Positive electrode material, preparation method thereof, positive electrode plate and electrochemical device

By forming a coating layer on the nickel-cobalt-manganese ternary material, the problem of poor structural stability of high-nickel cathode materials during the charge and discharge process is solved, achieving both high energy density and good electrochemical performance, and improving the cycle performance of the material. and thermal stability.

CN118738368APending Publication Date: 2024-10-01ENVISION DYNAMICS TECH (JIANGSU) CO LTD +1
View PDF 0 Cites 7 Cited by

Patent Information

Application Number
CN202310325762.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

High-nickel cathode materials have poor structural stability during the charge and discharge process, and are prone to lattice distortion and powdering, which affects their cycle performance and thermal stability.

Method used

The nickel-cobalt-manganese ternary material is used as the first material, and the coating layer is formed through two sinterings. The Co element is combined with other coating elements to form a second material coating layer with smaller particles on the surface to improve the stability of the material interface. and electrochemical performance.

Benefits of technology

It achieves both high energy density and good electrochemical performance, improves the specific capacity, cycle performance and thermal stability of the material, and overcomes the problem of insufficient structural stability of high-nickel cathode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738368A_ABST
    Figure CN118738368A_ABST
Patent Text Reader

Abstract

The invention provides a positive electrode material and a preparation method thereof, a positive electrode plate and an electrochemical device, and belongs to the technical field of lithium ion batteries, and the positive electrode material comprises a first substance and a second substance. Wherein the first substance comprises a nickel-cobalt-manganese ternary material; the particle size of the second substance is smaller than that of the first substance, the second substance is attached to the surface of the first substance, the second substance comprises a coating element combination, and the coating element combination comprises Co element. According to the positive electrode material, the preparation method of the positive electrode material, the positive electrode plate and the electrochemical device, the Co element and other elements are matched on the surface of the nickel-cobalt-manganese ternary material through two times of sintering to form a second substance coating layer with smaller particles, so that the surface defects of the material are repaired while the usage amount of the Co element in the high-nickel ternary material is reduced; the high energy density and good electrochemical performance are considered while the interface stability of the material is improved, so that the positive electrode material with high specific capacity, good cycle performance and excellent thermal stability is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a positive electrode material and a preparation method thereof, a positive electrode plate and an electrochemical device. Background Art

[0002] As a highly efficient energy storage device, lithium-ion batteries have been widely used in portable electronic digital products and electric vehicles, and play an increasingly important role in today's society.

[0003] As we all know, in NCM&NCA layered ternary positive electrode materials, the higher the nickel content, the higher the specific capacity. In order to cope with the decline in subsidies and market competition, the current mainstream direction in the industry is to use high nickel (hereinafter referred to as 811) or even ultra-high nickel (hereinafter referred to as 9 series) positive electrode materials to improve the energy density of the battery cell, but the safety performance, cycle performance, rate performance and thermal stability of high nickel positive electrode materials will decrease with the increase of nickel content. Among them, the residual lithium on the surface of high nickel positive electrode materials is high, and the side reactions between the interface and the electrolyte are deepened. Excessive side reactions will endanger the safety performance and service life of the battery, and too low cobalt content will cause diffusion barriers for lithium ions in the lattice, bringing serious kinetic hysteresis problems. At the same time, it will also reduce the stability of the crystal structure, increase the lattice distortion during charging and discharging, and affect the overall electrochemical performance of the material.

[0004] The high-nickel positive electrode material currently obtained using the conventional ternary positive electrode preparation process is limited by the stability defects of the high-nickel positive electrode material's own layered structure. Its material lattice is easily distorted during the charging and discharging process, which accelerates the particle pulverization and disintegration, causing the material's cycle performance, storage performance and thermal stability to deteriorate rapidly.

[0005] Therefore, it is necessary to design a positive electrode material and a preparation method thereof to solve the above problems. Summary of the invention

[0006] In view of the above shortcomings of the prior art, the present invention provides a positive electrode material and a preparation method thereof, a positive electrode plate and an electrochemical device, which can provide and prepare a high-nickel positive electrode material that has both high energy density and good electrochemical performance, thereby solving the technical problems that the high-nickel positive electrode material prepared by the prior art has poor structural stability and is prone to lattice distortion and material pulverization during the charging and discharging process.

[0007] To achieve the above object and other related objects, the present invention provides a positive electrode material, which includes a first substance and a second substance.

[0008] Wherein, the first substance comprises a nickel-cobalt-manganese ternary material, and the nickel-cobalt-manganese ternary material is LiNi x Co y Mn zO2, wherein 0.7≤x<1, 0≤y<0.3, z=1-xy; the particle size of the second substance is smaller than that of the first substance, the second substance is attached to the surface of the first substance, the second substance comprises a coating element combination, the coating element combination comprises at least two coating element coating element combinations, and the coating element combination comprises at least Co element.

[0009] In one example of the present invention, the chemical formula of the second substance is LiN x Co y O 2-b A b , 0.7≤x<1, 0≤y<0.3, 0≤b<0.1; wherein the coating elements contained in the N element include one or more of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce, and the A element includes one or more of F, N, Cl, S and P.

[0010] In one example of the present invention, the N element, in addition to the coating element, includes one or more of Mg, Sr, V, Se, Rh, Pd, Sb, Te, Ca, Zn, Ni, Mn and Zr.

[0011] In one example of the present invention, the coating element combination in the second substance is attached to the first substance through two sinterings; the first element combination in the coating elements is attached to the first substance through the first sintering, and the second element combination in the coating elements is attached to the first substance through the second sintering, and the first element combination includes the Co element.

[0012] In one example of the present invention, the first element combination includes Co and one or more of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce; the second element combination includes at least two combinations of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce.

[0013] In one example of the present invention, the second substance includes a first coating element, a second coating element and a third coating element, the first coating element is Co or a combination of Co and B, the second coating element is Al, and the third coating element includes one or more of W, Sn, Pb, Mg and Nb.

[0014] In one example of the present invention, the content of the first coating element in the positive electrode material is 100 to 30000 ppm, the content of the second coating element in the positive electrode material is 200 to 5000 ppm, and the content of the third coating element in the positive electrode material is 200 to 5000 ppm.

[0015] In an example of the present invention, the Co element in the second substance is at least partially located inside the first substance.

[0016] In an example of the present invention, the penetration depth of the coating element of the second substance in the first substance is 260 to 650 nm.

[0017] In an example of the present invention, the content of Co element in the positive electrode material is 5000 to 15000 ppm.

[0018] In one example of the present invention, the nickel-cobalt-manganese ternary material is doped with doping elements, and the doping elements include one or more of Zr, Mg, W, Ti, Al, Sr, Rb, Ru and Y.

