Stress-resistant flame-retardant ABS composite material and preparation method thereof

By adding flame retardant, stress eliminator and ultraviolet absorber to the ABS resin, and using the combination of nanoprecipitated barium sulfate and ultrafine high silica talc, the problem of stress cracking of flame retardant ABS materials in thick-walled product molding is solved. , improves the stress resistance and flame retardant properties of the material, and is suitable for industrial production.

CN118994838APending Publication Date: 2024-11-22NINGBO LANGSHENG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411305594.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Flame-retardant ABS materials are prone to stress cracking during the molding of thick-walled products, resulting in structural defects and mechanical properties degradation. The prior art improves by increasing the melt flow rate but has limited results.

Method used

ABS resin is used as the matrix material, combining flame retardant, stress eliminator and ultraviolet absorber, and the melt index is improved through ABS high glue powder, using a combination of nano-precipitated barium sulfate and ultrafine high silica talc powder to reduce through rapid nucleation. Stress, combined with anionic surfactant and titanate coupling agent, reduces solid-liquid separation stress and improves the stress cracking resistance of the material.

Benefits of technology

It significantly improves the stress crack resistance, flame retardant properties and UV resistance of ABS composite materials, reduces structural defects, enhances the forming and processing capabilities of thick-walled products, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials, and particularly relates to a stress-resistant flame-retardant ABS composite material and a preparation method thereof. The stress-resistant flame-retardant ABS composite material is prepared from the following components in parts by weight: 40 to 80 parts of ABS I, 10 to 30 parts of ABS II, 5 to 15 parts of ABS high rubber powder, 10 to 20 parts of a flame retardant, 1.0 to 3.0 parts of a stress relieving agent, 0.5 to 1.0 part of an antioxidant, 1.0 to 2.0 parts of a lubricating agent and 0.5 to 1.0 part of an ultraviolet light absorber, the stress relieving agent comprises the following components in parts by weight: 25-35 parts of nano precipitated barium sulfate, 60-70 parts of talcum powder, 0.5-1.5 parts of an anionic surfactant and 0.1-1.0 part of a titanate coupling agent, the nano precipitated barium sulfate, the talcum powder and the anionic surfactant are stirred and mixed at a high speed, then the titanate coupling agent is added, and the mixture is stirred and mixed at a low speed to obtain the stress relieving agent. The ABS composite material with excellent stress cracking resistance, flame retardance and ultraviolet resistance is obtained by taking ABS resin as a matrix material and combining with auxiliaries such as a flame retardant, a stress relieving agent and an ultraviolet light absorber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and particularly relates to a stress-resistant and flame-retardant ABS composite material and a preparation method thereof. Background Art

[0002] ABS resin (Acrylonitrile Butadiene Styrene) is a thermoplastic polymer material with high strength, good toughness and easy processing. The styrene component provides good processing performance, the acrylonitrile component contributes to the strength and chemical resistance of the resin, and the butadiene component brings good impact performance to the resin, making ABS resin show advantages such as high strength, corrosion resistance, and high temperature resistance. It is often used to manufacture plastic shells of instruments. Among them, flame-retardant ABS is widely used in electronic appliances and electrical products. Most of these products have complex structures and thick walls. Structural defects are more likely to occur during the preparation process. In addition, the product is used in a light environment, which makes ABS products prone to stress cracking in subsequent use. Stress cracking can cause defects such as deformation and fracture of ABS parts, seriously affecting their appearance quality and performance.

