Thin-wall carbon nanotube and preparation method thereof
By using low-flow propane in bimetallic catalysts to prepare thin-walled carbon nanotubes, the problems of many structural defects, large raw material consumption and low purity in the prior art are solved, and the efficient preparation of high-performance carbon nanotubes and high resource efficiency are achieved. use.
Patent Information
- Application Number
- CN202411048691.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
The existing carbon nanotube preparation methods have problems such as many structural defects, large raw material consumption, difficulty in separating metals and low purity, especially few researches on propane to form carbon nanotubes with high graphitization.
The low-flow velocity propane is used as the carbon source, and thin-walled carbon nanotubes are grown in bimetallic catalysts by chemical vapor deposition. The cobalt or iron source is mixed with magnesium source, citric acid and deionized water, and prepared by calcining and grinding. The catalyst powder was combined with dilute acid treatment and deionized washing to obtain high-purity thin-walled carbon nanotubes.
Reduces gas usage and operating costs, improves reaction safety performance, reduces structural defects of carbon nanotubes, realizes the large-scale preparation and application of high-performance carbon nanomaterials, and utilizes shale gas or petroleum refining by-product propane , fully explored the potential of petrochemical resources.
Smart Images

Figure CN118978151A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a thin-wall carbon nanotube and a preparation method thereof, belonging to the technical field of thin-wall carbon nanotube materials and preparation methods thereof. Background Art
[0002] As one of the allotropes of carbon, carbon nanotubes have attracted great attention in various fields such as chemistry, physics, materials science, and electronics at home and abroad since their discovery. This is mainly due to their unique structure, excellent mechanical and electrical properties, and their potential applications. Carbon nanotubes are a tubular nanostructure composed of one, two or more layers of graphene sheets arranged in a spiral manner around their central axis. This cylindrical structure has seamless hollowness and has end caps formed by half of the fullerene atoms. According to the number of layered graphene sheets, it can be divided into single-walled carbon nanotubes, double-walled carbon nanotubes, and multi-arm carbon nanotubes. Among them, the tubular structure formed by only one layer of graphene sheets is a single-walled carbon nanotube, the tubular structure formed by two layers of graphene sheets is a double-walled carbon nanotube, and the tubular structure formed by multiple layers of graphene sheets is called a multi-walled carbon nanotube. The growth conditions of double-walled carbon nanotubes are similar to those of single-walled carbon nanotubes. When single-walled or double-walled carbon nanotubes are synthesized by arc method and chemical vapor deposition method, in addition to single-walled (or double-walled) carbon nanotubes, the products are usually accompanied by a certain number of double-walled (or single-walled) carbon nanotubes. Sometimes, multi-walled carbon nanotubes with three layers of walls are even found. Therefore, the product containing both single-walled carbon nanotubes and double-walled carbon nanotubes is generally called thin-walled carbon nanotubes.
[0003] The existing methods for synthesizing carbon nanotubes mainly include arc discharge method, laser evaporation method, plasma method, template method and chemical vapor deposition method. Chemical vapor deposition method has the advantages of low cost, high yield and good scalability, and is currently the most widely used method. The method for preparing single-walled carbon nanotubes by arc discharge method, using transition metal as catalyst, the catalyst and graphite powder are fully mixed in proportion to obtain an anode rod, and the anode graphite is placed in an arc chamber filled with carbon monoxide and buffer gas and directly opposite to the cathode graphite rod, and arc discharge is performed. For example, patent No. CN117819534A discloses a method of utilizing the high temperature conditions of plasma arc to evaporate the catalyst material on the surface of the floating liquid anode to form fine particles, which are combined with the organic carbon source that is cracked at the same time to catalyze the growth into single-walled carbon nanotubes. However, the process of preparing the anode rod is relatively complicated, and needs to be carried out in a vacuum chamber, and the required current and voltage are large.