[0019] In one example of the present invention, the doping element is embedded in the single crystal lattice of the nickel-cobalt-manganese ternary material.

[0020] In one example of the present invention, the doping elements include a first doping element, a second doping element and a third doping element; the first doping element includes one or more of Zr, Ti, Nb and Mg, the second doping element includes one or more of Sr, Ru and Sn, and the third doping element includes one or more of Y, Ti and W.

[0021] In one example of the present invention, the content of the first doping element in the positive electrode material is 1000 to 5000 ppm, the content of the second doping element in the positive electrode material is 100 to 2000 ppm, and the content of the third doping element in the positive electrode material is 100 to 3000 ppm.

[0022] Another aspect of the present invention provides a method for preparing a positive electrode material, wherein the method prepares the positive electrode material described in any of the above examples, and the method comprises the following steps: mixing the first substance with at least two coating element sources corresponding to the coating element combination respectively and coating and sintering twice to form a second substance coating layer on the surface of the first substance; the first substance is a nickel-cobalt-manganese ternary material; the nickel-cobalt-manganese ternary material is LiNi x Co y Mn z O2, wherein 0.7≤x<1, 0≤y<0.3, z=1-xy, the coating element combination includes at least two coating elements, the coating element source is a compound carrying the coating element, and the coating element includes Co.

[0023] In one example of the present invention, before the two coating sintering, a first substance is further prepared, and the preparation of the first substance includes: mixing a nickel-cobalt-manganese ternary material precursor with a lithium source and a doping element source and then performing doping sintering to obtain the first substance, wherein the nickel-cobalt-manganese ternary material precursor is LiNi x Co y Mn z (OH)2, wherein 0.7≤x<1, 0≤y<0.3, x+y+z=1; the doping elements include one or more of Zr, Mg, W, Ti, Al, Sr, Rb, Ru and Y.

[0024] In one example of the present invention, the coating element also includes one or more of Al, W, Ti, Ru, La, Y, Nb, Mo, B, and Ce.

[0025] In one example of the present invention, the first coating sintering causes the first element combination of the coating element combination to adhere to the surface of the first material, and the second coating sintering causes the second element combination of the coating element combination to react with the first element combination on the surface of the first material to generate the second material coating layer, and the first element combination includes Co.

[0026] In one example of the present invention, the sintering temperature of the second coating sintering is lower than the sintering temperature of the first coating sintering, the first coating sintering temperature is 500-800°C, the first coating sintering cycle is 18-26h, the second coating sintering temperature is 300-600°C, and the second coating sintering cycle is 18-26h.

[0027] In one example of the present invention, the first element combination includes Co and one or more of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce; the second element combination includes at least two combinations of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce.

[0028] The present invention also provides a positive electrode plate, which includes a positive electrode current collector and a positive electrode active material layer. The positive electrode active material layer is made of the positive electrode material described in any of the above examples, or the positive electrode material prepared by the preparation method described in any of the above examples.

[0029] The present invention also provides an electrochemical device, which includes a negative electrode plate, a separator, an electrolyte, and a positive electrode plate as described in any one of the above examples.

[0030] The positive electrode material and its preparation method, positive electrode plate and electrochemical device in the present invention are sintered twice to make Co element cooperate with other elements on the surface of nickel-cobalt-manganese ternary material to form a second material coating layer with smaller particles, so as to reduce the usage of Co element in high-nickel ternary material while repairing the surface defects of the material, improve the material interface stability while taking into account high energy density and good electrochemical performance, so as to obtain a positive electrode material with high specific capacity, good cycle performance and excellent thermal stability. Therefore, the present invention effectively overcomes some practical problems in the prior art and has high utilization value and use significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 This is a scanning electron microscope test image of the positive electrode material in the present invention.

[0033] Figure 2 It is a schematic diagram of the process of preparing the positive electrode material in the present invention.

[0034] Figure 3 This is a graph showing the test results of charge and discharge gram capacity of secondary batteries equipped with the positive electrode materials of Examples 1 to 2 and Comparative Examples 1 to 4 of the present invention. DETAILED DESCRIPTION

[0035] The following is an explanation of the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the features in the following embodiments and the embodiments can be combined with each other without conflict. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods for which specific conditions are not specified in the following examples are usually carried out under conventional conditions or according to the conditions recommended by the manufacturers.

[0036] It should be noted that the terms such as "upper", "lower", "left", "right", "middle" and "one" etc. used in this specification are only for the convenience of description and are not intended to limit the scope of implementation of the present invention. Changes or adjustments to their relative relationships, without substantially changing the technical content, should also be regarded as the scope of implementation of the present invention.

[0037] The present invention relates to a cathode material, a preparation method thereof, a cathode electrode sheet, and an electrochemical device. By means of two sintering processes, Co elements are combined with coating elements at different sintering temperatures to form a second material coating layer with smaller particles on the surface of the nickel-cobalt-manganese ternary material, so as to form a coating layer with a high coating amount on the surface of the nickel-cobalt-manganese ternary material with a lower Co element usage amount, while stabilizing the lattice strength and interface stability of the high-nickel cathode material and ensuring the high specific capacity and high energy density of the material.

[0038] Please refer to Figure 1 , the cathode material of the present invention is a high-nickel ternary cathode material, specifically a nickel-cobalt-manganese ternary material with a high nickel content. The cathode material includes a first material and a second material. The first material is a nickel-cobalt-manganese ternary material, and the nickel-cobalt-manganese ternary material is LiNi x Co y Mn z O2, where 0.7 ≤ x < 1, 0 ≤ y < 0.3, z = 1 - x - y. The second material is attached to the surface of the first material as a coating layer. The particle size of the second material is smaller than that of the first material. The second material contains a coating element combination, and the coating element combination contains at least two coating elements. The coating element combination in the second material contains Co elements.

[0039] Among them, the chemical formula of the cathode material is Li 1+a [Ni x Co y Mn z M 1-x-y-z O 2-b A b , where 0.7 ≤ x < 1, 0 ≤ y < 0.3, 0 ≤ z < 0.3, -0.2 < a < 0.2, 0 ≤ b < 0.1. In an optional embodiment, the cathode material is preferably Li 1+a [Ni x Co y Mn z M 1-x-y-z O 2-b A b , where 0.8 ≤ x < 1, 0 ≤ y < 0.1, 0 ≤ z < 0.2, -0.2 < a < 0.2, 0 ≤ b < 0.2; further, the cathode material can be Li 1+a [Ni x Co y Mn z M 1-x-y-z O 2-b A b , where 0.88 ≤ x < 1, 0 < y ≤ 0.1, 0 ≤ z < 0.1, -0.2 < a < 0.2, 0 ≤ b < 0.2.