[0003] When the part structure and process cannot be adjusted, changing the structure of the material itself is conducive to improving stress. The magnitude of stress depends on factors such as the macromolecular structure and arrangement of the polymer, the rigidity of the chain segment, and the rheological properties of the melt. Generally, improving the fluidity of the material can improve stress cracking, but if the fluidity is too high, it is easy to cause solid-liquid stratification during the molding process when preparing thick-walled products, thereby causing structural defects and affecting its final mechanical properties. Existing flame-retardant ABS generally improves the material's resistance to stress cracking by increasing the melt flow rate. This can only improve the effect to a certain extent. After the solid-liquid stratification of thick-walled products occurs, it will eventually affect the product's mechanical properties such as falling ball impact strength. Summary of the invention

[0004] The purpose of the present invention is to provide a stress-resistant flame-retardant ABS composite material in view of the above technical problems. The ABS resin is used as a matrix material, combined with additives such as flame retardants, stress relief agents and ultraviolet absorbers, to obtain an ABS composite material with excellent stress cracking resistance, flame retardant properties and UV resistance.

[0005] The stress-resistant flame-retardant ABS composite material in the technical solution of the present invention comprises the following components in parts by weight: 40-80 parts of ABS 1, 10-30 parts of ABS 2, 5-15 parts of ABS high-rubber powder, 10-20 parts of flame retardant, 1.0-3.0 parts of stress reliever, 0.5-1.0 parts of antioxidant, 1.0-2.0 parts of lubricant, and 0.5-1.0 parts of ultraviolet absorber.

[0006] Furthermore, the melt flow rate of ABS-1 is 15.0-20.0 g / 10 min, and the notched impact strength is 250-300 J / m.

[0007] Furthermore, the melt flow rate of ABS II is 3.0~5.0g / 10min, and the notched impact strength is 320~380J / m.

[0008] Using ABS 1 and ABS 2 with different performances and adding ABS high-rubber powder to improve the melt index of the composite material is beneficial to enhancing its fluidity while ensuring the strength of the material, promoting the composite material to obtain uniform components, reducing structural defects, and enhancing its resistance to stress cracking; stress relievers can improve the stress resistance of the composite material while ensuring its mechanical properties, flame retardant properties and weather resistance, which is beneficial to the molding processing of thick-walled products.

[0009] Furthermore, the flame retardant is a mixture of an organic flame retardant and an inorganic flame retardant in a mass ratio of 3 to 6:1.

[0010] Preferably, the organic flame retardant may be one or more of halogen flame retardants such as epoxy bromide, decabromodiphenylethane, and bromotriazine, and bromine nitrogen flame retardants.

[0011] Preferably, the inorganic flame retardant may be one or more of antimony trioxide, magnesium hydroxide, aluminum hydroxide, and zinc borate pentahydrate flame retardant.

[0012] Furthermore, the stress relieving agent comprises the following components in parts by weight: 25-35 parts of nano-precipitated barium sulfate, 60-70 parts of ultrafine high-silicon talc powder, 0.5-1.5 parts of anionic surfactant, and 0.1-1.0 parts of titanate coupling agent.

[0013] Nano-precipitated barium sulfate can promote nucleation and reinforcement. Ultrafine high-silicon talc promotes nucleation and acts as a flame retardant. Combined with anionic surfactants and titanate coupling agents, rapid nucleation can reduce the stress caused by solid-liquid separation during the molding process, thereby effectively eliminating stress.

[0014] Preferably, the anionic surfactant may be one or more of sodium fatty alcohol alkyl sulfonate, alkylamine ester, lauryl alcohol phosphate, sodium ethoxylated alkyl sulfate, polyoxyethylene lauryl alcohol ether, sodium dodecylbenzene sulfonate, and magnesium stearate.

[0015] Furthermore, the stress relieving agent is obtained by mixing nano-precipitated barium sulfate, ultrafine high-silicon talc powder and anionic surfactant with high-speed stirring, and then adding a titanate coupling agent with low-speed stirring.

[0016] Furthermore, the rotation speed of the high-speed stirring is 2500-3500 rpm, and the time is 3-10 min.

[0017] Furthermore, the rotation speed of the low-speed stirring is 200-300 rpm, and the time is 3-10 min.

[0018] Preferably, the antioxidant is one or more of 2,6-di-tert-butyl-p-cresol (antioxidant BHT), pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxyhydrocinnamate) (antioxidant 1010), 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (antioxidant 1076), triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate (antioxidant 245), didodecyl thiodipropionate (antioxidant DLTP), and dioctadecyl 3,3'-thiodipropionate (antioxidant DSTP).

