04 (OH)2 is mixed with a mixed lithium source consisting of 1.04 mol of lithium hydroxide monohydrate and 0.005 mol of lithium carbonate to obtain a mixture A;

[0039] S2. Put the mixed material A obtained in S1 into a tubular furnace, control the oxygen concentration in the furnace to 92%, and set the sintering process as follows: increase the temperature to T1=875°C at a heating rate of 3°C / min, and sintering time t1=400min, then reduce the temperature to T2=760°C at a heating rate of 2°C / min, and sintering time t2=520min. The material obtained after natural cooling is crushed and sieved to obtain a high-nickel single crystal ternary positive electrode material.

[0040] Embodiment 2:

[0041] The method for preparing the high nickel single crystal ternary positive electrode material in this embodiment comprises the following steps:

[0042] S1, take 10mol, D 50 4um high nickel ternary hydroxide precursor material LiNi 0.9 Co 0.05 Mn 0.05 (OH)2 is mixed with a mixed lithium source consisting of 10.25 mol of lithium hydroxide monohydrate and 0.1 mol of lithium carbonate to obtain a mixture A;

[0043] S2. Put the mixed material A obtained in S1 into a box furnace, control the oxygen concentration in the furnace to 94%, and set the sintering process as follows: increase the temperature to T1=840°C at a heating rate of 2.5°C / min, and sintering time t1=360min, then reduce the temperature to T2=720°C at a heating rate of 1.5°C / min, and sintering time t2=480min. The material obtained after natural cooling is crushed and sieved to obtain a high-nickel single crystal ternary positive electrode material.

[0044] Embodiment 3:

[0045] The method for preparing the high nickel single crystal ternary positive electrode material in this embodiment comprises the following steps:

[0046] S1, take 10mol, D 50 3.7um high nickel ternary hydroxide precursor material LiNi 0.92 Co 0.04Mn 0.04 (OH)2 is mixed with a mixed lithium source consisting of 10.1 mol of lithium hydroxide monohydrate and 0.15 mol of lithium carbonate to obtain a mixture A;

[0047] S2. Put the mixed material A obtained in S1 into a box furnace, control the oxygen concentration in the furnace to 95%, and set the sintering process as follows: increase the temperature to T1=825°C at a heating rate of 2°C / min, and sintering time t1=350min, then reduce the temperature to T2=710°C at a heating rate of 1.25°C / min, and sintering time t2=465min. The material obtained after natural cooling is crushed and sieved to obtain a high-nickel single crystal ternary positive electrode material.

[0048] Embodiment 4:

[0049] The method for preparing the high nickel single crystal ternary positive electrode material in this embodiment comprises the following steps:

[0050] S1, take 100 mol, D 50 3.5um high nickel ternary hydroxide precursor material LiNi 0.95 Co 0.03 Mn 0.02 (OH)2 is mixed with a mixed lithium source consisting of 100.5 mol of lithium hydroxide monohydrate and 2 mol of lithium carbonate to obtain a mixture A;

[0051] S2. The mixed material A obtained in S1 is divided into four batches and loaded into a sagger and placed in a roller kiln. The oxygen concentration in the kiln is controlled to be 97%. The sintering process is set as follows: the temperature is increased to T1=815°C at a heating rate of 1.5°C / min, and the sintering time is t1=330min. Thereafter, the temperature is reduced to T2=690°C at a heating rate of 0.75°C / min, and the sintering time is t2=450min. The material obtained after cooling is crushed and sieved to obtain a high-nickel single crystal ternary positive electrode material.

[0052] Comparative Example 1:

[0053] The method for preparing the high nickel single crystal ternary positive electrode material in this embodiment comprises the following steps:

[0054] S1, take 1 mol, D 50 4.5um high nickel ternary hydroxide precursor material Ni 0.83 Co 0.13 Mn 0.04 (OH)2 is mixed with a mixed lithium source consisting of 1.04 mol of lithium hydroxide monohydrate and 0.005 mol of lithium carbonate to obtain a mixture A;

[0055] S2. Put the mixed material A obtained in S1 into a tubular furnace, control the oxygen concentration in the furnace to 92%, set the sintering process as follows: increase the temperature to T = 875 ° C at a heating rate of 3 ° C / min, and sinter for t = 400 min. The material obtained after natural cooling is crushed and sieved to obtain the material of comparative example 1.

[0056] Comparative Example 2:

[0057] The method for preparing the high nickel single crystal ternary positive electrode material in this embodiment comprises the following steps:

[0058] S1, take 1 mol, D 50 4.5um high nickel ternary hydroxide precursor material Ni 0.83 Co 0.13 Mn 0.04 (OH)2 is mixed with a mixed lithium source consisting of 1.04 mol of lithium hydroxide monohydrate and 0.005 mol of lithium carbonate to obtain a mixture A;

[0059] S2. Put the mixed material A obtained in S1 into a tubular furnace, control the oxygen concentration in the furnace to 92%, set the sintering process as follows: increase the temperature to T = 760 ° C at a heating rate of 3 ° C / min, and sinter for t = 520 min. The material obtained after natural cooling is crushed and sieved to obtain the material of comparative example 2.

