Cerium oxide doped carbon carrier platinum-carbon catalyst, preparation method thereof and application of cerium oxide doped carbon carrier platinum-carbon catalyst in hydrogen fuel cell
By using cerium oxide doped carbon carrier platinum carbon catalyst in hydrogen fuel cells, the problems of carbon carrier electrochemical corrosion and insufficient interaction force of platinum nanoparticles are solved, the stability and activity of the catalyst are significantly improved, and the electrochemical activity is prolonged. The service life of the area enhances the catalytic performance of the oxygen reduction reaction.
Patent Information
- Application Number
- CN202410999044.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In traditional hydrogen fuel cells, electrochemical corrosion of carbon carriers and insufficient interaction between platinum nanoparticles lead to catalyst deactivation and affect stack performance.
Using cerium oxide doped carbon carrier platinum carbon catalyst, through the combination of CeO2 doped carbon aerogel and platinum nanoparticles, a highly active oxygen reduction catalytic center is formed to enhance the stability and activity of the catalyst, using technologies such as microwave heating and ultrasonic dispersion. Improve catalyst performance.
It significantly improves the durability and electrochemical activity of the catalyst, extends the service life of the electrochemically active area, enhances the catalytic performance of the oxygen reduction reaction, and reduces the aggregation and loss of the metal catalyst.
Smart Images

Figure CN118738425A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of new energy battery materials, and specifically relates to a cerium oxide-doped carbon-supported platinum-carbon catalyst, a preparation method thereof, and an application thereof in a hydrogen fuel cell. Background Art
[0002] In recent years, the massive consumption of traditional energy has led to an increasingly severe energy crisis, and the resulting environmental pollution problems have also followed one after another. People are in urgent need of a new type of clean energy to replace traditional energy. As we all know, hydrogen is a clean energy with many advantages, such as high calorific value, pollution-free products and abundant reserves. Hydrogen fuel cells are a power generation device that can directly convert the chemical energy of hydrogen into electrical energy. Its large-scale commercial use can alleviate the environmental pollution problems caused by the use of traditional energy and realize the vision of clean energy transformation in the future.
[0003] The catalyst layer in a hydrogen fuel cell is the place where hydrogen and oxygen undergo electrochemical reactions to generate current, and is the core of a hydrogen fuel cell. At present, the most commonly used cathode and anode catalysts in hydrogen fuel cells are Pt / C catalysts, but the harsh working environment of hydrogen fuel cells can easily lead to catalyst degradation and loss of activity. Among the many factors that lead to catalyst electrocatalytic deactivation, the surface structure and composition of the carbon carrier are one of the most important influencing factors. Commercial carbon black has been widely used as a carrier material for Pt / C catalysts due to its low cost, high availability and high mesoporous distribution. However, this carbon material is prone to electrochemical corrosion at defects and edges, and its weak interaction with platinum nanoparticles can cause the migration and aggregation of platinum during the catalytic process. All of the above will lead to catalyst deactivation, thereby affecting the comprehensive performance of the membrane electrode and the final stack product.
[0004] The patent with the publication number CN 103831103 A published on June 4, 2014 discloses a graphene aerogel catalyst and a preparation method thereof. The catalyst uses graphene aerogel as a carrier, binary Pt-CeO2 as an active component, a platinum loading of 10-30wt%, and a molar ratio of Pt to CeO2 of 2:1. The preparation method is as follows: uniformly dispersing graphene aerogel and CeO2 in a mixed solution of ethylene glycol and isopropanol; adding chloroplatinic acid solution to the mixed solution to adjust the pH value of the solution to 10-12; then microwave heating, filtering, washing, and drying to obtain a Pt-CeO2 / graphene aerogel catalyst. The disclosed product has good electrocatalytic activity for methanol and CO poisoning resistance. However, it does not disclose how to solve the problem that carbon materials are prone to electrochemical corrosion at defects and edges and improve durability. Summary of the invention
[0005] The purpose of the present invention is to provide a cerium oxide-doped carbon carrier platinum-carbon catalyst and a preparation method thereof. In view of the problem that carbon materials are prone to electrochemical corrosion at defects and edges, and the weak interaction between them and platinum nanoparticles will cause the migration and aggregation of platinum during the catalytic process, resulting in catalyst deactivation, the present invention provides CeO2-doped carbon aerogel / carbon carrier, and utilizes a carbon aerogel material with good electrochemical stability as a catalyst carrier; and CeO2 is doped to further improve the catalytic activity and stability of the Pt / C catalyst ORR.