[0004] At present, the carbon source used for carbon nanotubes is mainly based on low-carbon alkanes, olefins, alcohols, etc., and the carbon source is mostly low-carbon alkanes such as methane, carbon monoxide, acetylene, etc., propane is less, and most of them need to be passed through a precursor gas to activate the catalyst, and the catalyst of the reaction often needs to add other elements, which will make the carbon nanotubes not easy to purify and the cost of preparation is high. For example, the patent document number CN102320593B discloses a method of using large-flow hydrogen as a carrier gas, ferrocene as a catalytic precursor, and sulfur powder is added to obtain carbon nanotubes using a floating chemical vapor deposition method. CN114604855A discloses a method for catalytically synthesizing single-walled carbon nanotubes based on atomic layer deposition, in which a silicon dioxide layer and a metal layer are deposited in sequence as catalysts, and acetylene, hydrogen, and argon are used as reaction gases to catalytically synthesize single-walled carbon nanotubes. The method has a large gas consumption, and the flow rates of acetylene and helium are up to 25 cubic meters per hour. CN113148982B discloses a method for preparing double-walled carbon nanotubes, which uses acid to activate the amphoteric metal oxides in the residual catalyst, then uses sodium hydroxide to completely remove the amphoteric metal oxides, and uses concentrated hydrochloric acid to remove the active metal and other residual metal oxides, and finally prepares double-walled carbon nanotubes. This method requires the use of multiple acids to purify carbon nanomaterials, and the purification steps are relatively complicated. In addition, it is known from the above-mentioned documents and patent reports that the current preparation of multi-walled carbon nanotubes still has problems such as low yield and low product purity.
[0005] In addition, propane, as a byproduct of shale gas and refining, has a wide range of sources and its main purpose is to use its chemical energy as a civilian fuel. In recent years, the proportion of clean energy represented by natural gas in the civilian gas market has risen rapidly, and propane consumption in the fuel market has declined. Therefore, converting low-carbon hydrocarbons such as propane into other carbon-containing chemicals is a powerful way to open up new application areas and achieve efficient resource utilization, and also provides research directions and technical support for the high-value utilization of low-carbon alkanes. For example, CN117820069B provides a method for propylene obtained by oxidative dehydrogenation of propane, and its preparation process is carried out at normal pressure using doped carbon-coated nickel-chromium alloy atomic clusters as non-precious metal catalysts. CN118028836A provides a method for electrochemical conversion of propane to propylene, in which a substance with a reduced oxygen content is prepared by cathode electrolysis of oxides, and propane is introduced into the anode for partial dehydrogenation to obtain propylene. In addition, there is also propane high-temperature dehydrogenation to produce propylene by heterogeneous catalysts. However, the above-mentioned prior art is all about the study of propane catalytic cracking of olefins, and there is less research on propane into carbon nanotubes with a high degree of graphitization. Therefore, it is very necessary to provide a method for preparing high-purity thin-walled carbon nanotubes using propane in a low flow rate state as a carbon source. Summary of the invention
[0006] The present invention aims to solve the problems of existing thin-walled carbon nanotube products, such as many structural defects, large raw material consumption, difficulty in separating metals and low purity, and provides a thin-walled carbon nanotube and a preparation method thereof.
[0007] The technical solution of the present invention:
[0008] One of the purposes of the present invention is to provide a method for preparing thin-walled carbon nanotubes, the preparation method comprising: using propane in a low flow rate state as a carbon source, and using a chemical vapor deposition method to grow thin-walled carbon nanotubes in a catalyst;
[0009] The preparation method comprises the following steps:
[0010] (1) adding a magnesium source or an aluminum source, citric acid and deionized water to a cobalt source or an iron source, mixing them evenly, and then heating to remove water to obtain a gel-like mixture, and then performing a secondary calcination treatment. The calcined product is ground to obtain a catalyst powder;
[0011] (2) Spreading the catalyst powder on a substrate, evacuating the substrate, filling it with an inert gas, heating it to a reaction temperature, and introducing propane. After the reaction is completed, thin-walled carbon nanotubes grown on the metal catalyst are obtained;
[0012] (3) Mixing the vapor-deposited thin-walled carbon nanotubes with dilute acid to dissolve the metal catalyst dispersed in the thin-walled carbon nanotube product, stirring and filtering, washing the precipitate with deionized water until it is neutral, soaking it with anhydrous ethanol, and drying it to obtain the thin-walled carbon nanotubes.