[0060] Comparative Example 3:

[0061] The method for preparing the high nickel single crystal ternary positive electrode material in this embodiment comprises the following steps:

[0062] S1, take 1 mol, D 50 4.5um high nickel ternary hydroxide precursor material Ni 0.83 Co 0.13 Mn 0.04 (OH)2 is mixed with 1.045 mol of lithium hydroxide monohydrate to obtain a mixture A;

[0063] S2. Put the mixed material A obtained in S1 into a tubular furnace, control the oxygen concentration in the furnace to 92%, set the sintering process as follows: increase the temperature to T = 850 ° C at a heating rate of 3 ° C / min, and sinter for t = 900 min. The material obtained after natural cooling is crushed and sieved to obtain the material of comparative example 3.

[0064] Comparative Example 4:

[0065] The difference between this comparative example and Example 1 is that the lithium source in step S1 is 1.05 mol of lithium hydroxide monohydrate.

[0066] Comparative Example 5:

[0067] The difference between this comparative example and Example 1 is that the lithium source in step S1 is 0.525 mol of lithium carbonate.

[0068] Comparative Example 6:

[0069] The difference between this comparative example and Example 1 is that the sintering time t1 in step S2 is 500 min.

[0070] Comparative Example 7:

[0071] The difference between this comparative example and Example 1 is that the sintering time t1 in step S2 is 300 min.

[0072] from Figure 1 It can be seen that the single crystal grows well and the particles are distinct, which is different from the single crystal material obtained by the traditional sintering scheme in Comparative Example 3 ( Figure 4 ), indicating that the method provided by the present invention can be used to obtain a high-nickel single crystal ternary positive electrode material with good morphology.

[0073] from Figure 2 It can be seen that the materials obtained in Comparative Examples 1 and 3 have obvious rock salt phase impurity peaks. Among them: the comparison of the results of Example 1 and Comparative Example 1 shows that the second stage of low-temperature long-time sintering adopted by the present invention can effectively restore the surface degradation and structural defects caused by the first stage of high-temperature short-time sintering, proving the rationality of the process; the comparison of the results of Example 1 and Comparative Example 3 shows that compared with the single crystal material obtained by the traditional sintering of Comparative Example 3, the method provided by the present invention can obtain a high-nickel single crystal ternary positive electrode material with better crystallinity and fewer defects.

[0074] from Figure 3 It can be seen that no single crystal is generated, but a polycrystalline secondary spherical particle morphology, which is different from Example 1 ( Figure 1 ) comparison shows that the first stage of high-temperature short-time sintering of the present invention is mainly for the formation of single crystal particle morphology, and the second stage of low-temperature long-time sintering is mainly for repairing structural defects. The organic combination of the two-stage sintering process can obtain a high-nickel single crystal ternary positive electrode material with good morphology.

[0075] Table 1 is a comparison of the performance of the ternary positive electrode materials prepared in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3 of the present invention. From the physicochemical indicators, it can be seen that the material obtained by the method provided by the present invention has higher I (003) / I (104) The value and lower lithium-nickel mixing rate are basically consistent with the polycrystalline material of Comparative Example 2, indicating that it has better crystallinity and the structural integrity can reach the level of polycrystalline materials. From the thermal safety and electrochemical performance, it can be seen that the high-nickel single crystal positive electrode material obtained by the method provided by the present invention has obvious advantages in the first-week discharge capacity and first effect while maintaining a higher DSC exothermic temperature and more stable long-cycle performance.

[0076] Table 2 is a comparison of the physicochemical indicators of the ternary positive electrode materials prepared in Example 1, Comparative Example 4 and Comparative Example 5 of the present invention. It can be seen that the material I obtained in Comparative Example 4 using only lithium hydroxide monohydrate as the lithium source is (003) / I (104) The value is low, the lithium-nickel mixing rate is high, and the lithium content in the material is less than 1. This is because the monohydrated lithium hydroxide is highly active, fully participates in the reaction in the high temperature section, and is easy to volatilize. However, the material will undergo surface degradation and structural defects in the high temperature section, resulting in the loss of active lithium. There is no additional lithium source in the low temperature section for lithium supplementation reaction, which then causes the material to be lithium-deficient and has poor crystallinity. In addition, the lithium content of the material obtained in Comparative Example 5, which only uses lithium carbonate as the lithium source, is significantly higher. Figure 5 It can be seen that due to the high decomposition temperature of lithium carbonate, low activity, small single crystal size of the material, poor dispersion, and the presence of obvious lithium carbonate on the surface that did not participate in the reaction, the "concave-convex" morphology caused by the residue, the main reason for its high lithium content is that there is a lot of residual lithium on the surface that has not entered the interior of the lattice, so its crystallinity is still poor, such as I (003) / I (104) The two comparative examples prove that only by using mixed lithium sources with different activities and reasonably controlling the proportion of use can the technical effect of the present invention be achieved.