[0019] Furthermore, the lubricant is one or more of vinyl bisstearamide, oxidized polyethylene wax, magnesium stearate, and white oil.

[0020] Furthermore, the ultraviolet absorber is one or more of N,N'-bis(4-ethoxycarbonylphenyl)-N-benzylformamidine (UV-3), 2-(2-hydroxy-5-methylphenyl)benzotriazole (UV-P), 2,2'-hydroxy-4-methoxybenzophenone (UV-24), and 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole (UV-328).

[0021] The present invention also provides a method for preparing the stress-resistant flame-retardant ABS composite material, comprising the following steps: mixing ABS 1, ABS 2, ABS high-rubber powder, flame retardant, stress relieving agent, antioxidant, lubricant and ultraviolet absorber, extruding through a twin-screw extruder, cooling, drying and granulating.

[0022] Furthermore, during extrusion, the main engine speed of the twin-screw extruder is 30-40 rpm.

[0023] Furthermore, the temperature of the twin-screw extruder during extrusion is 180-210°C.

[0024] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: (1) Using ABS resin as the matrix material, combined with additives such as flame retardants, stress relief agents and ultraviolet absorbers, an ABS composite material with excellent stress cracking resistance, flame retardancy and ultraviolet resistance is obtained; (2) ABS high-rubber powder can improve the melt index of the composite material, enhance its fluidity, help the composite material obtain uniform components, reduce structural defects, and enhance its stress cracking resistance; (3) Stress relief agents can improve the stress resistance of composite materials while ensuring their mechanical properties, flame retardancy and weather resistance, which is beneficial to the molding and processing of thick-walled products; (4) Nano-precipitated barium sulfate can promote nucleation and reinforcement. Ultrafine high-silicon talc promotes nucleation and acts as a flame retardant. Combined with anionic surfactants and titanate coupling agents, rapid nucleation can reduce the stress caused by solid-liquid separation during the molding process, thereby effectively eliminating stress. (5) The preparation method of the obtained stress-resistant flame-retardant ABS composite material is simple, efficient and suitable for industrial application. DETAILED DESCRIPTION

[0025] The technical scheme of the present invention is further described below by specific embodiments. It should be understood that the specific embodiments described herein are only used to help understand the present invention and are not intended to be used for specific limitations of the present invention. Unless otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.

[0026] In the following examples and comparative examples, ABS 1 is AG12A1 produced by Taiwan Formosa Chemicals & Chemicals Co., Ltd., ABS 2 is AE8000 produced by Taiwan Formosa Chemicals & Chemicals Co., Ltd., nano-precipitated barium sulfate is AB03N produced by Jimei Fine Chemicals (Guangdong) Co., Ltd., and ultrafine high-silicon talc is XF1250A produced by Quanzhou Xufeng Powder Raw Materials Co., Ltd.

[0027] Embodiment 1:

[0028] The preparation method of the stress-resistant flame-retardant ABS composite material of this embodiment comprises the following steps: (1) 30 parts of nano-precipitated barium sulfate, 68.5 parts of ultrafine high-silicon talc and 1.0 part of magnesium stearate were stirred and mixed at 3000 rpm for 5 minutes, and then 0.5 parts of isopropyl tri(isostearoyl) titanate were added and stirred and mixed at 200 rpm for 5 minutes to obtain a stress relief agent; (2) 50 parts of ABS 1, 20 parts of ABS 2, 10 parts of ABS high-rubber powder, 15 parts of bromotriazine, 3 parts of antimony trioxide, 2 parts of stress reliever, 0.2 parts of antioxidant 245, 0.4 parts of antioxidant DSTP, 1.4 parts of vinyl bisstearamide, 0.2 parts of white oil and 0.6 parts of UV-P were mixed and extruded through a twin-screw extruder with a main engine speed of 35 rpm, followed by cooling, drying and granulation.