[0013] It is further defined that the molar ratio of the cobalt source or iron source to the magnesium source or aluminum source in (1) is (0.1-0.3):1, and the proportion of citric acid in the mixture is 10-15%wt.
[0014] It is further defined that the molar ratio of the cobalt source or iron source to the magnesium source or aluminum source in (1) is 0.1:1.
[0015] It is further defined that the molar ratio of the cobalt source or iron source to the magnesium source or aluminum source in (1) is 0.14:1.
[0016] It is further defined that the molar ratio of the cobalt source or iron source to the magnesium source or aluminum source in (1) is 0.18:1.
[0017] It is further defined that the molar ratio of the cobalt source or iron source to the magnesium source or aluminum source in (1) is 0.22:1.
[0018] It is further defined that the molar ratio of the cobalt source or iron source to the magnesium source or aluminum source in (1) is 0.26:1.
[0019] It is further defined that the molar ratio of the cobalt source or iron source to the magnesium source or aluminum source in (1) is 0.3:1.
[0020] It is further defined that: (1) the cobalt source is a hydrate of cobalt nitrate; the iron source is a hydrate of iron nitrate; the magnesium source is a hydrate of magnesium nitrate; and the aluminum source is a hydrate of aluminum nitrate.
[0021] It is further defined that the mixing conditions of the cobalt source or iron source, magnesium source or aluminum source, citric acid and deionized water in (1) are: stirring at 450 rpm for 3-4 hours at room temperature.
[0022] It is further defined that the heating treatment conditions for removing moisture in (1) are: heating at 70-80°C for 4 hours, and transferring to a 70°C oven until a gel-like mixture is obtained.
[0023] It is further defined that the secondary calcination treatment process in (1) is as follows: first calcination: the gel state mixture is placed in a muffle furnace under an air atmosphere of 500-750°C and calcined for 15-25 minutes, and then naturally cooled to room temperature before the second calcination. The second calcination process is as follows: the mixture is placed in a muffle furnace under an air atmosphere of 700-1000°C and calcined for 30-40 minutes, and then naturally cooled to room temperature.
[0024] Furthermore, the first calcination temperature is 530°C.
[0025] Furthermore, the first calcination temperature is 570°C.
[0026] Furthermore, the first calcination temperature is 600°C.
[0027] Furthermore, the first calcination temperature is 670°C.
[0028] Furthermore, the first calcination temperature is 700°C.
[0029] Furthermore, the second calcination temperature is 720°C.
[0030] Furthermore, the second calcination temperature is 750°C.
[0031] Furthermore, the second calcination temperature is 770°C.
[0032] Furthermore, the second calcination temperature is 800°C.
[0033] Furthermore, the second calcination temperature is 820°C.
[0034] Furthermore, the second calcination temperature is 850°C.
[0035] Furthermore, the second calcination temperature is 870°C.
[0036] Further defined, (1) the calcined product obtained is lightly ground and passed through a 50-mesh sieve to obtain a catalyst powder.
[0037] It is further defined that in (2), the inert gas is introduced after evacuating the vacuum to a vacuum pressure reading of 100 kPa.
[0038] It is further defined that the inert gas in (2) is argon or nitrogen with a flow rate of 12-18 L / h; and the propane flow rate is 0.3-3 L / h.
[0039] It is further defined that the propane flow rate in (2) is 0.6 L / h.
[0040] It is further defined that the propane flow rate in (2) is 0.9 L / h.
[0041] It is further defined that the propane flow rate in (2) is 1.2 L / h.
[0042] It is further defined that the propane flow rate in (2) is 1.5 L / h.
[0043] It is further defined that the propane flow rate in (2) is 1.8 L / h.
[0044] It is further defined that the propane flow rate in (2) is 2.1 L / h.
[0045] It is further defined that the propane flow rate in (2) is 2.4 L / h.
[0046] It is further defined that the reaction temperature in (2) is 680-950°C and the heating rate is 20-30°C / min.
[0047] It is further defined that the temperature in (2) is 700°C.