[0040] In some embodiments, the M element in the positive electrode material is selected from any one or more of Sr, Y, Al, Ti, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Ni, Co, Mn and Zr. That is, the M element can be any one of the element types listed above, such as Al, Co, Ti, Zr, Mg, Sr, W, Mo, B, Nb, Sr, Rb, Ru or Y, etc., and the M element can be any two or more combinations of the element types listed above, for example, the M element is a combination of Sn and Zr, or a combination of Ti and W, or a combination of Nb and Sn, or a combination of Nb, Ru and Y, or a combination of Mg, Sr and Y, or a combination of Mg, Ti, Sr and W, etc., which are not listed one by one here.

[0041] The A element in the positive electrode material is selected from any one or more of F, N, Cl, S and P. That is, the A element can be any one of the element types listed above, such as F, N, Cl, S or P, etc.; the A element can be any combination of two or more of the element types listed above, for example, the A element is a combination of S and Cl, or a combination of F and S, or a combination of N and Cl, or a combination of S, P and Cl, or a combination of S, N, F and Cl, etc., which are not listed here one by one.

[0042] In addition, when the A element and the M element are two or more combinations, there is no restriction on the ratio of each element in the combination, and they can be mixed in any ratio, etc. In other embodiments, the A element and the M element can also be element types not listed above.

[0043] The coating elements contained in the second material include one or more of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce in addition to Co. Among them, the coating element Co and one or more of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce are combined by sintering to react and recombine with the nickel-cobalt-manganese ternary material on the surface of the first material to form the second material, so as to form a second material coating layer with a higher coating amount on the surface of the first material with a lower usage amount of Co element, and obtain a positive electrode material with high specific capacity, good conductivity, excellent cycle and thermal stability.

[0044] In some embodiments, the chemical formula of the second substance is LiN x Co y O 2-b A b, 0.7≤x<1, 0≤y<0.3, 0≤b<0.1; wherein, the N element may be a coating element or a metal element or doping element of the nickel-cobalt-manganese ternary material in the first substance, the coating element contained in the N element is one or more of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce, the N element includes one or more of Mg, Sr, V, Se, Rh, Pd, Sb, Te, Ca, Zn, Ni, Mn and Zr in addition to the coating element, and the A element includes one or more of F, N, Cl, S and P. In the above-mentioned second substance, the metal element or doping element of the nickel-cobalt-manganese ternary material contained in the A element and the N element is introduced into the second substance when the coating element reacts and adheres to the surface of the first substance.

[0045] In some embodiments, the N element in the second material is selected from any one or more of Ni, Mn, Zr, Y, Al, Ti, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca and Zn. That is, the N element can be any one of the element types listed above, such as Al, W, Ti, Ru, La, Y, Nb, Mo, B, Mn, Ni or Ce, etc. The N element can be any combination of two or more of the element types listed above, for example, the N element is a combination of Mn and Nb, or a combination of Al and Mo, or a combination of Ru and Pd, or a combination of Nb, Mo and Zn, or a combination of W, La and Se, or a combination of Nb, Ti, Ce and Zr, etc., which are not listed here one by one.

[0046] The A element in the second substance is selected from any one or more of F, N, Cl, S and P. That is, the A element can be any one of the element types listed above, such as F, N, Cl, S or P, etc.; the A element can be any combination of two or more of the element types listed above, for example, the A element is a combination of S and Cl, or a combination of F and S, or a combination of N and Cl, or a combination of S, P and Cl, or a combination of S, N, F and Cl, etc., which are not listed here one by one.

[0047] In addition, when the N element and the A element are two or more combinations, there is no restriction on the ratio of each element in the combination, and they can be mixed in any ratio, etc. In other embodiments, the N element and the A element can also be element types not listed above.

[0048] In some embodiments, the Co element in the second substance is at least partially located inside the first substance, the Co element partially located on the surface of the first substance is evenly distributed in the form of a second substance compound, and the Co element partially located inside the first substance is evenly embedded in the lattice of the nickel-cobalt-manganese ternary material. The surface Co element content in the positive electrode material is 5000 to 15000 ppm, and the penetration depth of the coating element in the second substance in the first substance is 260 to 650 nm.

[0049] In some embodiments, the coating element combination in the second substance is attached to the first substance through two sinterings, the first element combination in the coating element combination is attached to the first substance through the first sintering, and the second element group in the coating element combination forms a second substance coating layer on the surface of the first substance together with the first element combination through the second sintering. Wherein, the first element combination contains the Co element, and the first element combination carries the Co element and first attaches to the surface of the first substance at a higher sintering temperature in the first sintering, and then the coating element in the second element group forms a second substance coating layer on the surface of the first substance together with the coating element of the first element combination at a lower sintering temperature in the second sintering. Through two sinterings, the Co element and the coating elements of different sintering temperatures can be combined in the second substance attached to the surface of the first substance, thereby effectively increasing the coating amount of the Co element on the surface of the first substance, while preventing Co from excessively penetrating into the crystal lattice or grain boundary of the first substance at a high sintering temperature, causing the surface of the positive electrode material to lose activity, and reducing the specific capacity and cycle performance of the positive electrode material.

[0050] In some examples of this embodiment, the first element combination includes Co and one or more of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce, for example, a combination of Co and B, a combination of Co and Al, or a combination of Co, B and Al; the second element combination includes at least two combinations of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce, for example, a combination of Nb and Al, a combination of Al and Y, or a combination of Y, W and Al.

[0051] In this embodiment, the first element combination includes a first coating element and a second coating element, and the second element group includes a second coating element and a third coating element. The first coating element is Co or a combination of Co and B, the second coating element is Al, and the third coating element includes one or more of W, Sn, Pb, Mg and Nb. Preferably, the mass ratio of the first coating element, the second coating element and the third coating element is (0.1 to 100): (0.04 to 25): 1; further, based on the mass of the positive electrode material, the content of the first coating element is 100 to 30000 ppm, the content of the second coating element is 200 to 5000 ppm, and the content of the third coating element is 200 to 5000 ppm.

[0052] In addition, the applicant found that in the positive electrode material, the amount of Co element coated on the surface of the nickel-cobalt-manganese ternary material directly affects the kinetic properties of the material. If the amount of Co element coated on the surface of the nickel-cobalt-manganese ternary material is too low, the material will have high direct current resistance (DCR) performance and poor surface performance, while if the amount of Co element coated is too high, the material will have serious lattice mixing and excessive distortion, and will be easy to powder and disintegrate. Therefore, in some embodiments of the present application, the positive electrode material, on the one hand, uses Co element and other coating elements to form a second material coating layer on the surface of the first material to ensure the stability of the interface of the first material while reducing the amount of Co element used. On the other hand, the first material is doped with doping elements to improve the crystallinity and lattice strength of the material and avoid lattice mixing caused by excessive coating of Co element.