[0006] The present invention also provides an application of a cerium oxide-doped carbon-supported platinum-carbon catalyst in a hydrogen fuel cell, which is used to prepare a hydrogen fuel cell catalyst, and improves the problem of partial dissolution and oxidation aggregation of platinum-based catalysts as the oxygen reduction reaction proceeds under the actual operating environment of the fuel cell. The catalyst of the present invention is used in a hydrogen fuel cell, and the doping can form a highly active oxygen reduction catalytic active center with the coordinated carbon, and can form an "anchoring effect" to enhance the catalytic performance of the Pt alloy. The introduction of Ce atoms can embed or anchor Pt on the surface of the carrier C, thereby controlling the aggregation of the metal catalyst and reducing its loss. After 15,000 durability cycles, the electrochemical active area loss of Ce-CA-Pt is negligible.
[0007] The specific technical solutions of the present invention are as follows:
[0008] A method for preparing a cerium oxide-doped carbon-supported platinum-carbon catalyst comprises the following steps:
[0009] 1) dissolving resorcinol in a mixed solution of anhydrous ethanol and ultrapure water, adding concentrated hydrochloric acid and a cerium source, stirring under a closed condition at room temperature, and then adding formaldehyde solution dropwise, stirring to obtain a mixed solution;
[0010] 2) heating the mixed solution to react and obtain an organic wet gel;
[0011] 3) Carbonizing the organic wet gel to obtain CeO2-doped carbon aerogel / carbon carrier material;
[0012] 4) CeO2-doped carbon aerogel / carbon carrier material is dispersed in ethylene glycol, and H2PtCl6 solution is added dropwise to the obtained mixed solution under stirring. After adjusting the pH value to 12, microwave heating is performed for reaction, and after freeze-drying, a cerium oxide-doped carbon carrier platinum-carbon catalyst is obtained.
[0013] In step 1), the amount ratio of resorcinol to the mixed solution of anhydrous ethanol and ultrapure water is 0.10-0.12 g / mL;
[0014] In step 1), the volume ratio of anhydrous ethanol to ultrapure water is 1:1;
[0015] In step 1), the mass fraction of the concentrated hydrochloric acid is 37%;
[0016] In step 1), the cerium source is selected from Ce(NO3)3·6H2O;
[0017] In step 1), the volume ratio of the concentrated hydrochloric acid to the mixed solution of anhydrous ethanol and ultrapure water is 1:20;
[0018] In step 1), the mass of the cerium source added is 10% to 20% of the mass of resorcinol;
[0019] In step 1), the stirring is carried out under sealed conditions at room temperature for 1 hour;
[0020] In step 1), the mass fraction of the formaldehyde solution is 37%;
[0021] In step 1), the molar ratio of resorcinol to formaldehyde in the formaldehyde solution is n R :n F =1 / 2~1 / 3:1;
[0022] In step 1), the formaldehyde solution is added dropwise and stirred for 1 hour at room temperature;
[0023] In step 2), the heating reaction is oil bath heating, the reaction temperature is 55-80°C, and the reaction time is 6-12h;
[0024] In step 2), the prepared organic wet gel is first cooled to room temperature, washed with water by centrifugation for 3-5 times, dried in a vacuum drying oven at 80° C. for 12 h, and then carbonized;
[0025] In step 3), the carbonization treatment conditions are: carried out in a tube furnace in an argon atmosphere at 5°C min -1 The heating rate is from 650 to 850°C to the carbonization temperature, and the treatment time is from 3 to 5 hours.
[0026] The CeO2-doped carbon aerogel / carbon carrier material prepared in step 3) is a mesoporous material, labeled as Ce-CA, with a pore size of 3-4 nm, and the pore size is small and uniform.
[0027] In step 4), the CeO2-doped carbon aerogel / carbon carrier material and ethylene glycol are used in an amount ratio of 0.7-0.8 mg / mL, and ultrasonic dispersion is used to disperse them uniformly;
[0028] In step 4), the volume ratio of H2PtCl6 solution to ethylene glycol is 1:20, and the concentration of the H2PtCl6 solution is a Pt content of 10 mg / mL;
[0029] In step 4), the pH value of the mixed system is adjusted to 12 with a 1.0 M sodium hydroxide aqueous solution.