[0048] It is further defined that the temperature in (2) is 750°C.
[0049] It is further defined that the temperature in (2) is 800°C.
[0050] It is further defined that the reaction temperature in (2) is 850°C.
[0051] It is further defined that the temperature in (2) is 900°C.
[0052] It is further defined that the reaction temperature in (2) is 950°C.
[0053] It is further defined that after the reaction in (2) is completed, the propane is stopped from being introduced, the mixture is cooled to room temperature under the protection of an inert gas, and the material on the substrate is scraped off to obtain the thin-walled carbon nanotubes after the catalyst vapor deposition.
[0054] It is further defined that the dilute acid in (3) is a 5-7 mol / L nitric acid solution.
[0055] It is further defined that the stirring and dissolving catalyst conditions in (3) are: stirring at a speed of 450 r / min overnight.
[0056] The second object of the present invention is to provide a thin-walled carbon nanotube prepared by the above method, wherein the number of tube walls of the thin-walled carbon nanotube is within 3 layers, the tube diameter is 1.8-3.2nm, and the interlayer spacing is 0.31-0.36nm.
[0057] It is further defined that the tube diameter is 2.2-2.4 nm.
[0058] Beneficial effects:
[0059] The present invention uses propane with a low flow rate as a carbon source, and uses a bimetallic catalyst to prepare thin-walled carbon nanotubes by chemical vapor deposition. Compared with the existing traditional chemical vapor deposition method, it is not necessary to introduce a reducing precursor gas such as hydrogen, methane or carbon monoxide to pre-reduce the oxide to improve its catalytic activity, reduce the amount of such gas, and greatly reduce the operating cost while improving the safety performance of the reaction. In addition, the bimetallic catalyst selected by the present invention only needs to be washed with a dilute nitric acid solution to be removed, and the structural defects of the carbon nanotubes are also reduced. Further, the cobalt oxide in the bimetallic catalyst prepared by the present invention is compounded with magnesium oxide of various crystal forms, and there is no need to use MgO, Al2O3, SiO2 and other carriers, and the cobalt and magnesium elements are well dispersed, the structure is loose and dispersed, and the particles are fine and uniform, which is conducive to the growth of high-quality carbon nanotubes. In addition, the present invention uses propane from shale gas or petroleum refining byproducts as a carbon source, which can fully explore the potential of existing petrochemical resources, and the reaction process uses less raw materials, and the obtained carbon product has a high degree of graphitization, which provides a new way for the large-scale preparation and application of high-performance carbon nanomaterials. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 XRD spectrum of the bimetallic catalyst prepared in Example 1;
[0061] Figure 2 The SEM image and EDS spectrum of the bimetallic catalyst prepared in Example 1;
[0062] Figure 3 TEM photo of the thin-walled carbon nanotubes prepared in Example 1;
[0063] Figure 4 The Raman spectrum of the thin-walled carbon nanotubes prepared in Example 1;
[0064] Figure 5 The SEM image and EDS spectrum of the carbon product prepared in Example 1;
[0065] Figure 6 The XRD spectrum of the carbon product prepared in Example 1 after acid treatment;
[0066] Figure 7 The thermal gravimetric curve of the thin-walled carbon nanotubes prepared in Example 1;
[0067] Figure 8 XRD spectra of the bimetallic catalysts prepared in Examples 2, 3 and 4;
[0068] Fig. 9 XRD spectrum of the bimetallic catalyst prepared in Comparative Example 1;
[0069] Fig.10 The XRD comparison spectra of the product prepared in Comparative Example 1 before and after acid washing;
[0070] Fig.11 This is the particle size distribution diagram of the thin-walled carbon nanotubes prepared in Example 1. DETAILED DESCRIPTION
[0071] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0072] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0073] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0074] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art, and the purity of the solid and liquid reagents used is analytically pure.