[0053] The first substance of the positive electrode material is doped with doping elements, and the doping elements include any one or a combination of Zr, Mg, W, Ti, Al, Sr, Rb, Ru and Y, for example, a combination of Zr, Sr and W, a combination of Nb, Sn and Y, or a combination of Zr, Y and Al, etc., which are not listed here one by one. The doping elements are uniformly embedded in the lattice of the first substance through sintering, and the doping elements form a "pinning" effect on the lattice inside the first substance, which greatly improves the lattice strength of the material, thereby avoiding lattice mixing caused by excessive coating of the Co element.

[0054] In some embodiments, the doping elements in the first substance include a first doping element, a second doping element, and a third doping element; the first doping element includes one or more combinations of Zr, Ti, Nb, and Mg, the second doping element includes one or more combinations of Sr, Ru, and Sn, and the third doping element includes one or more combinations of Y, Ti, and W. In the doping sintering process, the mass ratio of the first doping element, the second doping element, and the third doping element mixed into the nickel-cobalt-manganese ternary material precursor is 1: (0.02 to 2): (0.02 to 3); further, based on the mass of the positive electrode material, the content of the first doping element is 1000 to 5000 ppm, the content of the second doping element is 100 to 2000 ppm, and the content of the third doping element is 100 to 3000 ppm.

[0055] In the above embodiment, preferably, the first doping element in the doping elements of the positive electrode material is Zr, the second doping element is Sr, and the third doping element is Y. Wherein, based on the mass of the positive electrode material, the Zr element content is 1500 to 3000 ppm, the Sr element content is 200 to 600 ppm, and the Y element content is 5000 to 10000 ppm.

[0056] See also Figure 2 The present invention provides a method for preparing the positive electrode material described in any of the above embodiments, the preparation method comprising: mixing the first substance with the coating element source corresponding to the coating element combination respectively and performing coating sintering twice to generate a second substance coating layer on the surface of the first substance; wherein the first substance is a nickel-cobalt-manganese ternary material with a high nickel content, and the molar ratio of Ni:Co:Mn in the first substance is (70-99):(1-30):(1-30), preferably, the molar ratio of Ni:Co:Mn in the first substance is (80-99):(1-10):(1-10); the coating element source is a compound carrying the coating element, for example, one or more of oxides, hydroxides, boric acid, borates, carbonates, nitrates or sulfates carrying the coating element, and the coating element includes Co and one or more of Al, W, Ti, Ru, La, Y, Nb, Mo, B, and Ce.

[0057] In some embodiments, in the above preparation method, two sinterings can attach the coating elements of the coating element sources with different sintering temperatures to the first substance, wherein the first coating sintering causes the first element combination in the coating element combination to attach to the surface of the first substance, and the second coating sintering causes the second element combination in the coating element combination to react with the first element combination on the surface of the first substance to form the second substance coating layer. Wherein, the first element combination contains the Co element, and the first coating sintering causes the Co source to attach to the surface of the first substance at a higher sintering temperature, and then the second coating sintering causes the carrier source of the second element combination to form the second substance coating layer on the surface of the first substance together with the coating elements of the first element combination at a lower sintering temperature. Through two sinterings, the Co element and the coating elements with different sintering temperatures can be combined in the second substance attached to the surface of the first substance, thereby effectively increasing the amount of Co element coating on the surface of the first substance, while preventing Co from excessively penetrating into the crystal lattice or grain boundary of the first substance at a high sintering temperature, causing the surface of the positive electrode material to lose activity, and reducing the specific capacity and cycle performance of the positive electrode material.

[0058] Furthermore, the first element combination includes Co and one or more of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce; the second element combination includes at least two combinations of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce.

[0059] like Figure 2 As shown, the two sintering steps in the preparation method include the following steps:

[0060] S1, mixing and sintering the first substance and the element carrier composed of the first element in an oxygen atmosphere to obtain a coating sintered material;

[0061] S2. Mix and sinter the coated sintered material and the element carrier of the second element combination in an oxygen atmosphere to obtain a positive electrode material, wherein the second substance is attached to the surface of the first substance in the positive electrode material, and the second substance contains the coating elements in the first element combination and the second element combination.

[0062] In some embodiments, the first element combination includes a first cladding element and a second cladding element, and the second element group includes a second cladding element and a third cladding element. The first cladding element is Co or a combination of Co and B, the second cladding element is Al, and the third cladding element includes one or more of W, Sn, Pb, Mg, and Nb.

[0063] Step S1 specifically includes mixing the first substance with the first coating element source and the second coating element source, and sintering the mixture for the first time at a temperature of 500 to 800° C. for 18 to 26 hours in an oxygen atmosphere with an oxygen content of more than 90 wt %, to obtain a coated sintered material; preferably, the first coating element source may be nano cobalt oxide, and the second coating element source may be nano aluminum oxide;

[0064] Step S2 specifically includes continuing to mix the coated sintered material with the second coating element source and the third coating element source, and performing a second coating and sintering at a temperature of 300 to 600°C for 18 to 26 hours in an oxygen atmosphere with an oxygen content of more than 90wt% to obtain a positive electrode material; preferably, the third coating element source includes a combination of nano tungsten oxide and boric acid.

[0065] The mass ratio of the first coating element, the second coating element and the third coating element mixed in steps S1 and S2 is (0.1 to 100): (0.04 to 25): 1. Further, based on the mass of the positive electrode material, the content of the first coating element is 100 to 30000 ppm, the content of the second coating element is 200 to 5000 ppm, and the content of the third coating element is 200 to 5000 ppm.

[0066] In a preferred example, the surface Co element content of the obtained positive electrode material is 5000 to 10000ppm; the surface Al element content is 500 to 1500ppm; the surface W element content is 500 to 1000ppm; the surface B element content is 500 to 1500ppm; the coating element layer penetration depth is 260 to 610nm; the surface coated free lithium content is 1200 to 1800ppm. The positive electrode material obtained in this example is about 5% higher in mass energy density than the nickel-cobalt-manganese ternary material with a nickel-cobalt-manganese molar ratio of 8:1:1, and the Co usage is lower, with good interface stability (low Li / Ni mixed row, first coulomb efficiency>88%, 800 cycle cycle capacity retention rate>85%) and electrochemical performance (specific capacity 197-219mAh / g, 3.0-4.25V, 0.333C).