[0030] In step 4), microwave heating reaction, the microwave heating temperature is 170° C., and the reaction time is 5 min;
[0031] In step 4), after the reaction is completed, the final product is collected by centrifugation, washed with deionized water for 3-5 times, and dried in a freeze dryer to obtain a cerium oxide-doped carbon-supported platinum-carbon catalyst, which is marked as Ce-CA-Pt catalyst material.
[0032] The stirring rate of the present invention is 300-500 r / min;
[0033] The present invention provides a cerium oxide-doped carbon-supported platinum-carbon catalyst, which is prepared by the above method.
[0034] The present invention provides an application of a cerium oxide-doped carbon-supported platinum-carbon catalyst in a hydrogen fuel cell, and the specific application method is as follows:
[0035] S1. preparing a cerium oxide-doped carbon-supported platinum-carbon catalyst into a catalyst slurry;
[0036] S2, spraying the catalyst slurry onto both sides of the proton exchange membrane by ultrasonic spraying;
[0037] S3. The proton exchange membrane prepared in step S2 is used in a hydrogen fuel cell.
[0038] Compared with the prior art, the present invention uses a carbon aerogel material with good electrochemical stability prepared by high-temperature carbonization as a catalyst carrier, specifically, a sol-gel method is used to prepare carbon aerogel (CA). CA has a higher degree of graphitization than commercial carbon black, so under extremely high potential conditions, CA has better electrochemical corrosion resistance. Platinum nanoparticles are loaded on CA, and the prepared Ce-CA-Pt has high catalytic activity and better ORR long-term cycle stability. After 15,000 durability cycles, the loss of electrochemical active area of Ce-CA-Pt is negligible. The results show that the carbon aerogel (CA) prepared by the sol-gel method is an excellent Pt-based catalyst carrier. The carbon material synthesized by the method of the present invention has a higher specific surface area and a better pore size, which provides a better environment for metal element doping and Pt particle attachment, mainly due to the introduction of doping substances and the control of preparation conditions during the preparation of organic wet gel. In addition, metal atom Ce doping can further improve the catalytic activity and stability of Pt / C catalyst ORR. Doping can form a highly active oxygen reduction catalytic active center together with the coordinated carbon, and can form an "anchoring effect" to enhance the catalytic performance of Pt alloy. The introduction of Ce atoms can make Pt embedded or anchored on the surface of the carrier C, thereby controlling the aggregation of metal catalysts and reducing their loss. Cerium (Ce) can lose one 5d electron and two 6s electrons to form Ce3+ , and can also lose an electron in the 4f orbital at the same time, forming a very stable 4f orbital to obtain Ce 4+ This This makes Ce have excellent redox properties. At the same time, as the oxidation state of cerium changes, cerium oxide forms oxygen vacancies or defects by losing oxygen or electrons, and the valence state and defect structure of cerium oxide are dynamic, which can easily form active sites that are beneficial to catalysis, thereby improving and regulating the physical parameters and performance of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is the scanning electron microscope image of Ce-CA2;
[0040] Figure 2 This is a transmission electron microscope scan of Ce-CA2;
[0041] Figure 3 Ce-CA2 element mapping diagram (C);
[0042] Figure 4 is the Ce-CA2 element mapping diagram (Ce);
[0043] Figure 5 is the Ce-CA2 element mapping diagram (O);
[0044] Figure 6 Polarization curves of CA-Pt and Ce-CA2-Pt. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0046] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0047] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0048] The present invention provides a method for preparing a cerium oxide-doped carbon-supported platinum-carbon catalyst, comprising the following steps:
[0049] 1) Dissolve resorcinol in a mixed solution of anhydrous ethanol and ultrapure water (the volume ratio of anhydrous ethanol to ultrapure water is 1:1), then add 37% by mass concentrated hydrochloric acid and Ce(NO3)3·6H2O, stir for 1 hour at room temperature under a closed condition, then add 37% by mass formaldehyde solution dropwise, stir for 1 hour at room temperature to obtain a mixed solution;
[0050] The dosage ratio of resorcinol to the mixed solution of anhydrous ethanol and ultrapure water is 0.10-0.12 g / mL; the volume ratio of the concentrated hydrochloric acid to the mixed solution of anhydrous ethanol and ultrapure water is 1:20; the mass of the cerium source added is 10% to 20% of the mass of resorcinol; the molar ratio of the resorcinol to the formaldehyde in the formaldehyde solution is n R :n F =1 / 2~1 / 3:1;
[0051] 2) heating the mixed solution in an oil bath at 55-80°C for 6-12 hours, first cooling to room temperature, centrifuging and washing with water for 3-5 times, and drying in a vacuum drying oven at 80°C for 12 hours to obtain an organic wet gel;
[0052] 3) Carbonization of organic wet gel was carried out in a tube furnace in an argon atmosphere at 5 °C min -1 The heating rate is increased to a carbonization temperature of 650-850°C and the processing time is 3-5h to obtain CeO2-doped carbon aerogel / carbon carrier material; marked as Ce-CA, with a pore size of 3-4nm, small and uniform pore size.