[0075] Example 1
[0076] The method for preparing thin-walled carbon nanotubes in this embodiment is carried out according to the following steps:
[0077] Step 1: Preparation of Co-Mg bimetallic catalyst by secondary calcination
[0078] 3.98 g of cobalt nitrate hexahydrate and 15.95 g of magnesium nitrate hexahydrate were mixed at a molar ratio of 0.22:1, and then 5.5 g of citric acid monohydrate and 50 mL of deionized water were added and stirred to dissolve. The mixture was heated and stirred at a speed of 450 rpm until it became a slurry (the heating temperature was controlled between 70-80° C. so that the water in the mixed solution could be separated quickly without boiling, and no precipitation or crystallization occurred during this process), and then transferred to a 70° C. oven and dried to obtain a gel-like mixture.
[0079] The gel state mixture was taken out and placed in a muffle furnace at 550°C for calcination for 15 minutes. After being taken out and naturally cooled, it was placed in a muffle furnace at 800°C and calcined for 0.5 hours. After being taken out and naturally cooled, it was lightly ground to obtain a bimetallic catalyst with a loose and dispersed structure, fine and uniform particles, and capable of passing through a 50-mesh sieve, which was set aside.
[0080] The structure of the obtained bimetallic catalyst was characterized, and the XRD spectrum was as follows: Figure 1 As shown by Figure 1 It can be seen that a composite bimetallic catalyst of MgO and CoO is obtained, and MgO has multiple crystal planes, specifically corresponding to (111), (200), (220), (311) and (222) crystal planes, and the peak intensity of cobalt oxide is obvious.
[0081] The obtained bimetallic catalyst was characterized by microstructure, SEM images and corresponding EDS analysis. Figure 2 As shown by Figure 2 It can be seen that the bimetallic catalyst has a loose and dispersed structure, fine and uniform particles, and EDS shows that the metal cobalt element is well composited with MgO on various crystal faces. Mg, Co, and O elements are dispersed at the nanoscale, and the content of Co element is relatively low compared to the other two elements, indicating that Co atoms are likely to be dispersed on the surface or subsurface of MgO, which can improve metal utilization efficiency, reduce the amount of transition metal used, and reduce the cost of catalyst preparation.
[0082] Step 2: Preparation of thin-walled carbon nanotubes by chemical vapor deposition
[0083] Weigh 0.2 g of the bimetallic catalyst obtained in step 1, and cover the bimetallic catalyst powder on a quartz thin sheet substrate, and then place the whole in the heating area of a horizontal quartz tube furnace. After sealing, evacuate until the vacuum pressure display reads to 100 kPa, fill with argon to normal pressure, heat to 750°C at a heating rate of 24°C / min, introduce propane at a flow rate of 0.9 L / h, and adjust the flow rate of argon to 15 L / h, maintain the reaction for 40 minutes, stop introducing propane, and continue to maintain the introduction of argon until it cools to room temperature, collect the carbon product on the quartz sheet, and weigh it to obtain about 0.36 g of carbon product.
[0084] The obtained carbon product was mixed with 6 mol / L nitric acid solution and stirred at 450 r / min overnight. After solid-liquid separation, the precipitate was washed with ionized water to a pH of 7, then rinsed with anhydrous ethanol and dried to obtain acid-treated thin-walled carbon nanotubes.
[0085] The microscopic morphology of the obtained thin-walled carbon nanotubes was characterized, and the TEM photos are shown in Figure 3 As shown by Figure 3 It can be seen that the prepared carbon nanotubes are within three layers, the interlayer spacing is between 0.31 and 0.36 nm, and the tube diameter is relatively large. Further analysis of the particle size distribution of the obtained thin-walled carbon nanotubes is shown in the following results: Fig.11 As shown by Fig.11 It can be seen that the diameter of thin-walled carbon nanotubes is 1.8-3.2nm, mainly distributed in 2.2-2.4nm.
[0086] The D peak in the Raman spectrum is caused by the defect structure in the carbon nanotubes, which is a disordered vibration between carbon bonds, mainly sp3 hybridization. The D peak intensity is positively correlated with the content of defect structure in the carbon nanotubes. G / I D Estimation of the purity of carbon nanotubes, I G / I D The larger the value, the more complete the carbon tube structure. The Raman spectrum of the thin-walled carbon nanotubes prepared in this example is as follows: Figure 4 As shown by Figure 4 It can be seen that the I G / I D As high as 10, it means that the obtained thin-walled carbon nanotubes have a high degree of graphitization and fewer defects. Figure 7 As shown by Figure 7 It can be seen that the sample loses weight at around 430°C to 600°C, which is mainly attributed to the SWCNTs and crystalline carbon particles contained in the sample, which are oxidized to produce carbon dioxide within this temperature range, resulting in a weight loss.