[0067] In addition, in some embodiments, the process further includes preparing a first substance before the two coating and sintering steps, and the preparing the first substance includes:

[0068] A nickel-cobalt-manganese ternary material precursor is mixed with a lithium source and a doping element source and then doped and sintered to obtain a first substance. The nickel-cobalt-manganese ternary material precursor is Ni x Co y Mn z (OH)2, 0.7≤x<1, 0≤y<0.3, 0≤z<0.3, x+y+z=1; preferably, the nickel-cobalt-manganese ternary material precursor is Ni x Co y Mn z (OH)2, 0.88≤x<1, 0 <y≤0.1,0≤z<0.1,x+y+z=1。

[0069] Wherein, the doping element source is a compound carrying a doping element, such as one or more of oxides, sulfates, oxalates, acetates, chlorides, nitrates or carbonates, and the doping element includes one or more of Zr, Mg, W, Ti, Al, Sr, Rb, Ru and Y. Preferably, the doping element source is any one or more combinations of nano-oxide species of Zr, Mg, W, Ti, Al, Sr, Rb, Ru and Y, such as a combination of zirconium oxide and aluminum oxide, a combination of strontium oxide and manganese oxide, a combination of strontium oxide and zirconium oxide, or a combination of zirconium oxide, strontium oxide and yttrium oxide, etc., which are not listed one by one here.

[0070] In some embodiments, the doping elements introduced in the preparation of the first substance include at least three, and the at least three doping elements include a first doping element, a second doping element and a third doping element, the first doping element includes any one of Zr, Ti, Nb or Mg or a combination of at least two, the second doping element includes any one of Sr, Ru or Sn or a combination of at least two, and the third doping element includes any one of Y, Ti or W or a combination of at least two.

[0071] In the above embodiment, the process of inserting doping elements into the first material includes: mixing the nickel-cobalt-manganese ternary material precursor with a lithium source, a first doping element source, a second doping element source and a third doping element source, and sintering at a temperature of 680 to 950° C. for 20 to 32 hours in an oxygen atmosphere with an oxygen content of more than 90wt%, thereby obtaining the first material. The mass ratio of the first doping element, the second doping element and the third doping element is 1: (0.02 to 2): (0.02 to 3); further, based on the mass of the positive electrode material, the content of the first doping element is 1000 to 5000ppm, the content of the second doping element is 100 to 2000ppm, and the content of the third doping element is 100 to 3000ppm.

[0072] Preferably, the first doping element source is nano zirconium oxide, the second doping element source is strontium oxide, and the third doping element source is yttrium oxide. The Zr content in the positive electrode material is 1500 to 3000 ppm, the Sr content is 200 to 600 ppm, and the Y content is 1000 to 1500 ppm.

[0073] It should be noted that in the present invention, the nickel-cobalt-manganese precursor can be prepared by conventional preparation methods in the art, such as coprecipitation method, gel method or solid phase method. As an example: first disperse the Ni source, Co source and Mn source in a solvent according to the stoichiometric ratio of n(Ni):n(Co):n(Mn)=x:y:z to obtain a mixed solution; then mix the mixed solution with a precipitant aqueous solution and a complexing agent aqueous solution to perform a coprecipitation reaction and ageing to obtain a solid-liquid mixture; filter the solid-liquid mixture to obtain a filter cake, wash the filter cake and dry it to obtain a nickel-cobalt-manganese precursor, for example [Ni x Co z Mn z ](OH)2.

[0074] The lithium source may be selected from one or more of lithium carbonate, lithium phosphate, lithium dihydrogen phosphate, lithium acetate, lithium hydroxide, lithium oxide and lithium nitrate. Further, the lithium source may be selected from one or more of lithium carbonate, lithium hydroxide and lithium nitrate. Further, the lithium source is lithium carbonate.

[0075] The present invention further provides a positive electrode plate, comprising a positive electrode current collector and a positive electrode active material layer disposed on the current collector, wherein the positive electrode active material layer comprises the positive electrode material of the present invention.

[0076] The preparation process of the positive electrode sheet is as follows: the positive electrode material, conductive agent and binder prepared above are mixed in a mass ratio of (95 to 98): (1 to 2): (1 to 2), preferably the mass ratio can be 97: 1.5: 1.5, and a solvent N-methylpyrrolidone (NMP) is added, and the mixture is stirred and mixed to obtain a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector aluminum foil, and the positive electrode sheet is prepared through drying, cold pressing, slitting and other processes. Among them, the conductive agent can be selected from at least one of Super P (carbon black), acetylene black, CNT (carbon nanotube), graphene, VGCF and other conductive materials, for example, the conductive agent is SP and CNT, and the mass ratio of SP and CNT is 1: 0.5; the binder can be selected from at least one of PVDF, PTFE and the like.

[0077] The present invention provides an electrochemical device, which includes the positive electrode material or positive electrode sheet of the present invention. The electrochemical device is, for example, a lithium-ion battery. Specifically, the lithium-ion battery includes a positive electrode sheet, a negative electrode sheet, a separator disposed between the positive electrode sheet and the negative electrode sheet, and an electrolyte.

[0078] Wherein, the positive electrode sheet is prepared by the preparation method described above in the present invention;

[0079] Preparation of negative electrode sheet: negative electrode materials such as graphite, conductive agent acetylene black, thickener CMC (sodium carboxymethyl cellulose) and binder SBR (styrene-butadiene rubber) are mixed in a mass ratio of 96.4:1:1.2:1.4, deionized water is added, and the mixture is stirred to obtain negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil, and the negative electrode sheet is prepared through drying, cold pressing, slitting and other processes;

[0080] Diaphragm: The diaphragm is made of PE or PP porous membrane, such as PP / PE / PP porous membrane, with a thickness of 9μm to 18μm, such as 9μm, 12μm, 16μm or 18μm; the air permeability is 180s / 100mL to 380s / 100mL, such as 180s / 100mL, 280s / 100mL or 380s / 100mL; the porosity is 30% to 50%, such as 30%, 40% or 50%.

[0081] Electrolyte preparation: EC (ethylene carbonate), EMC (ethyl methyl carbonate), and DMC (dimethyl carbonate) are mixed in a volume ratio of (2 to 4):(3 to 5):(2 to 4) to obtain an organic solvent. The preferred volume ratio can be 1:1:1. Then, the fully dried lithium salt LiPF6 is dissolved in the mixed organic solvent to prepare an electrolyte with a concentration of 4 - 24 wt%.

[0082] Battery assembly: The prepared positive electrode sheet, separator, and negative electrode sheet are stacked in sequence, with the separator placed between the positive and negative electrode sheets to play an insulating role. Then, it is wrapped with an aluminum-plastic film, dried, and the above-prepared electrolyte is injected. After processes such as encapsulation, standing, and formation, a soft-pack battery (i.e., a lithium-ion battery) with a capacity of 1 Ah is finally prepared.