[0053] 4) CeO2-doped carbon aerogel / carbon carrier material is ultrasonically dispersed in ethylene glycol, and an H2PtCl6 solution with a Pt content of 10 mg / mL is added dropwise to the obtained mixed solution under stirring, and the pH value of the mixed system is adjusted to 12 with a 1.0 M sodium hydroxide aqueous solution, and then subjected to microwave heating reaction at a temperature of 170°C and a reaction time of 5 min; after the reaction, the final product is collected by centrifugation, washed with deionized water 3-5 times, and dried in a freeze dryer to obtain a cerium oxide-doped carbon carrier platinum-carbon catalyst, marked as a Ce-CA-Pt catalyst material, to obtain a cerium oxide-doped carbon carrier platinum-carbon catalyst; wherein the amount ratio of CeO2-doped carbon aerogel / carbon carrier material to ethylene glycol is 0.7-0.8 mg / mL, and the volume ratio of H2PtCl6 solution to ethylene glycol is 1:20.
[0054] The application of the cerium oxide-doped carbon-supported platinum-carbon catalyst prepared by the present invention in a hydrogen fuel cell is specifically described as follows:
[0055] S1. Disperse the Ce-CA-Pt catalyst material in deionized water for full wetting, then add an alcohol system solvent and Naf ion solution, and obtain a catalyst slurry by shearing;
[0056] The mass ratio of Ce-CA-Pt catalyst material, deionized water, alcohol system solvent and Naf ion solution is 0.1:15:20:0.6; the alcohol system solvent used is anhydrous ethanol, isopropanol or isobutanol;
[0057] S2. Add the prepared catalyst slurry into the injection tube of ultrasonic spraying, and use ultrasonic spraying to spray the catalyst slurry onto both sides of the proton exchange membrane. The process parameters of ultrasonic spraying are set as follows: vacuum chuck temperature 105℃, nozzle pressure 110kPa, slurry flow 5mL / min, step width 8mm, nozzle height 30mm, nozzle travel speed 150mm / min. The effective working area of the obtained CCM is 5cm×5cm, and the amount of platinum used for the cathode and anode is 0.3 and 0.05mg / cm respectively. 2 .
[0058] S3. Before assembling a single cell, prepare the end plate, insulating plate, current collector, carbon plate (single serpentine flow channel), CCM, carbon paper, gasket, bolts, torque wrench and other parts and installation tools. The torque used when assembling a single cell is 4N·m. Before testing a single cell, check the air tightness of the battery to ensure that there is no gas leakage.
[0059] S4, fuel cell test system is Ningbo Beit single cell test bench, using 25cm 2 The membrane electrode test was carried out using a standard single cell fixture. During the test, the temperature of the humidification tank and the single cell fixture was controlled by electric heating to adjust the humidity of the positive and negative electrodes of the membrane electrode. The membrane electrode test conditions were as follows: the stoichiometric ratio of H2 / Ai r was 1.5 / 2.0, and the back pressure was 1 bar. The constant pressure activation was 30 minutes before the polarization curve test, and the cumulative activation was 120 minutes.
[0060] Several preferred embodiments of the present invention are as follows:
[0061] Example 1 (for comparison)
[0062] The preparation method of carbon aerogel / carbon carrier platinum-carbon catalyst (CA-Pt) comprises the following steps:
[0063] 1) Dissolve 11g of resorcinol in 100mL of anhydrous ethanol and ultrapure water (V (超纯水) :V (无水乙醇)=1:1), add 5 mL of concentrated hydrochloric acid (wt, 37%), stir for 1 h at 25 ° C under closed conditions until the reactants are completely dissolved, then add 15 mL of formaldehyde solution (wt, 37%) to the solution, stir for 1 h under the same conditions; then put in an oil bath at 75 ° C, stir with a stirrer at 300 r / min, react for 6 h to obtain an organic wet gel, cool to room temperature after drying, centrifuge and wash with water 3 times, dry in a vacuum drying oven at 80 ° C for 12 h, then put the obtained material into a tube furnace, in an argon atmosphere, at 5 ° C min -1 The carbon aerogel / carbon carrier (CA) material can be obtained by heating the material at a carbonization temperature of 750 °C and a carbonization time of 5 h.