[0077] Table 3 is a comparison of the physicochemical indicators of the ternary positive electrode materials prepared in Example 1, Comparative Example 6 and Comparative Example 7 of the present invention. It can be seen that when the sintering time of the high temperature section of Comparative Example 6 is too long, the crystallinity of the material decreases, and when the sintering time of the high temperature section of Comparative Example 7 is too short, the crystallinity of the material remains basically unchanged. Figure 6 The SEM images show that the single crystal particle size of the material is obviously small and the dispersion is poor. These two comparative examples prove that only by adopting the reasonable sintering parameters provided by the present invention can the technical effect be achieved.

[0078] Table 1 Comparison of performance of ternary positive electrode materials in Example 1 Comparative Examples 1-3

[0079]

[0080] Table 2 Comparison of physical and chemical indicators of ternary positive electrode materials in Example 1, Comparative Examples 4-5

[0081] Test items <![CDATA[I (003) / I (104) ]]> Li-Ni mixing rate (%) <![CDATA[Li (ICP) Content (mol%)]]> Example 1 1.490 1.996 1.011 Comparative Example 4 1.446 2.024 0.962 Comparative Example 5 1.423 2.112 1.038

[0082] Table 3 Comparison of physicochemical indicators of ternary positive electrode materials in Example 1, Comparative Examples 6-7

[0083] Test items <![CDATA[I (003) / I (104) ]]> Li-Ni mixing rate (%) Example 1 1.490 1.996 Comparative Example 6 1.467 2.011 Comparative Example 7 1.488 1.995

Claims

1. A method for preparing a high-nickel single crystal ternary positive electrode material, comprising the following steps: S1. mixing a high nickel ternary hydroxide precursor material with a mixed lithium source to obtain a mixture A; S2. In the presence of a protective atmosphere, the mixed material A is sintered once, wherein the first stage of the sintering process is set as: sintering temperature T1, sintering time t1, and the second stage of the sintering process is set as: sintering temperature T2, sintering time t2; cooling, crushing, and sieving to obtain a high-nickel single crystal ternary positive electrode material.

2. The method according to claim 1, characterized in that The chemical formula of the high nickel ternary hydroxide precursor material in step S1 is Ni x Co y M 1-x-y (OH)2, wherein 0.8≤x<1, 0≤y≤0.2, and the M element is at least one of Mn and Al.

3. The method according to claim 1 or 2, characterized in that: The particle size D of the high nickel ternary hydroxide precursor material in step S1 is 50 It is preferably 2 to 8 um, and more preferably 3 to 5 um.

4. The method according to any one of claims 1 to 3, characterized in that: The mixed lithium source in step S1 is a mixture of lithium hydroxide monohydrate and lithium carbonate.

5. The method according to any one of claims 1 to 4, characterized in that: In the step S1, the molar ratio of the high nickel ternary hydroxide precursor material, lithium hydroxide monohydrate and lithium carbonate is 1:(0.95-1.05):(0.005-0.05).

6. The method according to any one of claims 1 to 5, characterized in that: In the first sintering process in step S2, the sintering temperature T1 = [(-500x + 1290) ± 5] ° C, the sintering time t1 = [(-600x + 900) ± 30] min, where x is the chemical formula of the high nickel ternary hydroxide precursor material in step S1, Ni x Co y M 1-x-y The molar fraction x of nickel in (OH)2.

7. The method according to any one of claims 1 to 6, characterized in that: In the second sintering process in step S2, the sintering temperature T2 = [(-600x + 1260) ± 5] ° C, the sintering time t2 = [(-600x + 1020) ± 30] min, where x is the chemical formula of the high nickel ternary hydroxide precursor material Ni in step S1. x Co y M 1-x-y The molar fraction x of nickel in (OH)2.

8. The method according to any one of claims 1 to 7, characterized in that: The protective atmosphere in step S2 is an oxygen-containing atmosphere, wherein the oxygen concentration is preferably greater than 80v%, more preferably greater than 90v%.

9. The method according to any one of claims 1 to 8, characterized in that: In the first sintering process in step S2, the temperature is raised to the sintering temperature T1 at a heating rate of 1-5°C / min.

10. The method according to any one of claims 1 to 9, characterized in that: In the second sintering process in step S2, the temperature is lowered from sintering temperature T1 to T2 at a cooling rate of 0.5-2°C / min.

Citation Information

Cited By

  • Monocrystal ternary positive electrode material and preparation method thereof

    CN119920875A