[0087] The microstructure of the obtained carbon product was characterized by SEM photos and corresponding EDS analysis. Figure 5 As shown by Figure 5 It can be seen that the metal elements of the carbonized catalyst are evenly distributed in the thin-walled carbon nanotubes. Figure 3 It can be concluded that the distribution of each element before and after the catalyst reaction is uniform, which is conducive to the growth of thin-walled carbon nanotubes and the reduction of structural defects, saving metal consumption. The structure of thin-walled carbon nanotubes is further characterized, and the XRD spectrum is shown in Figure 6 As shown, compared Figure 6 and Figure 1It can be seen that after acid washing and purification, there is no metal phase in the thin-walled carbon nanotubes, only graphite carbon, and the corresponding crystal planes are (002) and (101), and the separation effect is good.
[0088] Example 2
[0089] The difference between this embodiment and embodiment 1 is that in step 1, the molar ratio of cobalt nitrate hexahydrate to magnesium nitrate hexahydrate is 0.1:1, and the remaining process steps and parameter settings are the same as those in embodiment 1, to prepare a Co-Mg bimetallic catalyst.
[0090] Example 3
[0091] The difference between this embodiment and embodiment 1 is that in step 1, the molar ratio of cobalt nitrate hexahydrate to magnesium nitrate hexahydrate is 0.22:1, and the remaining process steps and parameter settings are the same as those in embodiment 1, to prepare a Co-Mg bimetallic catalyst.
[0092] Example 4
[0093] The difference between this embodiment and embodiment 1 is that in step 1, the molar ratio of cobalt nitrate hexahydrate to magnesium nitrate hexahydrate is 0.3:1, and the remaining process steps and parameter settings are the same as those in embodiment 1, to prepare a Co-Mg bimetallic catalyst.
[0094] The structures of the Co-Mg bimetallic catalysts prepared in Examples 2 to 4 were characterized, and the XRD comparison spectra were as follows: Figure 8 As shown by Figure 8 It can be seen that in Example 2, when the Co content is low, there are only MgO and CoO phases; while in Example 1 (when Co / Mg=0.1), there are CoO and MgO phases. As the Co content increases (when Co / Mg=0.3), the Co3O4 phase appears and the strength increases. The corresponding crystal planes of Co3O4 are (111), (220), (311), (400), (511) and (440).
[0095] Comparative Example 1
[0096] The difference between this comparative example and Example 1 is that in step 1, ferric nitrate nonahydrate is used instead of cobalt nitrate hexahydrate, and aluminum nitrate nonahydrate is used instead of magnesium nitrate hexahydrate. The remaining process steps and parameter settings are the same as those in Example 1, and an Fe-Al bimetallic catalyst is prepared.
[0097] The structure of the Fe-Al bimetallic catalyst was characterized, and the XRD spectrum was as follows: Fig. 9 As shown by Fig. 9 It can be seen that a composite bimetallic catalyst of α-Fe2O3 and Al2O3 is obtained.
[0098] The Fe-Al bimetallic catalyst is used to prepare thin-walled carbon nanotubes. The specific process is as follows:
[0099] Weigh 0.2 g of the bimetallic catalyst obtained in step 1, and cover the bimetallic catalyst powder on a quartz thin sheet substrate, and then place the whole in the heating area of a horizontal quartz tube furnace. After sealing, evacuate to a vacuum pressure reading of 100 kPa, fill with argon to normal pressure, heat to 850°C at a heating rate of 24°C / min, introduce propane at a flow rate of 0.9 L / h, and adjust the flow rate of argon to 15 L / h, maintain the reaction for 40 minutes, stop introducing propane, and continue to maintain the introduction of argon until it cools to room temperature, collect the product on the quartz sheet, and weigh it to obtain a thin-walled carbon nanotube product.