[0064] 2) Disperse 150 mg of the CA material obtained in step 1) in 200 mL of ethylene glycol by ultrasonic treatment to obtain a mixture; add 10 mL of H2PtCl6 solution (10 mgPt mL -1 ) was added dropwise to the mixture under vigorous stirring, and the pH value of the resulting mixed system was adjusted to 12 with an aqueous sodium hydroxide solution (1.0 M). The reaction solution was then heated to 170° C. by microwave and heated at this temperature for 5 min. The final product was collected by centrifugation, washed 3 times with deionized water, and dried in a freeze dryer to obtain a CA-Pt catalyst material.
[0065] The application of carbon aerogel / carbon-supported platinum-carbon catalyst (CA-Pt) in hydrogen fuel cells is as follows:
[0066] Take 100 mg of the catalyst prepared in step 2), add 15 g of deionized water and 20 g of isopropanol successively, add 0.6 g of Nafi on solution (5 wt%) after ultrasonic dispersion for 30 min, and then high-speed shear dispersion for 50 min to obtain the final slurry. When preparing the catalyst slurry, keep the water in the ultrasonic cleaning machine in an ice-water bath state at 15°C. Add the prepared catalyst slurry into the injection tube of ultrasonic spraying, and use ultrasonic spraying to spray the catalyst slurry to both sides of the proton exchange membrane respectively. The process parameters of ultrasonic spraying are set as follows: vacuum chuck temperature 105°C, nozzle air pressure 110 kPa, slurry flow rate 5 mL / min, step width 8 mm, nozzle height 30 mm, nozzle travel speed 150 mm / min. The effective working area of the obtained CCM is 5 cm×5 cm, and the amount of platinum used for the cathode and anode is 0.3 and 0.05 mg / cm respectively. 2 .
[0067] Use 25cm 2The membrane electrode test was carried out using a standard single cell fixture. During the test, the temperature of the humidification tank and the single cell fixture was controlled by electric heating to adjust the humidity of the positive and negative electrodes of the membrane electrode. The membrane electrode test conditions were as follows: the stoichiometric ratio of H2 / Ai r was 1.5 / 2.0, and the back pressure was 1 bar. The constant pressure activation was 30 minutes before the polarization curve test, and the cumulative activation was 120 minutes.
[0068] Example 2
[0069] A method for preparing a cerium oxide-doped carbon-supported platinum-carbon catalyst (Ce-CA1-Pt), comprising the following steps:
[0070] 1) Dissolve 11g of resorcinol in 100mL of anhydrous ethanol and ultrapure water (V (超纯水) :V (无水乙醇) =1:1), then add concentrated hydrochloric acid (wt, 37%) 5mL and Ce(NO3)3·6H2O, 1.1g, stir at 25℃, closed conditions for 1h until the reactants are completely dissolved, then add formaldehyde solution (wt, 37%) 15mL to the solution, stir vigorously for 1h under the same conditions; then oil bath, 75℃, stir with a stirrer at 300r / min, react for 6h to obtain an organic wet gel, cool to room temperature after drying, centrifuge and wash with water 3 times, dry in a vacuum drying oven at 80℃ for 12h, then put the obtained material into a tube furnace, in an argon atmosphere, at 5℃min -1 The heating rate is 0.0447 W, the carbonization temperature is 750 °C, and the carbonization time is 5 h, then the CeO2-doped carbon aerogel / carbon carrier (Ce-CA1) material can be obtained.
[0071] 2) Disperse 150 mg of Ce-CA1 material obtained in step 1) in 200 mL of ethylene glycol by ultrasonic treatment to obtain a mixture. -1 ) was added dropwise to the mixture under vigorous stirring. The pH value of the mixture was adjusted to 12 with sodium hydroxide aqueous solution (1.0 M). Then, the reaction solution was quickly heated to 170° C. and heated at this temperature for 5 min. The final product was collected by centrifugation, washed 3 times with deionized water, and dried in a freeze dryer to obtain a Ce-CA1-Pt catalyst material.