[0083] The technical solution of the present invention will be described in detail below through several specific examples and comparative examples. Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available products or can be prepared by conventional methods in the art.

[0084] Example 1

[0085] Step 1: Mix the nickel-cobalt-manganese ternary material precursor (Ni x Co y Mn z (OH)2, 0.88 ≤ x < 1, 0 < y ≤ 0.1, 0 ≤ z < 0.1, x + y + z = 1) with a lithium source, nano-zirconia, nano-strontia, and nano-yttria, sinter at a doping sintering temperature of 735°C for 28 hours, and then crush and classify to obtain a first substance doped with Zr, Sr, and Y elements;

[0086] Step 2: Mix the first substance with nano-cobalt oxide, and perform the first coating sintering at a coating sintering temperature of 710°C for 26 hours, and then crush and classify to obtain a coated sintered material;

[0087] Step 3: Mix the coated sintered material with nano-aluminum oxide, nano-tungsten oxide, and boric acid, and perform the second coating sintering at a coating sintering temperature of 460°C for 24 hours, and then crush and classify to obtain a positive electrode material with a second substance coated on the surface;

[0088] Among them, in the positive electrode material prepared in Example 1, the content of the doped element Zr is 2479 ppm, the content of Sr is 649 ppm, and the content of Y is 1209 ppm; the content of the coated element Co on the surface of the positive electrode material is 1156 ppm, the content of Al is 1317 ppm, the content of W is 407 ppm, and the content of B is 883 ppm.

[0089] Example 2

[0090] The main difference between this embodiment and embodiment 1 is that in step 2, the mixing amount of nano cobalt oxide is adjusted so that the surface coating element Co content of the prepared positive electrode material is 5778 ppm.

[0091] Example 3

[0092] The main difference between this embodiment and embodiment 1 is that in step 2, the mixing amount of nano cobalt oxide is adjusted so that the surface coating element Co content of the prepared positive electrode material is 8613 ppm.

[0093] Example 4

[0094] The main differences between this embodiment and embodiment 1 are: in step 1, the doping and sintering are carried out at a doping and sintering temperature of 960° C. for 29 hours; in step 2, the mixing amount of nano cobalt oxide is adjusted so that the surface coating element Co content of the prepared positive electrode material is 7654 ppm.

[0095] Example 5

[0096] The main difference between this embodiment and embodiment 1 is that in step 1, only nano zirconium oxide is mixed into the nickel-cobalt-manganese ternary material precursor for doping and sintering, and the amount of nano zirconium oxide used is adjusted so that the content of doped element Zr in the prepared positive electrode material is 1227 ppm.

[0097] Example 6

[0098] The main difference between this embodiment and embodiment 1 is that in step 1, only nano tungsten oxide is mixed into the nickel-cobalt-manganese ternary material precursor for doping and sintering, and the amount of nano tungsten oxide used is adjusted so that the content of doping element W in the prepared positive electrode material is 1436 ppm.

[0099] Example 7

[0100] The main difference between this embodiment and embodiment 1 is that in step 1, nano zirconium oxide and nano yttrium oxide are mixed into the nickel-cobalt-manganese ternary material precursor for doping and sintering, and the usage of nano zirconium oxide and nano yttrium oxide is adjusted so that the content of doped elements Zr in the prepared positive electrode material is 1167ppm and the content of Y is 542ppm.

[0101] Example 8

[0102] The main difference between this embodiment and embodiment 1 is that in step 1, the nickel-cobalt-manganese ternary material precursor is mixed with nano-zirconium oxide, nano-aluminum oxide and nano-tungsten oxide, sintered at a doping sintering temperature of 960°C for 29 hours, and the usage of nano-zirconium oxide, nano-aluminum oxide and nano-tungsten oxide is adjusted so that the content of doped elements Zr in the prepared positive electrode material is 1098ppm, the content of Al is 413ppm, and the content of W is 1326ppm.

[0103] Example 9

[0104] The main difference between this embodiment and embodiment 1 is that in step 2, the mixing amount of nano cobalt oxide is adjusted so that the surface coating element Co content of the prepared positive electrode material is 8105ppm, Al content is 1307ppm, W content is 421ppm, and B content is 917ppm.

[0105] Example 10

[0106] The main difference between this embodiment and embodiment 9 is that: in step 2, the first coating and sintering is carried out at a coating and sintering temperature of 760°C for 26 hours; so that the surface coating element Co content of the prepared positive electrode material is 7439ppm, Al content is 1238ppm, W content is 406ppm, and B content is 787ppm.

[0107] Comparative Example 1

[0108] The main difference between this embodiment and embodiment 1 is that in step 2, the mixing amount of nano cobalt oxide is adjusted so that the surface coating element Co content of the prepared positive electrode material is 7513 ppm.

[0109] Comparative Example 2

[0110] The main difference between this embodiment and embodiment 1 is that in step 2, the first coating sintering is performed without mixing nano cobalt oxide.

[0111] Comparative Example 3

[0112] The main difference between this embodiment and embodiment 1 is that in step 1, nano zirconium oxide and nano alumina are mixed into the nickel-cobalt-manganese ternary material precursor for doping and sintering, and the usage of nano zirconium oxide and nano alumina is adjusted so that the content of doped element Zr in the prepared positive electrode material is 1024ppm and the content of Al is 465ppm.

[0113] Comparative Example 4

[0114] The main difference between this embodiment and embodiment 1 is that in step 1, doping sintering is performed without mixing any doping elements.

[0115] Comparative Example 5

[0116] The main difference between this embodiment and embodiment 1 is that the first coating sintering of step 2 is not performed on the first material.

[0117] The positive electrode materials prepared in Examples 1 to 10 and Comparative Examples 1 to 5 were assembled into soft-pack batteries according to the assembly method of the present invention for battery performance testing. The test was conducted using a battery performance testing system of Shenghong Electric Co., Ltd. (equipment model: BTS05 / 10C8D-HP). The battery performance test included a battery gram capacity test and a cycle capacity retention test.

[0118] Gram capacity test method: At 25°C, charge and discharge for one week at 0.063A / g. The charge and discharge capacity obtained is divided by the amount of positive electrode used, which is the first charge / discharge gram capacity. The first discharge capacity divided by the first charge capacity is the first coulomb efficiency.

[0119] Cycle capacity retention test method: Cycle at 25°C with a charge and discharge rate of 0.19A / g (calculated based on the mass of the positive electrode material). After 800 cycles, the discharge capacity of the battery at this time is divided by the discharge capacity of the first cycle, which is the 800-cycle cycle capacity retention rate of the battery.