[0029] Embodiment 2:

[0030] The preparation method of the stress-resistant flame-retardant ABS composite material of this embodiment comprises the following steps: (1) 28 parts of nano-precipitated barium sulfate, 65 parts of ultrafine high-silicon talc and 1.2 parts of magnesium stearate were stirred and mixed at 2800 rpm for 5 minutes, and then 0.6 parts of di(dioctylpyrophosphoryl) titanium oxyacetate were added and stirred and mixed at 220 rpm for 5 minutes to obtain a stress relief agent; (2) 45 parts of ABS 1, 25 parts of ABS 2, 15 parts of ABS high-rubber powder, 15 parts of bis(hexachlorocyclopentadiene)cyclooctane, 3 parts of antimony trioxide, 2.5 parts of stress reliever, 0.6 parts of antioxidant 245, 0.2 parts of antioxidant 1076, 1.4 parts of vinyl bisstearamide, 0.4 parts of white oil and 0.7 parts of UV-24 were mixed and extruded through a twin-screw extruder with a main engine speed of 35 rpm, followed by cooling, drying and granulation.

[0031] Embodiment three:

[0032] The preparation method of the stress-resistant flame-retardant ABS composite material of this embodiment comprises the following steps: (1) 32 parts of nano-precipitated barium sulfate, 63 parts of ultrafine high-silicon talc and 0.8 parts of magnesium stearate were stirred and mixed at 3200 rpm for 5 minutes, and then 0.4 parts of isopropyl tri(n-ethylamino-ethylamino) titanate were added and stirred and mixed at 250 rpm for 5 minutes to obtain a stress relief agent; (2) 60 parts of ABS 1, 20 parts of ABS 2, 10 parts of ABS high-rubber powder, 12 parts of decabromodiphenylethane, 6 parts of aluminum hydroxide, 1.5 parts of stress reliever, 0.3 parts of antioxidant DLTP, 0.5 parts of antioxidant DSTP, 1.3 parts of vinyl bisstearamide, 0.5 parts of white oil and 0.8 parts of UV-P were mixed and extruded through a twin-screw extruder with a main engine speed of 35 rpm, followed by cooling, drying and granulation.

[0033] Embodiment 4:

[0034] The difference between this embodiment and embodiment 1 is that in step (1), 20 parts of nano-precipitated barium sulfate, 68.5 parts of ultrafine high-silicon talc and 1.0 part of magnesium stearate are stirred and mixed at 3000 rpm for 5 minutes, and then 0.5 parts of isopropyl tri(isostearoyl) titanate are added and stirred and mixed at 200 rpm for 5 minutes to obtain a stress reliever.

[0035] Embodiment five:

[0036] The difference between this embodiment and embodiment 1 is that in step (1), 40 parts of nano-precipitated barium sulfate, 68.5 parts of ultrafine high-silicon talc and 1.0 part of magnesium stearate are stirred and mixed at 3000 rpm for 5 minutes, and then 0.5 parts of isopropyl tri(isostearoyl) titanate are added and stirred and mixed at 200 rpm for 5 minutes to obtain a stress reliever.

[0037] Embodiment six:

[0038] The difference between this embodiment and embodiment 1 is that in step (1), 30 parts of nano-precipitated barium sulfate, 55 parts of ultrafine high-silicon talc and 1.0 part of magnesium stearate are stirred and mixed at 3000 rpm for 5 minutes, and then 0.5 parts of isopropyl tri(isostearoyl) titanate are added and stirred and mixed at 200 rpm for 5 minutes to obtain a stress reliever.

[0039] Embodiment seven:

[0040] The difference between this embodiment and embodiment 1 is that in step (1), 30 parts of nano-precipitated barium sulfate, 75 parts of ultrafine high-silicon talc and 1.0 part of magnesium stearate are stirred and mixed at 3000 rpm for 5 minutes, and then 0.5 parts of isopropyl tri(isostearoyl) titanate are added and stirred and mixed at 200 rpm for 5 minutes to obtain a stress reliever.