[0072] The application of cerium oxide doped carbon supported platinum carbon catalyst (Ce-CA1-Pt) in hydrogen fuel cells is as follows:
[0073] Take 100 mg of the catalyst prepared in step 2), add 15 g of deionized water and 20 g of isopropanol successively, add 0.6 g of Nafi on solution (5 wt%) after ultrasonic dispersion for 30 min, and then high-speed shear dispersion for 50 min to obtain the final slurry. When preparing the catalyst slurry, keep the water in the ultrasonic cleaning machine in an ice-water bath state at 15°C. Add the prepared catalyst slurry into the injection tube of ultrasonic spraying, and use ultrasonic spraying to spray the catalyst slurry to both sides of the proton exchange membrane respectively. The process parameters of ultrasonic spraying are set as follows: vacuum chuck temperature 105°C, nozzle air pressure 110 kPa, slurry flow rate 5 mL / min, step width 8 mm, nozzle height 30 mm, nozzle travel speed 150 mm / min. The effective working area of the obtained CCM is 5 cm×5 cm, and the amount of platinum used for the cathode and anode is 0.3 and 0.05 mg / cm respectively. 2 .
[0074] Use 25cm 2 The membrane electrode test was carried out using a standard single cell fixture. During the test, the temperature of the humidification tank and the single cell fixture was controlled by electric heating to adjust the humidity of the positive and negative electrodes of the membrane electrode. The membrane electrode test conditions were as follows: the stoichiometric ratio of H2 / Ai r was 1.5 / 2.0, and the back pressure was 1 bar. The constant pressure activation was 30 minutes before the polarization curve test, and the cumulative activation was 120 minutes.
[0075] Example 3
[0076] A method for preparing a cerium oxide-doped carbon-supported platinum-carbon catalyst (Ce-CA2-Pt), comprising the following steps:
[0077] 1) Dissolve 11g of resorcinol in 100mL of anhydrous ethanol and ultrapure water (V (超纯水) :V (无水乙醇) =1:1), then add concentrated hydrochloric acid (wt, 37%) 5mL and Ce(NO3)3·6H2O, 1.65g, stir at 25℃, closed conditions for 1h until the reactants are completely dissolved, then add formaldehyde solution (wt, 37%) 15mL to the solution, stir vigorously for 1h under the same conditions, oil bath, 75℃, stir with a stirrer at 300r / min, react for 6h to obtain an organic wet gel, cool to room temperature after drying, centrifuge and wash with water 3 times, dry in a vacuum drying oven at 80℃ for 12h, then put the obtained material into a tube furnace, in an argon atmosphere, at 5℃min -1 The heating rate is 0.0447 W, the carbonization temperature is 750 °C, and the carbonization time is 5 h, then the CeO2-doped carbon aerogel / carbon carrier (Ce-CA2) material can be obtained.
[0078] Figure 1 This is the scanning electron microscope image of Ce-CA2 carbon support. Figure 2This is a transmission electron microscope scan of Ce-CA2 carbon support. Figure 3 is the C element mapping diagram of Ce-CA2, Figure 4 is the Ce element mapping diagram of Ce-CA2, Figure 5 This is the O element mapping diagram of Ce-CA2. Figure 1-5 From the characterization data, it can be seen that the doping material is a Ce-containing material, that is, cerium-doped carbon aerogel / carbon carrier material.
[0079] 2) 150 mg of Ce-CA2 material prepared in step 1) was evenly dispersed in 200 mL of ethylene glycol by ultrasonic treatment, and 10 mL of H2PtCl6 solution (10 mg Pt mL -1 ) was added dropwise to the mixture under vigorous stirring. The pH value of the mixture was adjusted to 12 with sodium hydroxide aqueous solution (1.0 M). Then, the reaction solution was rapidly microwaved to 170° C. and heated at this temperature for 5 min. The final product was collected by centrifugation, washed 3 times with deionized water, and dried in a freeze dryer to obtain a Ce-CA2-Pt catalyst material.