[0120] The content of each element in the positive electrode materials prepared in Examples 1 to 10 and Comparative Examples 1 to 5, the penetration depth of the coating elements, and the content of free lithium elements coated on the surface were tested.

[0121] The content of each element in the positive electrode material is tested by the inductively coupled plasma (ICP) method: ICP, the high-frequency energy provided by the radio frequency generator is added to the inductive coupling coil, and the plasma torch is placed in the center of the coil, so that a high-frequency electromagnetic field is generated in the torch, and the micro-spark is used to ignite the argon gas entering the torch, which generates electrons and ions and conducts electricity. The conductive gas is affected by the high-frequency electromagnetic field to form an eddy current area concentric with the coupling coil. The high heat generated by the strong current forms a torch-shaped and self-sustaining plasma. Due to the skin effect of the high-frequency current and the effect of the inner tube carrier gas, the plasma has a ring structure. The sample that forms the plasma is brought into the atomization system by the carrier gas (usually argon) for atomization, and then enters the axial channel of the plasma in the form of aerosol. It is fully evaporated, atomized, ionized and excited in the high temperature and inert atmosphere, and emits the characteristic spectrum of the elements contained. The presence or absence of characteristic spectral lines can be used to identify whether a sample contains a certain element (qualitative analysis); the content of the corresponding element in the sample can be determined based on the intensity of the characteristic spectral lines (quantitative analysis). For specific ICP tests, please refer to conventional test methods in the field.

[0122] Element penetration depth test method: The powder particles are cut using a focused ion beam method, and then the distribution depth of the coated elements is tested using a time-of-flight secondary ion mass spectrometer (TOF-SIMS).

[0123] Method for calculating the surface free lithium coating amount: Place 1g powder in deionized water and stir with a glass rod for 5 minutes. After standing for 4 hours, take the supernatant and use a potentiometric titrator to test the content of LiOH and Li2CO3. The amount of lithium element in it is the surface coated free lithium content.

[0124] Gram capacity test method: At 25°C, charge and discharge for one week at 0.063A / g. The charge and discharge capacity obtained is divided by the amount of positive electrode used, which is the first charge / discharge gram capacity. The first discharge capacity divided by the first charge capacity is the first coulomb efficiency.

[0125] Cycle capacity retention test method: Cycle at 25°C with a charge and discharge rate of 0.19A / g (calculated based on the mass of the positive electrode material). After 800 cycles, the discharge capacity of the battery at this time is divided by the discharge capacity of the first cycle, which is the 800-cycle cycle capacity retention rate of the battery.

[0126] The test results of Examples 1 to 10 and Comparative Examples 1 to 5 are shown in Table 1, Table 2 and Table 3.

[0127] Table 1: Electrochemical performance of positive electrode materials prepared in Examples 1 to 4 and Comparative Examples 1 to 2 at different Co coating amounts

[0128]

[0129] Table 2: Electrochemical performance of positive electrode materials prepared in Examples 5 to 8 and Comparative Examples 3 to 4 under different doping elements

[0130]

[0131]

[0132] Table 3: Electrochemical performance of positive electrode materials prepared in Examples 9 to 10 and Comparative Examples 1 and 5 under different doping elements

[0133]

[0134] The test results of Examples 1 to 4 and Comparative Examples 1 to 2 show that the amount of Co coating on the surface of the positive electrode material directly affects the kinetic performance of the material. If the amount of Co coating on the surface is too low, the kinetics are poor, the material DCR is high, and the surface stability is poor, resulting in poor cycle performance and low rate performance; if the amount of Co coating on the surface is too high, the lattice is severely mixed, the distortion is large, and the cost is increased.

[0135] The test results of Examples 5 to 8 and Comparative Examples 3 to 4 show that during the preparation of positive electrode materials, an appropriate amount of precursor element doping can make the doping elements evenly distributed in the lattice compared to dry doping, and the doping elements form a "pinning" effect on the lattice, greatly improving the lattice strength; but excessive element doping will increase the lattice distortion and increase the element mixing, resulting in reduced capacity and deterioration of long-term performance.

[0136] The test results of Examples 9 to 10 and Comparative Examples 1 and 5 show that by coating the second material coating layer on the surface of the positive electrode material through two coating sinterings, the Co element can be combined with the coating elements of different sintering temperatures on the surface of the positive electrode material, which can effectively increase the coating amount of the Co element on the surface of the first material, greatly improve the long-term performance of the positive electrode material, and use a lower sintering temperature during the second coating sintering to avoid excessive penetration of Co into the lattice or grain boundary of the first material at a high sintering temperature, thereby improving the stability of the interface of the positive electrode material and ensuring the specific capacity and cycle performance of the positive electrode material. In summary, the positive electrode material and preparation method thereof provided by the present invention first use doping sintering to place at least one doping element of Zr, Mg, W, Ti, Al, Sr, Rb, Ru, and Y into the nickel-cobalt-manganese ternary material to enhance the crystallinity and lattice strength of the material, thereby providing a basis for coating the positive electrode material with a higher coating amount of Co element under the premise of stabilizing the structure; and then successively through two coating sinterings, Co and at least one coating element of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce are combined on the surface of the positive electrode material to form a second material coating layer, thereby forming a coating layer with a high Co coating amount on the surface of the nickel-cobalt-manganese ternary material with a lower Co element usage, so that the prepared positive electrode material takes into account both structural stability and electrochemical performance, and has high specific capacity, high energy density and good cycle performance.

[0137] The positive electrode material and preparation method thereof, the positive electrode plate and the electrochemical device of the present invention are sintered twice to make the Co element cooperate with other elements on the surface of the nickel-cobalt-manganese ternary material to form a second material coating layer with smaller particles, so as to reduce the use of the Co element in the high-nickel ternary material while repairing the surface defects of the material, improve the material interface stability while taking into account high energy density and good electrochemical performance, so as to obtain a positive electrode material with high specific capacity, good cycle performance and excellent thermal stability. The charge and discharge voltage of the positive electrode material reaches 4.25V, and the compaction density can reach 3.55mg / cm 3 ; The specific capacity can reach 210-222mAh / g (3.0-4.25V, 0.333C), which is an excellent raw material for producing high-end power batteries. Therefore, the present invention effectively overcomes some practical problems in the prior art and has high utilization value and use significance.

[0138] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A positive electrode material, characterized in that: include: The first substance includes a nickel-cobalt-manganese ternary material, wherein the nickel-cobalt-manganese ternary material is LiNi x Co y Mn z O2, where 0.7≤x<1, 0≤y<0.3, z=1-xy; The second substance has a particle size smaller than that of the first substance, the second substance is attached to the surface of the first substance, the second substance comprises a coating element combination, the coating element combination comprises at least two coating elements, and the coating element combination comprises at least Co element.