[0041] Comparative Example 1 The difference between this comparative example and Example 1 is that in step (2), 50 parts of ABS 1, 20 parts of ABS 2, 10 parts of ABS high-rubber powder, 15 parts of bromotriazine, 3 parts of antimony trioxide, 0.5 parts of stress reliever, 0.2 parts of antioxidant 245, 0.4 parts of antioxidant DSTP, 1.4 parts of vinyl bisstearamide, 0.2 parts of white oil and 0.6 parts of UV-P are mixed, and the material is extruded through a twin-screw extruder with a main engine speed of 35 rpm, and then cooled, dried and granulated.

[0042] Comparative Example 2 The difference between this comparative example and Example 1 is that in step (2), 50 parts of ABS 1, 20 parts of ABS 2, 10 parts of ABS high-rubber powder, 15 parts of bromotriazine, 3 parts of antimony trioxide, 3.5 parts of stress reliever, 0.2 parts of antioxidant 245, 0.4 parts of antioxidant DSTP, 1.4 parts of vinyl bisstearamide, 0.2 parts of white oil and 0.6 parts of UV-P are mixed, and the material is extruded through a twin-screw extruder with a main engine speed of 35 rpm, and then cooled, dried and granulated.

[0043] Comparative Example 3 The difference between this comparative example and Example 1 is that in step (2), 50 parts of ABS 1, 20 parts of ABS 2, 15 parts of bromotriazine, 3 parts of antimony trioxide, 2 parts of stress reliever, 0.2 parts of antioxidant 245, 0.4 parts of antioxidant DSTP, 1.4 parts of vinyl bisstearamide, 0.2 parts of white oil and 0.6 parts of UV-P are mixed, and the material is extruded through a twin-screw extruder with a main engine speed of 35 rpm, and then cooled, dried and granulated.

[0044] Comparative Example 4 The difference between this comparative example and Example 1 is that in step (2), 70 parts of ABS 1, 10 parts of ABS high-rubber powder, 15 parts of bromotriazine, 3 parts of antimony trioxide, 2 parts of stress reliever, 0.2 parts of antioxidant 245, 0.4 parts of antioxidant DSTP, 1.4 parts of vinyl bisstearamide, 0.2 parts of white oil and 0.6 parts of UV-P are mixed, and the material is extruded through a twin-screw extruder with a main engine speed of 35 rpm, and then cooled, dried and granulated.

[0045] Comparative Example 5 The difference between this comparative example and Example 1 is that in step (2), 70 parts of ABS II, 10 parts of ABS high-rubber powder, 15 parts of bromotriazine, 3 parts of antimony trioxide, 2 parts of stress reliever, 0.2 parts of antioxidant 245, 0.4 parts of antioxidant DSTP, 1.4 parts of vinyl bisstearamide, 0.2 parts of white oil and 0.6 parts of UV-P are mixed, and the material is extruded through a twin-screw extruder with a main engine speed of 35 rpm, and then cooled, dried and granulated.

[0046] The mechanical properties of the ABS composite materials obtained in the above examples and comparative examples were tested, wherein the melt flow rate was tested at 220°C / 10.0kg according to ISO 1133 standard, and the notched impact strength was tested according to ISO 180 standard. The test results are shown in Table 1.