[0080] The application of cerium oxide doped carbon supported platinum carbon catalyst (Ce-CA2-Pt) in hydrogen fuel cells is as follows:
[0081] Take 100 mg of the catalyst prepared in step 2), add 15 g of deionized water and 20 g of isopropanol successively, add 0.6 g of Nafi on solution (5 wt%) after ultrasonic dispersion for 30 min, and then high-speed shear dispersion for 50 min to obtain the final slurry. When preparing the catalyst slurry, keep the water in the ultrasonic cleaning machine in an ice-water bath state at 15°C. Add the prepared catalyst slurry into the injection tube of ultrasonic spraying, and use ultrasonic spraying to spray the catalyst slurry to both sides of the proton exchange membrane respectively. The process parameters of ultrasonic spraying are set as follows: vacuum chuck temperature 105°C, nozzle air pressure 110 kPa, slurry flow rate 5 mL / min, step width 8 mm, nozzle height 30 mm, nozzle travel speed 150 mm / min. The effective working area of the obtained CCM is 5 cm×5 cm, and the amount of platinum used for the cathode and anode is 0.3 and 0.05 mg / cm respectively. 2 .
[0082] Use 25cm 2 The membrane electrode test was carried out using a standard single cell fixture. During the test, the temperature of the humidification tank and the single cell fixture was controlled by electric heating to adjust the humidity of the positive and negative electrodes of the membrane electrode. The membrane electrode test conditions were as follows: the stoichiometric ratio of H2 / Ai r was 1.5 / 2.0, and the back pressure was 1 bar. The constant pressure activation was 30 minutes before the polarization curve test, and the cumulative activation was 120 minutes.
[0083] Figure 6 The polarization curves of CA-Pt prepared in Example 1 and Ce-CA2-Pt prepared in Example 3 are shown in Figure 1. The comparison shows that at 2000 mA / cm 2 Under the current density, the voltage of the sample prepared by Ce-doped material reached 0.625V, exceeding the 0.585V of the undoped one.
[0084] Example 4
[0085] A method for preparing a cerium oxide-doped carbon-supported platinum-carbon catalyst (Ce-CA3-Pt), comprising the following steps:
[0086] 1) Dissolve 11g of resorcinol in 100mL of anhydrous ethanol and ultrapure water (V (超纯水) :V (无水乙醇) =1:1), then add concentrated hydrochloric acid (wt, 37%) 5mL and Ce(NO3)3·6H2O, 2.2g, stir at 25℃, closed conditions for 1h until the reactants are completely dissolved, then add formaldehyde solution (wt, 37%) 15mL to the solution, stir vigorously for 1h under the same conditions, oil bath, 75℃, stir with a stirrer at 300r / min, react for 6h to obtain an organic wet gel, cool to room temperature after drying, centrifuge and wash with water 3 times, dry in a vacuum drying oven at 80℃ for 12h, then put the obtained material into a tube furnace, in an argon atmosphere, at 5℃min -1 The heating rate is 0.0447 W, the carbonization temperature is 750 °C, and the carbonization time is 5 h, then the CeO2-doped carbon aerogel / carbon carrier (Ce-CA3) material can be obtained.
[0087] 2) Disperse 150 mg of Ce-CA3 material obtained in step 1) in 200 mL of ethylene glycol by ultrasonic treatment. -1 ) was added dropwise to the mixture under vigorous stirring. The pH value of the mixture was adjusted to 12 with sodium hydroxide aqueous solution (1.0 M). Then, the reaction solution was rapidly microwaved to 170° C. and heated at this temperature for 5 min. The final product was collected by centrifugation, washed 3 times with deionized water, and dried in a freeze dryer to obtain a Ce-CA3-Pt catalyst material.
[0088] The application of cerium oxide doped carbon supported platinum carbon catalyst (Ce-CA3-Pt) in hydrogen fuel cells is as follows:
[0089] Take 100 mg of the catalyst prepared in step 2), add 15 g of deionized water and 20 g of isopropanol successively, add 0.6 g of Nafi on solution (5 wt%) after ultrasonic dispersion for 30 min, and then high-speed shear dispersion for 50 min to obtain the final slurry. When preparing the catalyst slurry, keep the water in the ultrasonic cleaning machine in an ice-water bath state at 15°C. Add the prepared catalyst slurry into the injection tube of ultrasonic spraying, and use ultrasonic spraying to spray the catalyst slurry to both sides of the proton exchange membrane respectively. The process parameters of ultrasonic spraying are set as follows: vacuum chuck temperature 105°C, nozzle air pressure 110 kPa, slurry flow rate 5 mL / min, step width 8 mm, nozzle height 30 mm, nozzle travel speed 150 mm / min. The effective working area of the obtained CCM is 5 cm×5 cm, and the amount of platinum used for the cathode and anode is 0.3 and 0.05 mg / cm respectively. 2 .