2. The positive electrode material according to claim 1, characterized in that: The chemical formula of the positive electrode material is Li 1+a [Ni x Co y Mn z M 1-x-y-z O 2-b A b , 0.7 ≤ x < 1, 0 ≤ y < 0.3, 0 ≤ z < 0.3, -0.2 < a < 0.2, 0 ≤ b < 0.1, wherein the M element includes one or more of Sr, Y, Al, Ti, Mg, Sr, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Ni, Co, Mn, and Zr, and the A element includes one or more of F, N, Cl, S, and P.

3. The positive electrode material according to claim 1, characterized in that: The chemical formula of the second substance is LiN x Co y O 2-b A b , 0.7≤x<1, 0≤y<0.3, 0≤b<0.1; wherein the N element includes the coating element, the coating element contained in the N element includes one or more of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce, and the A element includes one or more of F, N, Cl, S and P.

4. The positive electrode material according to claim 3, characterized in that: In addition to the coating element, the N element also includes one or more of Mg, Sr, V, Se, Rh, Pd, Sb, Te, Ca, Zn, Ni, Mn and Zr.

5. The positive electrode material according to claim 3, characterized in that: The coating element combination in the second substance is attached to the first substance through two sinterings; the first element combination in the coating element combination is attached to the first substance through the first sintering, and the second element combination in the coating element combination is attached to the first substance through the second sintering, and the first element combination includes Co element.

6. The positive electrode material according to claim 5, characterized in that: The first element combination includes Co and one or more of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce; the second element combination includes a combination of at least two of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce.

7. The positive electrode material according to claim 3, characterized in that: The second substance includes a first coating element, a second coating element and a third coating element, the first coating element is Co or a combination of Co and B, the second coating element is Al, and the third coating element includes one or more of W, Sn, Pb, Mg and Nb.

8. The positive electrode material according to claim 7, characterized in that: The content of the first coating element in the positive electrode material is 100 to 30000 ppm, the content of the second coating element in the positive electrode material is 200 to 5000 ppm, and the content of the third coating element in the positive electrode material is 200 to 5000 ppm.

9. The positive electrode material according to claim 1, characterized in that: The Co element in the second substance is at least partially located inside the first substance.

10. The positive electrode material according to claim 9, characterized in that: The penetration depth of the coating element of the second substance in the first substance is 260 to 650 nm.

11. The positive electrode material according to claim 1, characterized in that: The content of Co element in the positive electrode material is 5000 to 15000 ppm.

12. The positive electrode material according to claim 1, characterized in that: The nickel-cobalt-manganese ternary material is doped with doping elements, and the doping elements include one or more of Zr, Mg, W, Ti, Al, Sr, Rb, Ru and Y.

13. The positive electrode material according to claim 12, characterized in that: The doping element is embedded in the single crystal lattice of the nickel-cobalt-manganese ternary material.

14. The positive electrode material according to claim 12, characterized in that: The doping elements include a first doping element, a second doping element and a third doping element; the first doping element includes one or more of Zr, Ti, Nb and Mg, the second doping element includes one or more of Sr, Ru and Sn, and the third doping element includes one or more of Y, Ti and W.

15. The positive electrode material according to claim 14, characterized in that: The content of the first doping element in the positive electrode material is 1000 to 5000 ppm, the content of the second doping element in the positive electrode material is 100 to 2000 ppm, and the content of the third doping element in the positive electrode material is 100 to 3000 ppm.

16. A method for preparing the positive electrode material according to any one of claims 1 to 15, characterized in that: include: The first substance is mixed with the coating element source corresponding to the coating element combination and coated and sintered twice to form a second substance coating layer on the surface of the first substance; the first substance is a nickel-cobalt-manganese ternary material, and the nickel-cobalt-manganese ternary material is LiNi x Co y Mn z O2, where 0.7≤x<1, 0≤y<0.3, z=1-xy; Wherein, the coating element combination includes at least two coating elements, the coating element source is a compound loaded with coating elements, and the coating element includes Co.

17. The method for preparing the positive electrode material according to claim 16, characterized in that: Before the two coating sintering, the first substance is also prepared, and the preparation of the first substance includes: mixing the nickel-cobalt-manganese ternary material precursor with the lithium source and the doping element source and then performing doping sintering to obtain the first substance, wherein the nickel-cobalt-manganese ternary material precursor is LiNi x Co y Mn z (OH)2, wherein 0.7≤x<1, 0≤y<0.3, x+y+z=1; the doping elements include one or more of Zr, Mg, W, Ti, Al, Sr, Rb, Ru and Y.

18. The method for preparing the positive electrode material according to claim 16, characterized in that: The coating elements also include one or more of Al, W, Ti, Ru, La, Y, Nb, Mo, B, and Ce.

19. The method for preparing the positive electrode material according to claim 18, characterized in that: The first coating sintering causes the first element combination of the coating element combination to adhere to the surface of the first material, and the second coating sintering causes the second element combination of the coating element combination to react with the first element combination on the surface of the first material to generate the second material coating layer, and the first element combination includes Co.

20. The method for preparing the positive electrode material according to claim 19, characterized in that: The sintering temperature of the second coating sintering is lower than the sintering temperature of the first coating sintering. The first coating sintering temperature is 500-800°C, the first coating sintering cycle is 18-26h, the second coating sintering temperature is 300-600°C, and the second coating sintering cycle is 18-26h.

21. The method for preparing the positive electrode material according to claim 19, characterized in that: The first element combination includes Co and one or more of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce; the second element combination includes at least two combinations of Al, W, Ti, Ru, La, Y, Nb, Mo, B and Ce.

22. A positive electrode plate, characterized in that: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer, and the positive electrode active material layer comprises the positive electrode material according to any one of claims 1 to 15 or the positive electrode material prepared by the preparation method according to any one of claims 16 to 21.

23. An electrochemical device, characterized in that: It comprises a negative electrode plate, a separator, an electrolyte and the positive electrode plate as claimed in claim 22.

Citation Information

Cited By

  • Polycrystalline ultrahigh-nickel ternary positive electrode material and preparation method and application thereof

    CN119092694A

  • Cathode material with coating layer, preparation method of cathode material and lithium ion battery

    CN119890275A

  • Cobalt-aluminum-titanium co-coated positive electrode material as well as preparation method and application thereof

    CN119890277A

  • Ultrahigh-nickel ternary positive electrode material as well as preparation method and application thereof

    CN120581567A

  • Ternary positive electrode material with coating layer, preparation method of ternary positive electrode material, positive electrode and battery

    CN121149213A