[0047]

[0048] In Examples 1-3, ABS resin is used as the matrix material, combined with additives such as flame retardants, stress relievers and ultraviolet absorbers, and the resulting ABS composite materials exhibit excellent mechanical properties; in Example 4, a relatively small amount of nano-precipitated barium sulfate is used as the stress reliever, and in Example 6, a relatively small amount of ultrafine high-silicon talc is used as the stress reliever, so the nucleation effect and the reinforcement effect are reduced, the stress relief effect is deteriorated, and the mechanical properties of the resulting composite materials are deteriorated; in Example 5, a relatively large amount of nano-precipitated barium sulfate is used as the stress reliever, and in Example 7, a relatively large amount of ultrafine high-silicon talc is used as the stress reliever, which increases the difficulty of dispersing the stress reliever in the system, deteriorates the uniformity of the resulting composite materials, and causes mechanical properties to deteriorate. In comparative example 1, less stress relieving agent is used, and the obtained composite material is more prone to stress cracking, resulting in poor mechanical strength; in comparative example 2, more stress relieving agent is used, and the obtained composite material has greater strength, but poor elasticity, resulting in reduced elongation at break and impact strength; in comparative example 3, no ABS high-rubber powder is added, the fluidity of the obtained composite material is weakened, the structural defects increase, stress cracking is prone to occur, and the mechanical strength deteriorates; in comparative example 4, no ABS II is used, and the mechanical fluidity of the obtained composite material is greater, and the mechanical strength deteriorates; in comparative example 5, no ABS I is used, and the fluidity of the obtained composite material is poor, the structural defects increase, stress cracking is prone to occur, and the mechanical properties deteriorate.

[0049] Finally, it should be noted that the specific embodiments described herein are merely examples of the spirit of the present invention, and are not intended to limit the implementation methods of the present invention. Those skilled in the art of the present invention may make various modifications or supplements to the described embodiments or replace them in similar ways. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.

Claims

1. A stress-resistant flame-retardant ABS composite material, characterized in that: The invention comprises the following components in parts by weight: 40-80 parts of ABS 1, 10-30 parts of ABS 2, 5-15 parts of ABS high-rubber powder, 10-20 parts of flame retardant, 1.0-3.0 parts of stress relieving agent, 0.5-1.0 parts of antioxidant, 1.0-2.0 parts of lubricant and 0.5-1.0 parts of ultraviolet absorber.

2. The stress-resistant flame-retardant ABS composite material according to claim 1, characterized in that: The melt flow rate of ABS is 15.0~20.0g / 10min, and the notched impact strength is 250~300J / m.

3. The stress-resistant flame-retardant ABS composite material according to claim 1, characterized in that: The melt flow rate of ABS II is 3.0~5.0g / 10min, and the notched impact strength is 320~380J / m.

4. The stress-resistant flame-retardant ABS composite material according to claim 1, characterized in that: The flame retardant is a mixture of an organic flame retardant and an inorganic flame retardant in a mass ratio of 3 to 6:

1.

5. The stress-resistant flame-retardant ABS composite material according to claim 1, characterized in that: The stress relieving agent comprises the following components in parts by weight: 25-35 parts of nano-precipitated barium sulfate, 60-70 parts of ultrafine high-silicon talc powder, 0.5-1.5 parts of anionic surfactant, and 0.1-1.0 parts of titanate coupling agent.

6. The stress-resistant flame-retardant ABS composite material according to claim 5, characterized in that: The stress relieving agent is obtained by mixing nano-precipitated barium sulfate, ultrafine high-silicon talc powder and anionic surfactant with high-speed stirring, and then adding a titanate coupling agent with low-speed stirring.

7. The stress-resistant flame-retardant ABS composite material according to claim 6, characterized in that: The speed of high-speed stirring is 2500~3500rpm, and the time is 3~10min.

8. The stress-resistant flame-retardant ABS composite material according to claim 6, characterized in that: The speed of low-speed stirring is 200~300rpm, and the time is 3~10min.

9. The stress-resistant flame-retardant ABS composite material according to claim 1, characterized in that: The lubricant is one or more of vinyl bisstearamide, oxidized polyethylene wax, magnesium stearate and white oil.

10. A method for preparing the stress-resistant flame-retardant ABS composite material according to claim 1, characterized in that: The following steps are involved: ABS 1, ABS 2, ABS high rubber powder, flame retardant, stress reliever, antioxidant, lubricant and UV absorber are mixed, extruded through a twin-screw extruder, cooled, dried and granulated.