[0090] Use 25cm 2 The membrane electrode test was carried out using a standard single cell fixture. During the test, the temperature of the humidification tank and the single cell fixture was controlled by electric heating to adjust the humidity of the positive and negative electrodes of the membrane electrode. The membrane electrode test conditions were as follows: the stoichiometric ratio of H2 / Ai r was 1.5 / 2.0, and the back pressure was 1 bar. The constant pressure activation was 30 minutes before the polarization curve test, and the cumulative activation was 120 minutes.
[0091] The electrochemical test results show that the performance improvement effect is obvious. 2 At the current density, the voltage of the sample prepared by Ce doping material exceeds that of the undoped one.
[0092] Comparative Example 1
[0093] The general method for preparing carbon aerogel is to use resorcinol and formaldehyde as raw materials, obtain wet gel by sol-gel method under the action of acidic or alkaline catalyst, and then carry out solvent exchange, supercritical drying and high-temperature carbonization to finally obtain carbon aerogel material. In addition, resorcinol and formaldehyde are used as precursors, and the reverse suspension polymerization method is adopted to use alcohols and esters to regulate the structure. There are also methods to obtain carbon aerogel materials with high specific surface area through normal pressure drying, carbonization and activation processes. For details, see: {Jin Liang et al. Preparation and application of resorcinol-formaldehyde based carbon aerogel [J]. Anhui Chemical Industry, 2013, 5(49), 74}.
[0094] By comparison, it can be seen that the calcination temperature and time adopted in the present invention, as well as the use of concentrated hydrochloric acid in the acidic conditions for the preparation of the wet gel, result in a product with high microstructure uniformity and a chain-like distribution, which can provide a large number of uniform attachment points for Pt particles, provide maximized active sites for the hydrogen-oxygen catalytic reaction, improve the catalytic efficiency, and thus improve the overall electrochemical performance of the membrane electrode.
[0095] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A method for preparing a cerium oxide-doped carbon-supported platinum-carbon catalyst, characterized in that: The preparation method comprises the following steps: 1) dissolving resorcinol in a mixed solution of anhydrous ethanol and ultrapure water, adding concentrated hydrochloric acid and a cerium source, stirring under a closed condition at room temperature, and then adding formaldehyde solution dropwise, stirring to obtain a mixed solution; 2) heating the mixed solution to react and obtain an organic wet gel; 3) Carbonizing the organic wet gel to obtain CeO2-doped carbon aerogel / carbon carrier material; 4) CeO2-doped carbon aerogel / carbon carrier material is dispersed in ethylene glycol, and H2PtCl6 solution is added dropwise to the obtained mixed solution under stirring. After adjusting the pH value to 12, microwave heating is performed for reaction, and after freeze-drying, a cerium oxide-doped carbon carrier platinum-carbon catalyst is obtained.
2. The preparation method according to claim 1, characterized in that: In step 1), the volume ratio of anhydrous ethanol to ultrapure water is 1:
1.
3. The preparation method according to claim 1, characterized in that: In step 1), the molar ratio of resorcinol to formaldehyde in the formaldehyde solution is n R :n F =1 / 2~1 / 3:
1.
4. The preparation method according to claim 1, characterized in that: In step 1), the cerium source is selected from Ce(NO3)3·6H2O, and the mass of the added cerium source is 10% to 20% of the mass of resorcinol.
5. The preparation method according to claim 1 or 4, characterized in that: In step 2), the heating reaction is carried out in an oil bath, the reaction temperature is 55-80° C., and the reaction time is 6-12 h.
6. The preparation method according to claim 1, characterized in that: In step 3), the carbonization treatment conditions are: in an argon atmosphere, the carbonization temperature is 650-850° C., and the treatment time is 3-5 hours.
7. The preparation method according to claim 1, characterized in that: In step 4), the dosage ratio of CeO2 doped carbon aerogel / carbon carrier material to ethylene glycol is 0.7-0.8 mg / mL, the volume ratio of H2PtCl6 solution to ethylene glycol is 1:20, and the concentration of the H2PtCl6 solution is a Pt content of 10 mg / mL.
8. The preparation method according to claim 1 or 7, characterized in that: In step 4), the reaction is heated by microwave, the microwave heating temperature is 170° C., and the reaction time is 5 min.
9. A cerium oxide-doped carbon-supported platinum-carbon catalyst prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the cerium oxide-doped carbon-supported platinum-carbon catalyst according to claim 9 in a hydrogen fuel cell.