[0100] The obtained product was mixed with a 6 mol / L nitric acid solution and stirred at a speed of 450 r / min overnight. After solid-liquid separation, the solid was washed with ionized water to a pH of 7, and then rinsed with anhydrous ethanol and dried to obtain purified thin-walled carbon nanotubes.
[0101] The structure of the product before and after acid washing was characterized. Fig.10 As shown by Fig.10 It can be seen that there are iron carbide peaks, aluminum oxide peaks and sharp graphite carbon (002) crystal planes before and after acid washing, indicating that single acid washing cannot purify the iron and aluminum of carbon nanotubes.
[0102] Although the present invention has been disclosed as above in the preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
Claims
1. A method for preparing thin-walled carbon nanotubes, characterized in that: Using propane in a low flow rate state as a carbon source, a chemical vapor deposition method is used to grow thin-walled carbon nanotubes in a catalyst. The preparation method comprises: (1) adding a magnesium source or an aluminum source, citric acid and deionized water to a cobalt source or an iron source, mixing them evenly, and then heating to remove water to obtain a gel-like mixture, and then performing a secondary calcination treatment. The calcined product is ground to obtain a catalyst powder; (2) spreading the catalyst powder on a substrate, evacuating the substrate, filling it with an inert gas, heating it to a reaction temperature, and introducing propane. After the reaction is completed, a thin-walled carbon nanotube product grown on the metal catalyst is obtained; (3) Mixing the vapor-deposited thin-walled carbon nanotubes with dilute acid to dissolve the metal catalyst dispersed in the thin-walled carbon nanotube product, stirring and filtering, washing the precipitate with deionized water until it is neutral, soaking it with anhydrous ethanol, and drying it to obtain the thin-walled carbon nanotubes.
2. The preparation method according to claim 1, characterized in that: (1) The molar ratio of the cobalt source or iron source to the magnesium source or aluminum source is (0.1-0.3):1, and the proportion of citric acid in the mixture is 10-15%wt.
3. The preparation method according to claim 1, characterized in that: The heating conditions for removing moisture in (1) are: heating at 70-80°C for 4 hours, and transferring to a 70°C oven until a gel-like mixture is obtained.
4. The preparation method according to claim 1, characterized in that: The secondary calcination process in (1) is as follows: the gel state mixture is placed in a muffle furnace under an air atmosphere of 500-750°C and calcined for 15-25 minutes, and then naturally cooled to room temperature. Then, the mixture is placed in a muffle furnace under an air atmosphere of 700-1000°C and calcined for 30-40 minutes, and then naturally cooled to room temperature.
5. The preparation method according to claim 1, characterized in that: (1) The calcined product was ground and passed through a 50-mesh sieve to obtain catalyst powder.
6. The preparation method according to claim 1, characterized in that: (2) The inert gas is argon or nitrogen with a flow rate of 12-18 L / h; the propane flow rate is 0.3-3 L / h.
7. The preparation method according to claim 1, characterized in that: (2) The reaction temperature is 680-950°C and the heating rate is 20-30°C / min.
8. The preparation method according to claim 1, characterized in that: (3) The dilute acid is a 5-7 mol / L nitric acid solution.
9. The preparation method according to claim 1, characterized in that: (3) The stirring conditions for dissolving the catalyst are: stirring at 450 r / min overnight.
10. A thin-walled carbon nanotube prepared by the method according to any one of claims 1 to 9, characterized in that: The number of tube wall layers is less than 3, the interlayer spacing is 0.31-0.36nm, and the tube diameter is 1.8-3.2nm.
Citation Information
Patent Citations
High-magnification carbon nanotubes having ultrafine tube diameter and prepared by two-stage method, catalyst and preparation method of catalyst
CN110801843A
Preparation method for growing narrow-diameter-distribution single-walled carbon nanotubes under assistance of high-melting-point metal oxide by taking methane as carbon source
CN116375004A
Method and equipment for preparing Nano carbon tube with multiple walls
CN1539731A
Composite material including carbon nanotube bulk structure
JP2014122154A